Palladium catalyst system for reforming in circulating flow reactor

By using a palladium-based catalyst system in the countercurrent reactor and controlling the temperature, the problem of catalytic activity being reduced under high temperature conditions is solved, and the stability and efficiency of the catalyst are improved.

CN119032064APending Publication Date: 2024-11-26EXXONMOBIL TECHNOLOGY & ENGINEERING CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031756.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-07
Filing Date
2023-04-05
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In a reforming environment in a countercurrent reactor, catalytic activity decreases over time, especially at high temperatures, resulting in a decrease in system efficiency.

Method used

Using a system containing palladium (Pd) as a catalyst, the catalyst is reduced by depositing the catalyst on the support structure and controlling the temperature between 900°C and 1300°C in the reaction zone to avoid oxidation and volatility of palladium and maintaining its metallic state. loss of activity.

Benefits of technology

It effectively reduces the activity loss of the catalyst, improves the stability and efficiency of the system, and extends the service life of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032064A_ABST
    Figure CN119032064A_ABST
Patent Text Reader

Abstract

Palladium-based catalyst systems for reforming hydrocarbons and methods for using such catalyst systems are provided. The catalyst system may be deposited or otherwise coated on a surface or structure, such as a monolith, to achieve improved activity and / or structural stability. It has been found that for a palladium-based catalyst system, the loss of catalytic activity for reforming over time can be reduced or minimized by operating the reactor / performing a reaction cycle such that a portion of the reaction environment containing the palladium-based catalyst system is not exposed to oxidation conditions of 600 DEG C to 900 DEG C. Optionally, the reactor may also be operated / the reaction cycle may also be designed such that a peak temperature of the portion of the reaction environment containing the palladium-based catalyst system is 1300 DEG C or less during a reforming cycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to palladium-based catalyst systems for the reforming of hydrocarbons in high temperature environments. Background Art

[0002] Countercurrent reactor is an example of a reactor type useful in a process with cyclic reaction conditions. For example, due to the endothermic nature of the reforming reaction, it is necessary to introduce additional heat into the reforming reaction environment on a stable basis. Countercurrent reactor can provide an effective way to introduce heat into the reaction environment. After a part of a reaction cycle for reforming or another endothermic reaction, the second part of the reaction cycle can be used for combustion or another exothermic reaction, to add heat to the reaction environment, in preparation for the next reforming step. U.S. Patent No. 7,815,873 and U.S. Patent No. 8,754,276 provide examples of various endothermic processes using a countercurrent reactor in a cyclic reaction environment.

[0003] Endothermic reactions such as reforming can also benefit from having a large amount of available catalytic surface area. Ceramic monolithic structures are examples of types of structures that can provide high available surface area. One option can be to use a monolith that corresponds to a stacked array of pores or channels through which the reactant gases pass. A washcoat is added to such a monolith to provide catalytic activity.

[0004] Although a countercurrent reactor provides an efficient means for introducing heat into a reaction environment, the peak temperatures encountered within the reforming environment in a countercurrent reactor may tend to be higher than the peak temperatures in a conventional steam methane reformer. These higher temperatures may result in lower catalytic activity over time, although at least some of the mechanisms leading to such activity loss have not been well characterized. It would be beneficial to have a system and method for conducting reforming reactions in a countercurrent reactor environment that can reduce, minimize, or mitigate changes in catalytic activity over time.

[0005] U.S. Patent Application Publication 2020 / 0030778 describes a monolithic structure for hydrocarbon reforming, wherein the monolithic structure is composed of a mixture of one or more doping metal oxides and one or more structural oxides. The doping metal and structural oxide are selected based on their relative Gibbs free energy values. NiO and Al2O3 are described as examples of suitable combinations of doping metal oxides and structural oxides for forming the monolithic structure. Summary of the invention

[0006] In various aspects, a method for reforming hydrocarbons is provided. The method comprises exposing a reactant stream containing reformable hydrocarbons to a catalyst system in a reaction zone within a reactor to form a product stream comprising H2. The reaction zone comprises the catalyst system supported on one or more surfaces of a support structure. The catalyst system comprises Pd in ​​at least a portion of the reaction zone. Additionally, the method comprises reacting a mixture comprising a fuel and 0.1 vol% or more O2 in a combustion zone within a reactor under combustion conditions to heat one or more surfaces in the reaction zone to a regeneration surface temperature of 1000°C to 1300°C. In various aspects, the minimum temperature in at least a portion of the reaction zone at the end of the exposure is 900°C or higher, and / or the minimum temperature in at least a portion of the reaction zone at the start of the reaction may be 900°C or higher. BRIEF DESCRIPTION OF THE DRAWINGS

[0007] FIG1 shows an example of the operation of a countercurrent reactor.

[0008] Figure 2 An example of a countercurrent reactor is shown.

[0009] Figure 3 An example of a catalyst system deposited on the surface of a honeycomb monolith is shown.

[0010] Figure 4 An example of a temperature profile for steam reforming in a countercurrent reactor is shown.

[0011] Figure 5 Shown are flame ionization detection (FID) results of the output stream of the reforming of a methane stream in the presence of a Ni-based catalyst.

[0012] Figure 6 Shown are the FID results for the output stream of the reforming of a methane stream in the presence of a relatively small amount of a Ni-based catalyst.

[0013] Figure 7 Shown are the FID results for the output stream of the reforming of a methane stream in the presence of an Rh-based catalyst.

[0014] Figure 8 Shown are the FID results for the output stream of the reforming of a methane stream in the presence of a Pd-based catalyst.

[0015] Fig. 9 The conversion of methane during reforming under cyclic reforming conditions in the presence of various catalyst systems is shown.

[0016] Fig.10 Shown are thermal conductivity results obtained for exposing an O2-containing gas stream to a catalyst system containing Pd at different temperatures. DETAILED DESCRIPTION

[0017] All numerical values ​​in the detailed description and claims herein are modified by the indicated value of "about" or "approximately", and take into account experimental error and variations that would be expected by a person of ordinary skill in the art.

[0018] Overview

[0019] In various aspects, a palladium-based catalyst system for reforming hydrocarbons and a method for using such a catalyst system are provided. The catalyst system can be deposited or otherwise coated on a surface or structure such as a monolith to achieve improved activity and / or structural stability. It has been found that for palladium-based catalyst systems, by operating a reactor / performing a reaction cycle so that a portion of the reaction environment containing the palladium-based catalyst system is not exposed to oxidizing conditions of 600° C. to 900° C., the catalytic activity loss for reforming over time can be reduced or minimized. Optionally, the reactor can also be operated / the reaction cycle can also be designed so that during the reforming cycle, the peak temperature of the portion of the reaction environment containing the palladium-based catalyst system is 1300° C. or less.

[0020] It should be noted that oxidation of Pd may also occur below 600°C, and that the Pd in ​​the catalyst system may be present in the form of an oxide before the cyclic reforming process is started. When the temperature of the Pd-containing portion of the catalyst system is below 600°C, the Pd-containing portion of the catalyst system may be heated in the presence of a reducing and / or inert environment so that the Pd-containing portion of the catalyst system returns to a temperature above 900°C before being exposed to an oxidizing environment. It should be noted that a Pd-containing catalyst system may also be referred to as a palladium-based catalyst system. It should be further noted that a Pd-containing catalyst system / palladium-based catalyst system does not require Pd to be distributed throughout the catalyst system. For example, a first portion of the catalyst system may contain Pd, while a second portion of the catalyst system intended to operate at a lower temperature may have a lower concentration of Pd or may even be substantially free of Pd.

[0021] Without being bound by any particular theory, it has been found that in direct heat transfer, circulating flow reaction environments, the partial loss of reforming activity of the catalyst system may be due to the volatility of the catalytic metal at the relatively high temperature present in such environments. Such metals can volatilize in oxide form or metallic form. When the metal volatilizes, the flow in the reaction environment can bring the metal to different locations in the reaction environment and / or completely remove the metal from the reaction environment. This may lead to the loss of catalytic activity (due to the catalyst being transferred to the various parts of the reaction environment operating at a lower temperature). Additionally, such metal losses may also reduce the stability of the catalyst system over time.

[0022] It is further found that the use of a palladium-based catalyst system can reduce or minimize difficulties associated with catalyst volatility when the palladium-based catalyst system is paired with an appropriate reforming reaction cycle. In various aspects, a reforming reaction cycle can be used so that in at least a portion of the reaction zone in the reactor containing the palladium-based catalyst system, a temperature distribution is maintained, wherein the palladium-based catalyst system is exposed to oxidizing conditions at a temperature of 900°C or higher (such as up to 1300°C). In other words, at the beginning of exposure to oxidizing conditions, the minimum temperature of the portion of the reaction zone containing the Pd-containing catalyst system can be 900°C or higher. Additionally or alternatively, during and / or at the end of exposure to oxidizing conditions, the peak or maximum temperature in the portion of the reaction zone containing the Pd-containing catalyst can be 1300°C or lower. For example, when the fuel reacts with oxygen in or near the reaction zone to provide heat for the next reforming step in the reforming reaction cycle, it may be exposed to oxidizing conditions. In some aspects, still further stability can be achieved by maintaining the Pd-containing portion of the catalyst system when exposed to oxidizing conditions at temperatures of 950° C. or greater, or 1000° C. or greater, such as up to 1300° C. Pd oxidation in the palladium-based catalyst system can be reduced, minimized, or avoided by maintaining the temperature in at least one zone at 900° C. or greater when reacting fuel with oxygen in the vicinity of the palladium-based catalyst system (and / or in other aspects when oxidizing conditions exist).

[0023] At temperatures of 900°C or higher, Pd is not easily converted to an oxide form. However, at temperatures of 900°C or higher, the volatility of the oxide form of Pd is significantly higher than that of metal Pd. By reducing, minimizing or eliminating the exposure of Pd to oxidizing conditions below 900°C during the reforming cycle, the Pd in ​​the palladium-based catalyst system can be maintained in a metallic state throughout the reforming cycle. Due to the significantly lower volatility of metal Pd at temperatures between 900°C and 1300°C, any catalytic activity loss due to catalyst volatility is reduced or minimized, and the difficulties associated with the volatilization of Pd oxides at elevated temperatures can be avoided. When the temperature is above 1300°C, Pd will begin to volatilize even if it is not exposed to an oxidizing environment. Without being bound by any particular theory, it should be noted that the melting point of Pd is approximately 1550°C. It is believed that at temperatures above 1300°C, the volatility of metal Pd increases to a sufficient level to reduce or minimize the benefits of the volatility difference between Pd metal and Pd oxide.

[0024] In this discussion, the catalyst system is defined as comprising at least one catalytic metal (metallic or oxide state) and at least one metal oxide support layer. In at least a portion of the reaction zone, the catalyst system may include Pd. Optionally, other catalytic metals (in metal form and / or oxide form) may also be present in at least a portion of the reaction zone and / or in other portions of the reaction zone. In some aspects, the catalyst and the metal oxide support layer may be coated on the monolith simultaneously, such as in the form of a support coating on a support. In such aspects, the catalyst may be mixed with the metal oxide support layer. Alternatively, the catalyst and the metal oxide support layer may be deposited sequentially, such that the support layer is deposited first, followed by the catalyst. In some optional aspects, the metal oxide support layer may correspond to a thermally stable metal oxide support layer, such as a metal oxide support layer that is thermally stable at a temperature of 800° C. to 1600° C. Optionally, before depositing the catalyst system, an intermediate bonding layer may be applied to at least a portion of the monolith or other structure. The catalyst system may be useful for use in a cyclic reaction environment, such as a countercurrent reactor or other types of reactors that use flow operations in opposite directions and at different times in a reaction cycle. Reaction conditions in a cyclic reaction environment may also experience fluctuations in temperature and / or pressure during the reaction cycle.

[0025] In order to use the catalyst system in a cyclic reaction environment, the catalyst system can be coated or otherwise loaded on a structure or surface that will be present in the reaction environment during the reforming process cycle. For example, the catalyst system can be applied as a carrier coating on the surface of one or more monoliths or other structures placed in the reactor. Such monoliths or other structures can contain a large amount of channels or pores per unit surface area to significantly increase the amount of structural surface area that can be coated with the catalyst system. In some aspects, the catalyst system can be deposited on a monolith or other structure consisting of a low surface area material that is phase-stable under high temperature reforming conditions. In such aspects, the catalyst system and the monolith or other structure can be annealed at a temperature equal to or higher than the processing temperature before use. This can provide further structural stability for the catalyst system, so that the catalyst system can substantially maintain the amount of time for the desired reforming activity level to increase unexpectedly.

[0026] Figure 3 An example of a portion of a monolith 300 is shown, the portion comprising a catalyst system 310 deposited (or otherwise coated) on a surface of the monolith 300. Figure 3In the example shown, a portion of the monolith corresponds to a regular pattern of square channels that allow reactant gas (such as reforming feed gas flow) to pass through the channels. In other aspects, any convenient type of channel shape can be used, such as circular or hexagonal channels. Catalyst system 310 corresponds to a layer comprising catalyst 312 and metal oxide support 314, which is coated on the surface of the channels of the monolith.

[0027] In some aspects, the catalyst system can correspond to one or more catalysts in a single zone, wherein at least one of the catalysts corresponds to Pd. In other aspects, the catalyst system can correspond to multiple catalyst zones, wherein a catalyst corresponding to Pd is present in at least one of the catalyst zones. Optionally, in such aspects, at least one catalyst zone can comprise a catalyst different from the catalyst in the second catalyst zone.

[0028] Reforming of hydrocarbons to form synthesis gas is a potentially desirable approach for reducing or minimizing CO2 emissions associated with hydrocarbon fuels. Reforming can convert hydrocarbon fuels into H2 (a fuel without CO2 emissions) and CO or CO2. By separating H2 from carbon oxides at a single location, some of the difficulties associated with preventing CO2 emissions can be reduced or minimized. However, due to the elevated temperatures required for hydrocarbon reforming, balancing efficient reforming of hydrocarbons with energy consumption and the operating life of the equipment remains a challenge.

[0029] A kind of selection for improving the energy efficiency of reforming process can be to use reaction system, such as countercurrent reactor, or another type of reaction system, wherein during reforming step and regeneration (heating) step, stream passes through reactor in opposite direction.Countercurrent reactor (and other similar type of reactor) can provide several advantages.First, by using multiple steps with different streams during reaction cycle, heat can be added to reaction zone, in which reforming is carried out by burning in or near reaction zone.This can reduce or minimize heat loss, while trying to increase the heat of reaction zone.Using flow in opposite direction can provide other benefit about forming desired temperature distribution in reaction zone.Countercurrent reactor will be used as the example of this type system in this article, but it should be understood that countercurrent reactor is the example of reactor that can provide such benefit.

[0030] Reforming catalyst and metal oxide support layer

[0031] In various aspects, one option for adding a reforming catalyst to a monolith can be to coat the monolith with a mixture of a catalyst (optionally in the form of an oxide) and a metal oxide support layer. For example, a powder of a catalyst oxide and a metal oxide support layer can be used to form a support coating, which is then applied to the monolith (or other structure). This can produce a catalyst system in which the catalyst is mixed / distributed throughout the metal oxide support layer, which is different from the catalyst deposited on the top of the metal oxide support layer. In other words, at least a portion of the catalyst system can correspond to a mixture of a catalyst and a support layer. In other aspects, any convenient method for depositing or otherwise coating the catalyst system on a monolith or other structure can be used. The weight of the catalyst system on the monolith (or other structure) can correspond to 0.1wt% to 10wt%, or 0.5wt% to 10wt%, or 2.0wt% to 10wt%, or 0.1wt% to 6.0wt%, or 0.5wt% to 6.0wt% or 2.0wt% to 6.0wt% of the total weight of the catalyst system plus the monolith.

[0032] In some aspects, the catalyst system can include a thermally stable metal oxide support layer. A thermally stable metal oxide support layer corresponds to a metal oxide that is thermally stable with respect to a structural phase transition at a temperature between 800° C. and 1600° C. In some aspects, such a thermally stable metal oxide support layer can be formed by using a surface area of ​​20 m 2 / g or less of metal oxide powder coated on the surface (such as using a carrier coating). For example, the surface area of ​​the metal oxide powder used to form the thermally stable metal oxide coating can be 0.5 m 2 / g to 20m 2 / g, or 1.0m 2 / g to 20m 2 / g or 5.0m 2 / g to 20m 2 / g. In various aspects, the catalyst can be annealed at a temperature of 1000°C or higher, or 1100°C or higher, or 1200°C or higher, or 1300°C or higher, such as up to 1500°C or possibly higher. This temperature can be substantially similar to or higher than the peak temperature to which the catalyst is exposed in the reforming process cycle. In some aspects, the annealing temperature can be between 1000°C and 1300°C. An annealing temperature substantially similar to the peak temperature can correspond to an annealing temperature that differs from the peak temperature by 0°C to 50°C.

[0033] As an example of a thermally stable metal oxide support layer, alumina has multiple phases including α-Al2O3, γ-Al2O3 and θ-Al2O3. The surface area of ​​the metal powder of α-Al2O3 can be generally 20 m 2 / g or less. In contrast, the surface area of ​​the γ-Al2O3 phase and the θ-Al2O3 phase is higher, and the surface area of ​​the metal powder in the washcoat solution for γ-Al2O3 and / or θ-Al2O3 will be greater than 20 m 2 / g. It is generally believed that phases such as θ-alumina or γ-alumina are superior as support structures for deposited catalysts because the greater surface area per gram of θ-alumina or γ-alumina will allow for the availability of more catalyst active sites than α-alumina. However, phases such as γ-Al2O3 and θ-Al2O3 are not thermally phase-stable at temperatures between 800°C and 1600°C. At such high temperatures, phases such as γ-Al2O3 and θ-Al2O3 will undergo phase transitions to higher stability phases. For example, at elevated temperatures, γ-Al2O3 will first convert to Δ-Al2O3 at about 750°C; then Δ-Al2O3 will convert to θ-Al2O3 at about 950°C; then, θ-Al2O3 will convert to α-Al2O3 with further exposure to elevated temperatures between 1000°C and 1100°C. Therefore, α-Al2O3 is the thermally phase-stable form of Al2O3 at temperatures between 800°C and 1600°C.

[0034] Without being bound by any particular theory, it is believed that such phase changes during exposure to elevated temperatures may result in degradation of the structure of the catalyst and / or supported catalyst. In contrast, by using a carrier that is phase-stable at an elevated annealing temperature, and then annealing the catalyst (including the carrier) at an elevated annealing temperature, the resulting catalyst can substantially maintain an initial catalytic activity level over an extended period of time. It should be noted that the initial catalytic activity obtained by depositing the catalyst on a monolith formed of a phase-stable low per gram surface area material may be lower than depositing the catalyst on a similar monolith formed of a material with a higher per gram surface area. However, it has been found that this initial activity advantage of higher surface area materials is rapidly lost during exposure to cyclic high temperature reforming conditions.

[0035] As a further illustration, without being bound by any particular theory, γ-Al2O3 is a transition alumina that can be viewed as a defective oxyhydroxide with a spinel-related crystalline structure. In previous academic work, γ-Al2O3 has been formulated into alumina spinels with defect sites having The molecular formula is represents an open cationic site. Containing a hydroxyl group, it can be considered Such γ-Al2O3 is thermally unstable relative to α-Al2O3. Although θ-Al2O3 is more crystalline and has a smaller surface area and hydroxide content than γ-Al2O3, θ-Al2O3 also contains defect sites (i.e., open cation sites) and is also thermally unstable relative to α-Al2O3. Therefore, both γ- and θ-Al2O3 have defect sites that can react with multivalent cations (or metal oxides) Both Rh(O) and Ni(O) can react to produce a denser phase, where Rh and Ni are chemically less prone to catalytic reactions than their oxide or metallic states. Even without reacting with Rh or Ni, γ- and θ-Al2O3 are thermodynamically unstable relative to α-Al2O3 at high temperature conditions.

[0036] It has been found that using heat-stable metal oxides in catalyst systems, combined with annealing of the catalyst system on the monolith at high temperatures, can provide unexpected activity benefits and structural stability benefits over an extended period of time. Without being bound by any particular theory, when a catalyst system comprising a non-heat-stable metal oxide is used for the coating of a monolith, exposing such a catalyst system to a circulating high-temperature reforming environment may cause the structural degradation of the catalyst system. It is believed that this structural degradation of the catalyst system may reduce the available catalyst sites, which may be due to the catalyst being buried in the degraded structure and / or the additional sintering or agglomeration of the catalyst, because the non-heat-stable metal oxide in the catalyst system is converted into a phase with a lower surface area. For example, by inspecting the catalyst system on the monolith after being exposed to a circulating high-temperature reaction environment, this structural degradation can be observed. For conventional catalyst systems, after being exposed to a circulating high-temperature reaction environment, the catalyst system can be easily scraped off from the underlying structure. Additionally, a significant reduction in activity can be observed.

[0037] In contrast, when using a catalyst system comprising a heat-stable metal oxide, the activity of the catalyst in the catalyst system can unexpectedly maintain a long run time, with little or no activity loss. Additionally, after being exposed to a circulating high temperature reforming environment, the catalyst system may unexpectedly remain firmly adhered or coated on a bottom monolith or other structure. It should be noted that the initial catalyst activity may be lower than the activity of a conventional system, because the heat-stable metal oxide generally has a relatively low surface area. This is considered to initially reduce the number of available catalytic sites. However, because the heat-stable metal oxide does not undergo phase change when exposed to heat, the catalytic activity of the catalyst system comprising a heat-stable metal oxide can be maintained. Due to the rapid deactivation of a conventional catalyst or catalyst system, the activity of a conventional catalyst system may rapidly drop to an activity lower than that of a catalyst system using a heat-stable metal oxide.

[0038] For example, the catalyst system can be applied to a monolith or other structure by applying the catalyst system as a carrier coating suspension. In order to form a carrier coating suspension, the catalyst system can be added to water to form an aqueous suspension with 10wt% to 50wt% solids. For example, the aqueous suspension can contain 10wt% to 50wt% solids, or 15wt% to 40wt% or 10wt% to 30wt%. Optionally, an acid or base can be added to the aqueous suspension to reduce or increase the pH, respectively, thereby changing the particle size distribution of the alumina catalyst and / or binder particles. For example, acetic acid or another organic acid can be added to reach a pH of 3 to 4. The suspension can then be ball milled (or processed in another way) to obtain the desired particle size of the catalyst particles, such as a particle size of 0.5μm to 5μm. After grinding, the suspension can be stirred until use so that the particles are substantially evenly distributed in the solution.

[0039] The washcoat suspension may then be applied to the monolith structure to obtain a desired amount of catalyst (e.g., nickel or rhodium) on the surface of the monolith structure. For example, in one aspect, a washcoat thickness of 10 microns is achieved by forming a washcoat corresponding to 10 wt% of the monolith structure. Any convenient type of monolith structure may be used to provide sufficient surface area for the support of the catalyst particles. The washcoat may be applied to the monolith to form pores with the inner surface coated with the catalyst. One option for applying the washcoat may be to immerse or otherwise submerge the monolith in the washcoat suspension.

[0040] After cleaning the cell channels of excess washcoat, the catalyst system coated on the monolith can be optionally dried. Drying can correspond to heating at 100° C. to 200° C. for 0.5 to 24 hours. After any optional drying, calcination can be performed. In some aspects, calcination can correspond to heating at 200° C. to 800° C. for 0.5 to 24 hours.

[0041] In other aspects, a high temperature calcination step can be used so that the calcination temperature of the catalyst system coated on the monolith is substantially similar to or higher than the peak temperature to which the monolith will be exposed during the cyclic high temperature reforming reaction. For the monolith in the high temperature zone, this can correspond to calcining the catalyst system coated on the monolith at a temperature of 900°C or higher, or 1000°C or higher, or 1200°C or higher, or 1300°C or higher, such as up to 1500°C or possibly still higher. It should be noted that if multiple catalyst zones are present, the calcination of the monolith in different catalyst zones can be different.

[0042] It has been unexpectedly found that during the cyclic high temperature reforming process, calcining at a temperature similar to or higher than the peak temperature can unexpectedly improve the activity of the catalyst system and / or the adhesion of the catalyst system to the bottom monolith. Without being bound by any particular theory, it is believed that before the catalyst is exposed to the cyclic reaction environment, exposing the monolith and the deposited catalyst system to an elevated temperature can promote the formation of a stable interface between the catalyst system and the monolith. This stable interface can have improved tolerance to high temperature oxidation and / or reduction environments during the reforming process, thereby improving the stability for maintaining the catalyst system on the surface of the monolith.

[0043] In various aspects, at least a portion of the catalyst system can have Pd as a catalyst (or as at least a portion of the catalyst). During operation, when the catalyst is exposed to oxidizing conditions, this area or zone can be maintained at a temperature between 900°C and 1300°C. Since the oxidizing conditions are used to provide heat for the reaction cycle, in some aspects, maintaining the temperature between 900°C and 1300°C can correspond to starting the regeneration step of the reaction cycle with at least one zone containing Pd as a catalyst at a temperature of 900°C or higher, and then having a temperature of 1300°C or lower at the end of the regeneration step.

[0044] It should be noted that even if some of the Pd in ​​the reaction zone is initially present in the form of palladium oxide, such Pd can be readily converted to metallic Pd. This can be accomplished, for example, using an initial activation step in the presence of H2. Another option may be to simply conduct one or more reforming cycles as long as at least some H2 is present in the portion of the reaction zone containing Pd. Because Pd resists oxidation at temperatures between 900°C and 1300°C, once the Pd is converted to metallic form, the Pd can be substantially maintained in the metallic state during the cyclic reforming reaction in which the Pd is exposed to oxidizing conditions between 900°C and 1300°C.

[0045] In some aspects, when using Pd and another catalytic metal, a catalyst system can be used. In other aspects, multiple catalyst regions or districts can be used, wherein the first region or district comprises a catalyst containing Pd, and one or more other districts can be selected to have different catalysts, possibly corresponding to a catalyst that does not comprise Pd. In the aspect that the catalyst comprises a metal other than Pd and / or a part of the catalyst does not comprise Pd, suitable catalytic metals can include but are not limited to Ni, Co, Fe, Rh, Ru, Pt, Ir, Cu, Ag, Au, Zr, Cr, Ti, V, Mo, Nb and combinations thereof. Catalytic metals can be selected based on the desired catalytic activity type. Such catalytic metals can be used in catalysts in the form of metal oxides. In some aspects, in order to reform hydrocarbons in the presence of H2O and / or CO2 to prepare hydrogen, Ni, Rh, Ru, Pt, Ir, Cu, Co or a combination thereof can be a suitable catalytic metal in combination with Pd and / or in a region or district using a catalyst other than Pd. The weight of the catalytic metal oxide in the catalyst system can be in the range of 0.1 wt% to 70 wt%, or 1.0 wt% to 60 wt%, or 2.0 wt% to 50 wt%, relative to the total weight of the catalyst system. In some aspects where the catalytic metal corresponds to a noble metal or a precious metal, the weight of the catalytic metal oxide in the catalyst system can be in the range of 0.1 wt% to 10 wt%, or 0.2 wt% to 7.0 wt%, or 0.5 wt% to 4 wt%.

[0046] The catalytic metal can be selected to provide long-term stable performance in a specific temperature zone of the catalyst bed. This can allow stable methane conversion, phase stability of the metal oxide carrier, and sintering of the catalytic metal to be reduced or minimized. As an example involving three catalyst zones, the catalyst system in the highest temperature catalytic zone (e.g., 900-1300°C) exposed to some of the highest temperatures and most violent temperature fluctuations can be composed of Pd as a catalytic metal and Al2O3 as a metal oxide carrier. This catalyst system can be formed, for example, by using a mixture of Pd and Al2O3 as a carrier coating on an α-Al2O3 monolith. In such examples, the catalyst system in the medium temperature catalytic zone (e.g., 600-1150°C) can be composed of Ni and Rh as catalytic metals (NiO and Rh2O3 as catalytic metal oxides) and Al2O3 as a metal oxide carrier. To form this catalyst system, a mixture of NiO and Rh2O3 as catalytic materials and Al2O3 (optionally but preferably α-Al2O3) as a metal oxide support material can be wash-coated on a monolith including 95wt% α-Al2O3, 4wt% SiO2, and 1wt% TiO2. In such an example, the catalyst system in the low-temperature catalytic zone (e.g., 400-1050°C) can be composed of Rh as a catalytic metal (Rh2O3 as a catalytic metal oxide) and α-Al2O3 as a metal oxide support. To form this catalyst system, a mixture of Rh2O3 and α-Al2O3 as catalytic materials can be wash-coated on a monolith including 93wt% α-Al2O3, 5wt% SiO2, and 2wt% MgO.

[0047] In various aspects, suitable metals for the metal oxide support layer in the catalyst system may include but are not limited to Al, Si, Mg, Ca, Sr, Ba, K, Na, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Ni, Co, Y, La, Ce and combinations thereof. The metal (or metals) for the metal oxide support may be selected so that the metal oxide support is not substantially converted to a metallic form under the reducing conditions present in the cyclic reaction environment. As an example, when the catalytic metal oxide is NiO, one option for the metal oxide support is Al2O3, preferably α-Al2O3. Another example of a suitable metal oxide support optionally combined with NiO as a catalytic metal oxide is a mixture of Al2O3 and SiO2, MgO and / or TiO2. In such examples, SiO2 may be combined with Al2O3 to form a mullite phase, which may increase resistance to thermal shock and / or mechanical failure. Additionally or alternatively, in such examples, MgO and / or TiO2 may be added. The weight of the metal oxide support in the catalyst bed may range from 1.0 wt% to 40 wt%, or from 2.0 wt% to 30 wt%, or from 3.0 wt% to 20 wt%, relative to the total weight of the monolith in the catalyst bed.

[0048] In various aspects, the metal oxide support layer (such as a thermally stable metal oxide support layer) can correspond to at least one oxide selected from the group consisting of corundum, stabilized zirconia, perovskite, pyrochlore, spinel, hibonite, zeolite, and mixtures thereof. The weight of the metal oxide support can be in the range of 1.0 wt% to 40 wt%, or 2.0 wt% to 30 wt%, or 3.0 wt% to 20 wt%, relative to the total weight of the monolith plus the catalyst system.

[0049] One class of metal oxide support layers may correspond to conventional refractory oxides commonly used to form supported catalysts. For example, the metal oxide support may correspond to α-Al2O3, LaAlO3, LaAl 11 O 18 , MgO, CaO, ZrO2, TiO2, CeO2, Y2O3, La2O3, SiO2, Na2O, K2O and mixtures thereof. This family is defined herein as the "corundum" family of oxides, although many oxides in this family do not have a corundum lattice structure. For example, CeO2 and MgO can both have a halite crystal structure. α-Al2O3 consists essentially of a dense arrangement of oxygen ions in a hexagonal closest packing, with Al on two-thirds of the available octahedral sites. 3+ ions. LaAlO3, often abbreviated as LAO, is an optically transparent ceramic oxide with a distorted perovskite structure. 11 O18 It can be formed by the solid-state reaction of LaAlO3 and α-Al2O3. 11 O 18 The plate-like crystals are particularly useful as metal oxide supports because catalytic metals can be trapped between the plate-like crystal structures. It inhibits sintering of minute catalytic metals in the active material wash-coated on the monolith of the catalyst bed. Additional examples of corundum oxides may include, but are not limited to, based on the weight of the metal oxide support: i) 95 wt% α-Al2O3 and 5 wt% SiO2; ii) 93 wt% α-Al2O3, 5 wt% SiO2, and 2 wt% MgO; iii) 94 wt% α-Al2O3, 4 wt% SiO2, 2 wt% MgO, and 1 wt% Na2O; iv) 95 wt% α-Al2O3, 4 wt% SiO2, and 1 wt% TiO2 ; v) 7wt% CeO2 and 93wt% MgO; vi) 5wt% CaO and 95wt% α-Al2O3; vii) 5wt% MgO, 5wt% CeO2 and 90wt% α-Al2O3; viii) 20wt% ZrO2 and 80wt% CeO2; ix) 5wt% CeO2, 20wt% ZrO2 and 75wt% α-Al2O3; and x) 6wt% La2O3 and 94wt% α-Al2O3.

[0050] Another class of metal oxides used for the metal oxide support layer corresponds to stabilized zirconia. In this discussion, stabilized zirconia as a metal oxide support is defined as an oxide comprising zirconium oxide (ZrO2, zirconia) and at least one added oxide corresponding to Y2O3, CaO, MgO, HfO2, CeO2, SiO2, Sc2O3, La2O3, Al2O3 and mixtures thereof. Pure ZrO2 undergoes a phase transition from a monoclinic structure (stable at room temperature) to a tetragonal structure (at about 1173°C) and then to a cubic (at about 2370°C) structure. When the metal oxide support is made of pure zirconia, it may lead to fracture at lower temperatures because it transforms from a tetragonal structure to a monoclinic structure, which results in volume expansion. To alleviate this problem, pure ZrO2 can be stabilized as a cubic polymorph over a wide temperature range. This can be achieved by using slightly larger ions such as Y 3+ ions (with an ionic radius of 0.096 nm) and / or ions from other added oxides to replace some Zr in the lattice 4+ions (with an ionic radius of 0.082 nm). The resulting doped zirconia material is called stabilized zirconia. In the present invention, the weight of the added oxide in the stabilized zirconia may be in the range of 5wt% to 70wt%, or 6wt% to 60wt% or 7wt% to 50wt%, relative to the total weight of the stabilized zirconia composition. The preferred stabilized zirconia is yttria (Y2O3) stabilized zirconia, usually abbreviated as YSZ. YSZ is a metal oxide support in which the cubic crystal structure of the zirconia is stabilized at room temperature by adding yttria in an amount of 10wt% to 30wt% relative to the total weight of YSZ. Other examples of stabilized zirconia as metal oxide supports include, but are not limited to: i) 10 wt% Sc2O3 stabilized zirconia (ScSZ); ii) 6 wt% Sc2O3 and 1 wt% Al2O3 stabilized zirconia (ScAlSZ); iii) 65 wt% CeO2 stabilized zirconia (CSZ); and iv) 30 wt% CeO2 and 20 wt% Al2O3 stabilized zirconia (CeAlSZ).

[0051] Still another class of metal oxides used for metal oxide support layers corresponds to perovskites. Perovskites as metal oxide supports are based on a cubic perovskite structure of the general formula (ABO3). The "A" site and the "B" site can be doped with a large number of metal cations within size limits. This can allow the properties of the metal oxide support to be adjusted to achieve various purposes. The A site cation is larger than the B site cation. The ideal cubic structure has a 6-fold coordinated B site cation surrounded by an octahedron of anions and a 12-fold cubo-octahedral coordinated A site cation. The relative ion size requirements for the stability of the cubic structure are very strict, so slight bending and twisting may produce several distorted forms with lower symmetry, in which the coordination number of the A site cation, the B site cation, or both is reduced. Therefore, the doped perovskite structure can be represented by the following chemical formula: A x A' 1-x B y B' 1-y O 3-n , wherein A or A' is an element selected from La, Sr, Ba, Ca, Zr and Y; wherein B or B' is an element selected from Mg, Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, Ga, Zr, Y and Zn; wherein both x and y are numbers independently selected in the range of 0.0 to 1.0; and wherein n is a number in the range of 0.0 to 0.5. Examples of perovskite structures for metal oxide support layers may include, but are not limited to, SrTiO3, CaTiO3, YAlO3, LaMnO3, LaCo 0.4 Ni 0.6 O3(LCN), Sr 0.65 La 0.35TiO3(SLT), BaZr 0.8 Y 0.2 O3(BZY), La 0.8 Sr 0.2 MnO3(LSM), La 0.6 Sr 0.4 Co 0.2 Fe 0.8 O3(LSCF), Ba 0.5 Sr 0.5 Co 0.8 Fe 0.2 O3(BSCF), La 0.6 Sr 0.4 Co 0.8 Cr 0.2 O3(LSCC), La 0.6 Sr 0.4 Co 0.8 Mn 0.2 O3(LSCM), La 0.8 Sr 0.2 FeO3(LSF) and Y 0.1 Ba 0.9 CoO3(YBC).

[0052] Yet another class of metal oxides for metal oxide support layers corresponds to pyrochlores. Pyrochlores as metal oxide supports are based on the mineral pyrochlore crystal structure of the general formula A2B2O7, where the "A" and "B" species are typically rare earth or transition metal species. The pyrochlore structure is a superstructure derivative of the simple fluorite structure. Thus, similar to perovskites, the doped pyrochlore structure can be represented by the following chemical formula: A x A' 2-x B y B' 2-y O 7-n , wherein A or A' is an element selected from La, Sr, Ba, Ca, Gd, Bi, Dy, Tl, Cd and Y; B or B' is an element selected from Zr, Ti, Cr, Mn, Fe, Co, Ni, Ru, Mo and Re; wherein both x and y are numbers independently selected in the range of 0.0 to 2.0; and n is a number in the range of 0.0 to 0.5. Examples of pyrochlore structures for metal oxide support layers include, but are not limited to, La2Zr2O7, Gd 1.9 Ca 0.1 TiO 6.9 , Bi2Ru2O7, Dy2Ti2O7, Y2Mo2O7, Tl2Ru2O7 and Cd2Re2O7.

[0053] Still another class of metal oxides used for metal oxide support layers corresponds to spinels. Spinels as metal oxide supports are based on the spinel structure of the general formula AB2O4, in which the O anions are arranged in a cubic close-packed lattice, and the cations "A" and "B" occupy some or all of the octahedral and tetrahedral sites in the lattice. Although the charges of A and B in the prototype spinel structure are +2 and +3, respectively, A 2+ B 3+ 2O 2- 4, but other combinations combining divalent, trivalent or tetravalent cations (including Mg, Zn, Fe, Mn, Al, Cr, Ti and Si) are also possible. A and B can also be the same metal with different valences, such as magnetite Fe3O4 (as Fe 2+ Fe 3+ 2O 2- 4), which is the most abundant member of the spinel family. Therefore, the spinel structure can be represented by the following chemical formula: AB2O4, wherein A is an element selected from Mg, Be, Zn, Fe, Ni, Co, Mn, Cu, Ti, Si and mixtures thereof; B is an element selected from the group consisting of Al, Mg, Fe, Mn, Cr, Co, V and mixtures thereof. Examples of spinel structures for metal oxide supports include, but are not limited to, MgAl2O4, BeAl2O4, ZnAl2O4, FeAl2O4, NiAl2O4, MnAl2O4, (Mg,Fe)Al2O4, CuFe2O4, (Fe,Mn,Zn)(Fe,Mn)2O4, MnFe2O4, MgFe2O4, NiFe2O4, TiFe2O4, (Zn,Fe)Fe2O4, FeCr2O4, NiCr2O4, MgCr2O4, ZnCr2O4, Mn 1.5 Co 1.5 O4, FeV2O4, MgV2O4, (Mg,Fe)2SiO4 and BeMgAl4O8.

[0054] Yet another class of metal oxides for metal oxide support layers corresponds to chernobelite. 12 O 19 The mineral calcite crystal structure of the present invention is a calcite crystal structure, wherein "A" is an element selected from Mg, Ca, Sr, Ba, Fe, Ni, Co, La, Ce and mixtures thereof; and "B" is an element selected from Al, Si, Ti, Zr, Hf, Mg, Ca and mixtures thereof. Examples of calcite structures for metal oxide supports include, but are not limited to, CaAl 12 O 19 、(Ca,Ce)(Al,Ti,Mg) 12 O 19、(Ca,Ce,La)(Al,Ti,Mg) 12 O 19 and (Fe,Mg)Al 12 O 19 . Hidrogenite (Ca, Ce)(Al, Ti, Mg) 12 O 19 The plate-like crystals of the catalyst can be particularly useful as metal oxide supports because the catalytic metal can be trapped between the plate-like crystal structures, which can inhibit the sintering of minute catalytic metals in the active material wash-coated on the monolith of the catalyst bed.

[0055] Still another class of metal oxides for metal oxide carrier layers corresponds to zeolites. In this discussion, zeolites as metal oxide carriers refer to aluminosilicate materials consisting of Si, Al, O, H, optionally further comprising metals such as Na, Ca, K, Mg, Ti, Sn, Zn and mixtures thereof, which are members of the microporous solid family known as molecular sieves. The term molecular sieve refers to a specific characteristic of these materials, which selectively sorts molecules based primarily on a size exclusion process. This is due to the very regular pore structure of molecular size. The maximum size of molecules or ionic species that can enter the pores of zeolites is controlled by the size of the channel. These are usually defined by the ring size of the aperture, wherein for example, the term "8-ring" refers to a closed ring consisting of eight tetrahedral coordinated silicon (or aluminum) atoms and 8 oxygen atoms. Due to various reasons, these rings are not always completely symmetrical, and the reasons include strain caused by the combination between the units required to produce the overall structure, or coordination of some oxygen atoms in the ring with cations in the structure. The zeolite used as a metal oxide carrier in the present invention includes more than 245 unique zeolite frameworks produced on a large scale in industry and more than 40 naturally occurring zeolite frameworks. Some examples of zeolites that can be used as metal oxide carriers include USY zeolite, L zeolite, mordenite, ferrierite, beta zeolite, ZSM-5, MCM-68 and mixtures thereof. The zeolite is particularly suitable for use as a metal oxide carrier for active materials in the low temperature catalytic zone of RFR because certain zeolite frameworks are known to be structurally stable at temperatures up to about 750°C. The stable micropores of the zeolite provide a broad surface area for the dispersion of catalytic metals. Other examples of zeolites used as metal oxide carriers include various types of faujasite. This may include faujasite-Na, faujasite-Mg and faujasite-Ca. By varying the amounts of sodium, magnesium and calcium, the faujasites all have the same basic molecular formula, (Na2, Ca, Mg) 3.5 [Al7Si 17 O 48 ] 32(H2O). Like other zeolites, faujasite is synthesized from an alumina source such as sodium aluminate and a silica source such as sodium silicate. Other aluminosilicates, such as kaolin, are also used. These ingredients are dissolved in an alkaline environment such as aqueous sodium hydroxide solution and crystallized at 70-300°C. After crystallization, faujasite is in its sodium form and can be ion-exchanged with ammonium to improve stability. The ammonium ions are later removed by calcination, which puts the zeolite in its acid form. Synthesized faujasite is divided into X zeolite and Y zeolite according to the silica to alumina ratio of its framework. In X zeolite, the silica to alumina ratio is between 2 and 3, while in Y zeolite, the ratio is 3 or more. The negative charge of the framework is balanced by the positive charge of the cations in the non-framework positions. Such zeolites have ion exchange, catalytic and adsorption properties. The stability of the zeolite increases with the silica to alumina ratio of the framework. The stability is also affected by the type and amount of cations located in the non-framework positions. For catalytic cracking, Y zeolite is usually used in rare earth-hydrogen exchange form. By using thermal, hydrothermal or chemical methods, some alumina can be removed from the Y zeolite framework to obtain high-silicon Y zeolite. Such zeolites are used for cracking and hydrocracking catalysts. Complete delamination produces faujasite-silica. Still another example of a zeolite that can be used as a metal oxide support layer is chabazite, which has the formula (Ca, Na2, K2, Mg)Al2Si4O 12 ·6H2O. Depending on the prominence of a given cation, recognized varieties include chabazite-Ca, chabazite-K, chabazite-Na, and chabazite-Sr. Chabazite crystallizes in the triclinic system with typical rhombohedral crystals.

[0056] Structures (monoliths) for supporting catalyst systems

[0057] One of the purposes of using a monolith or another support structure in a reforming environment is to increase the available surface area to accommodate the deposited catalyst / catalyst system. To achieve this, some monoliths correspond to structures having a large number of pores or channels that allow gas to flow through the monolith. Because each individual pore provides surface area for the deposition of catalyst, the inclusion of a large number of pores or channels per unit area can significantly increase the available surface area for the catalyst.

[0058] Typically, the monolith or other structure used to support the catalyst / catalyst system can be formed from a material represented by formula (PQ). P can be at least one metal selected from the group consisting of Al, Si, Mg, Ca, Sr, Ba, K, Na, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Ni, Co, Y, La, Ce, and mixtures thereof. Q is an oxide. Therefore, the monolith material (PQ) is a metal oxide.

[0059] In some preferred aspects, the metal oxide may correspond to aluminum oxide (also known as alumina), Al2O3. The preferred Al2O3 in the present invention is α-Al2O3. Although α-Al2O3 is the preferred crystalline phase, another phase containing sodium oxide (Na2O) may also exist, namely Na2O(Al2O3) 11 Or NaAl5O8, sodium oxide is sometimes an inevitable impurity in α-Al2O3.

[0060] Optionally, the monolith or structural material (PQ) may be α-Al2O3 containing at least one additional oxide selected from the group consisting of SiO2, MgO, CaO, TiO2, Na2O, KO and mixtures thereof. The weight of the additional oxide in the monolith material composition may be in the range of 0.1 wt% to 15 wt%, or 1.0 wt% to 10 wt% or 2.0 wt% to 8.0 wt%, relative to the total weight of the monolith material composition. As non-limiting illustrative examples, the monolith material (PQ) may be: i) 95 wt% α-Al2O3 and 5 wt% SiO2; ii) 93 wt% α-Al2O3, 5 wt% SiO2 and 2 wt% MgO; iii) 93 wt% α-Al2O3, 4 wt% SiO2, 2 wt% MgO and 1 wt% Na2O; and iv) 95 wt% α-Al2O3, 4 wt% SiO2 and 1 wt.% TiO2.

[0061] In other aspects, the monolithic material (PQ) can be partially composed of non-alumina-based oxides or essentially composed of non-alumina-based oxides. As non-limiting illustrative examples, the monolithic material (PQ) can be silicon dioxide (SiO2), magnesium oxide (MgO), cerium oxide (CeO2), titanium dioxide (TiO2), zirconium oxide (ZrO2), cordierite (2MgO 2Al2O32SiO2), mullite (3Al2O3 2SiO2), aluminum titanate (Al2TiO5), magnesium aluminate (MgAl2O4), calcium stabilized zirconium oxide (CaO-ZrO2), magnesium stabilized zirconium oxide (MgO-ZrO2), yttria stabilized zirconium oxide (Y2O3-ZrO2), yttrium oxide (Y2O3), barium zirconate (BaZrO3), strontium zirconate (SrZrO3), and mixtures thereof. Other examples of potential monolithic materials include SiC, Si3N4, yttrium-stabilized zirconia, and Al2TiO5 ceramics. It should be noted that SiC and Si3N4 do not follow the (PQ) structural formula.

[0062] In some aspects, the monolithic material (PQ) may further comprise supplementary components. Such supplementary components may facilitate ease of extrusion and correspond to additional structural components within the monolithic material composition. For example, the monolithic material composition may further comprise one or more silicates comprising a metal selected from the group consisting of: Al, Si, Ca, Mg, K, Na, Y, Zr, Hf, Ti, Cr, Mn, Fe, Ni, Co, and mixtures thereof. An example is bentonite, which is an aluminum phyllosilicate clay primarily composed of montmorillonite. Different types of bentonites are each named after the corresponding primary element, such as potassium (K), sodium (Na), calcium (Ca), and aluminum (Al). For example, the chemical formula of sodium-based bentonite is Al2H2Na2O 13 Si4. Some hydroxyl ions (OH-) may be present in silicates, but under high temperature calcination and sintering conditions, such hydroxyl groups may be converted to oxide form. Yet another example is talc, a compound with the chemical formula Mg3Si4O 10 A clay mineral composed of hydrated magnesium silicate of (OH) 2. Due to the nature of its basal cleavage and uneven flat fracture, it is foliated in the form of two-dimensional plates, which is beneficial for the extrusion of monolithic materials.

[0063] In various aspects, the monolith or other structure for providing a surface for the reforming catalyst system can be prepared by manufacturing techniques, such as but not limited to conventional ceramic powder manufacturing and processing techniques, such as mixing, grinding, degassing, kneading, pressing, extrusion, casting, drying, calcining and sintering. The starting material can correspond to a suitable ceramic powder and an organic binder powder in a suitable volume ratio. Certain process steps can be controlled or adjusted to obtain the desired particle size and porosity range and performance characteristics, such as by including various manufacturing, characteristic adjustment and processing additives and reagents known in the art. For example, two or more types of oxide powders can be mixed in the presence of an organic binder and one or more suitable solvents for a time sufficient to allow the powders to be substantially dispersed from each other. As another example, the precursor of the oxide present in the monolith can be dissolved in water at a desired ratio, spray dried, and calcined to prepare a mixed powder. Such precursors include, but are not limited to, chlorides, sulfates, nitrates and mixtures thereof. The calcined powder can be further mixed in the presence of an organic binder and a suitable solvent to prepare a mixed "dough". The mixed "dough" of materials can then be placed in a mold or form, extruded, dried or otherwise formed into a desired shape. The resulting "green body" can then be sintered at a temperature ranging from about 1200° C. to 1700° C. for at least ten minutes, such as 10 minutes to 10 hours, or possibly from 10 minutes to 48 hours or still longer.

[0064] The sintering operation can be carried out in an oxidizing atmosphere, a reducing atmosphere, or an inert atmosphere, and at ambient pressure or vacuum. For example, the oxidizing atmosphere can be air or oxygen, the inert atmosphere can be argon, and the reducing atmosphere can be hydrogen, CO / CO2, or a H2 / H2O mixture. Thereafter, the sintered body is allowed to cool, typically to ambient conditions. The cooling rate can also be controlled to provide a desired set of grain and pore structures and performance characteristics in a particular composition.

[0065] In some aspects, the monolith material (PQ) may further comprise an intermediate bonding layer. The intermediate bonding layer may be applied to the monolith surface prior to washcoating the active material comprising the metal oxide support and the catalytic metal. The intermediate bonding layer provides better adhesion to the washed active material. The intermediate bonding layer is a metal oxide (M) x O y , wherein (M) is at least one metal selected from the group consisting of Al, Si, Mg, Ca, Sr, Ba, K, Na, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Fe, Ni, Co, Y, La, Ce, and mixtures thereof. Aluminum oxide (also known as aluminum oxide), Al2O3, is a preferred metal oxide for the bonding layer. As an example of a method for forming an intermediate bonding layer, the selected metal oxide (M) may be x O y dispersed in a solution to form a slurry. The slurry can then be wash coated on the monolith. The selected metal oxide (M) x O y The washcoated monolith was dried and sintered at a temperature ranging from 1100°C to 1600°C to prepare an intermediate bonding layer.

[0066] It has been found that limiting the maximum porosity in the final sintered body tends to effectively (if not actually) limit the interconnectivity of pore space with other pore space to an extent that increases or maximizes the volumetric heat capacity of the sintered body. The porosity range of the monolith or other structure can depend on the desired final component properties, but within the range defined by one or more minimum porosity values ​​and one or more maximum porosity values, or any set of values ​​not explicitly enumerated between the minimum and maximum values. Examples of suitable porosity values ​​are porosities of 0 vol% to 20 vol%, or 0 vol% to 15 vol%, or 0 vol% to 10 vol%, or 0 vol% to 5 vol%.

[0067] The sintered monolith and / or other shaped ceramic structures can have any convenient shape suitable for use as a surface for receiving a catalyst or catalyst system. An example of a monolith can be an extruded honeycomb monolith. Honeycomb monolith can be an extruded structure comprising many (e.g., multiple, meaning more than one) small gas flow passages or conduits arranged in parallel with thin walls therebetween. A small reactor can include a single monolith, while a larger reactor can include multiple monoliths, and still larger reactors can be substantially filled with the arrangement of many honeycomb monoliths. Each monolith can be formed by extruding a monolith block having a shaped (e.g., square, triangle or hexagonal) cross section, and stacking such blocks up and down, left and right, in two dimensions or three dimensions. Monoliths can be attractive as reactor internal structures because they provide high heat transfer capabilities with minimal pressure drop.

[0068] In some aspects, the honeycomb monolith can be characterized as having an open frontal area (or geometric void volume) between 25% and 55%, and a conduit density of 50 to 2000 pores or channels per square inch (CPSI), or 100 to 900 channels per square inch, or 100 channels per square inch to 600 channels per square inch. For example, in one embodiment, the diameter / characteristic channel side length of the conduits can be only a few millimeters, such as on the order of about one millimeter. The reactor media component, such as the monolith or alternative bed media, can provide channels containing filler having an average wetted surface area per unit volume of 50 ft based on the volume of the first reactor used to transport the reactants. -1 Up to 3000ft -1 (About 0.16km -1 About 10km -1 ), or 100ft -1 Up to 2500ft -1 (about 0.32km -1 About 8.2km -1 ) or 200ft -1 Up to 2000ft -1 (about 0.65km -1 About 6.5km -1 ). These relatively high surface area per unit volume values ​​can help achieve relatively rapid temperature changes through the reactor, as generally demonstrated by the relatively steep slopes in the exemplary temperature gradient graphs shown in Figures 1(a) or 1(b) of Figure 1.

[0069] The reactor medium component may also provide channels containing fillers having high volumetric heat transfer coefficients (e.g., 0.02 cal / cm 3 s℃ or higher, or 0.05cal / cm 3 s℃ or higher or 0.10cal / cal / cm3 s°C or higher); it has low resistance to flow (low pressure drop); its operating temperature range coincides with the highest temperature encountered during regeneration; it has high resistance to thermal shock; and / or it has a high bulk heat capacity (e.g., 0.10 cal / cm 3 s℃ or higher or 0.20cal / cm 3 s°C or higher). As with high surface area values, these relatively high volumetric heat transfer coefficient values ​​and / or other characteristics can help achieve relatively rapid temperature changes through the reactor, as generally demonstrated by the relatively steep slopes in the exemplary temperature gradient graphs in Figures 1(a) and 1(b) of Figure 1. The values ​​cited are average values ​​based on the volume of the reactor used to transport the reactants.

[0070] In various aspects, a sufficient heat transfer rate can be characterized by a heat transfer parameter ΔTHT of less than 500° C., or less than 100° C., or less than 50° C. As used herein, the parameter ΔTHT is the ratio of the average volumetric heat transfer rate of the bed required for recuperation to the volumetric heat transfer coefficient hv of the bed. The volumetric heat transfer rate (e.g., cal / cm2) sufficient for recuperation is 3 sec) can be calculated as the product of the gas flow rate (e.g., grams per second) and the gas heat capacity (e.g., cal / g °C) and the expected end-to-end temperature change (excluding any reactions, e.g., °C), and this amount can then be divided by the volume of the reactor (or portion of the reactor) that the gas passes through (e.g., cm 3 The volumetric heat transfer coefficient hv of a bed can usually be calculated as an area-based coefficient (e.g., cal / cm 2 s℃) and heat transfer specific surface area (av, e.g. cm 2 / cm 3 ) is usually called the wetted area of ​​the filler.

[0071] Multi-zone catalyst system

[0072] In some aspects, reforming can be further improved by using a variety of catalysts in the catalyst system. In such aspects, different regions of the reaction zone can contain different catalysts. Due to the nature of the countercurrent reactor, a temperature distribution can be formed in the reactor so that some reaction zones are at higher temperatures, while other reaction zones are at lower temperatures. By using a catalyst system comprising a variety of catalysts, the catalyst in the reaction zone can be selected to provide improved activity based on the temperature distribution for the temperature in the reaction zone.

[0073] Figure 4An example of a temperature profile obtained during steam reforming of a methane feed in a 12 inch (about 30 cm) pilot scale countercurrent reactor is shown. The pilot scale reactor contains multiple catalyst zones, wherein the first (higher temperature) zone contains a nickel-based catalyst and the second (lower temperature) zone contains a rhodium-based catalyst. Figure 4 The reforming zone of the reactor corresponds to the 4-12 inches of the reactor. The 0-4 inch portion of the reactor corresponds to the inlet end of the reactor for the regeneration gas stream. The location about 4 inches into the reactor corresponds to the location where the regeneration gas stream is burned. Figure 4 As shown, the temperature distribution at the end of the regeneration step is higher than the temperature distribution at the end of the reforming step. This is due to the cycle of consuming heat during the reforming period and then replenishing it during the regeneration period. However, the overall shape of the temperature distribution is similar after both the reforming and regeneration steps. It is believed that the general shape of the temperature distribution also exists at intermediate times.

[0074] based on Figure 4 An example of a temperature profile is shown, during operation of a countercurrent reactor for performing reforming, with certain zones in the reactor at higher temperatures and other zones in the reactor at intermediate or lower temperatures. Because the locations of the high, intermediate, and low temperature zones are relatively stable during a reaction cycle, it has been discovered that further benefits can be obtained by using a catalyst having improved activity for various temperatures in a given zone of the reactor.

[0075] When multiple catalyst zones are used in the reactor, any convenient number of zones may be used. Thus, when multiple catalyst zones are present, the number of catalyst zones may be in the range of 2 zones to 10 zones, or 2 zones to 6 zones, or 3 zones to 10 zones, or 3 zones to 6 zones. Of course, since it is also possible to have a single catalyst zone, in some aspects, the number of catalyst zones may be in the range of 1 zone to 10 zones, or 1 zone to 6 zones.

[0076] Figure 4 The temperature distribution in can be used to illustrate the concept of using multiple catalyst zones. Figure 4 One way to define the temperature distribution of the catalyst zone may be to use two zones corresponding to a high temperature catalyst zone and a low temperature catalyst zone. Figure 4 In a reactor with a temperature distribution in the reactor, 4-6 inches (or 4-7 inches) of the reactor can correspond to the high temperature zone, and 6-12 inches (or 7-12 inches) of the reactor can correspond to the low temperature zone. Another option is to use three zones, namely a high temperature zone, a medium temperature zone, and a low temperature zone. For example, for a reactor for generating Figure 4In a reactor with a medium temperature distribution, 4-6 inches can correspond to a high temperature zone, 6-9 inches can correspond to a medium temperature zone, and 9-12 inches can correspond to a low temperature zone. Other options for organizing the reactor into two zones, three zones, four zones, or any other convenient number of zones are also available, depending on the desired catalyst system and the temperature distribution of the reactor.

[0077] In some aspects, when different catalyst systems are used in different zones, the zones can be characterized based on the peak temperatures in the different zones. For example, the peak temperature in the first zone can be 100°C or more, or 200°C or more, or 300°C or more, such as up to 700°C or possibly still higher, than the peak temperature in the second zone. The peak temperature in a zone refers to the position in the zone with the highest average temperature at the end of the regeneration step. The average temperature at a certain position at the end of the regeneration cycle can be calculated based on averaging the temperature at the end of the regeneration step in 10 complete cycles.

[0078] Process Example - Countercurrent Reforming and Regeneration

[0079] In various aspects, the reforming of hydrocarbons can be carried out under steam reforming conditions in the presence of H2O, under dry reforming conditions in the presence of CO2, or under conditions where both H2O and CO2 exist in a reaction environment. As a general overview of operations during reforming in a swing reactor such as a countercurrent reactor, a part of a regeneration step or reaction cycle can be used to provide heat for the reactor. Then, during a part of the reforming step or cycle, reforming can occur in the reactor, wherein the reforming reaction consumes the heat provided during the reactor regeneration step. During reactor regeneration, fuel and oxidant are introduced into the reactor from the regeneration end of the reactor. The bed and / or monolith in the regeneration part of the reactor can absorb heat, but generally do not contain a catalyst for reforming. When the fuel and oxidant pass through the regeneration part, heat is transferred from the regeneration section to the fuel and oxidant. Combustion does not occur immediately, but the position of combustion is controlled to occur in the middle part of the reactor. During the regeneration step, the flow of reactants continues, causing the heat generated by combustion to be transferred to the reforming end of the reactor in addition.

[0080] After a sufficiently long period of time, the combustion reaction stops. Any remaining combustion products and / or reactants can be optionally removed. Then a part of the reforming step or reaction cycle can be started. The reactants for reforming can be introduced into the reforming end of the reactor, and therefore relative to the flow during regeneration, it actually flows in the opposite direction. The bed and / or monolith in the reforming part of the reactor can include a catalyst for reforming. In various aspects, at least a portion of the catalyst can correspond to a catalyst formed by the ceramic composition described herein. When reforming occurs, the heat introduced into the reforming zone during combustion may be consumed by the endothermic reforming reaction. After leaving the reforming zone, the reforming product (and unreacted reactants) is no longer exposed to the reforming catalyst. When the reforming product passes through the regeneration zone, heat can be transferred from the product to the regeneration zone. After a sufficiently long period of time, the reforming process can be stopped, the remaining reforming product can be optionally collected or removed from the reactor, and the cycle can be started again by the regeneration step.

[0081] The reforming reaction carried out in the reactor may correspond to the reforming of methane and / or other hydrocarbons using steam reforming in the presence of H2O; using dry reforming in the presence of CO2; or using "dual" reforming in the presence of both H2O and CO2. Examples of the stoichiometry of steam reforming, dry reforming, and "dual" reforming of methane are shown in equations (1) to (3).

[0082] (1) Dry reforming: CH4+CO2=2CO+2H2

[0083] (2) Steam reforming: CH4+H2O=CO+3H2

[0084] (3) Double preparation: 3CH4+2H2O+CO2=4CO+8H2.

[0085] As shown in equations (1) to (3), dry reforming can produce a lower H2 to CO ratio than steam reforming. Reforming reactions performed with steam alone can typically produce an H2 to CO ratio of about 3, such as 2.5 to 3.5. In contrast, reforming reactions performed in the presence of CO2 can produce much lower ratios, perhaps approaching an H2 to CO ratio of about 1.0 or even lower. By using a combination of CO2 and H2O during reforming, the reforming reaction can potentially be controlled to produce a wide variety of H2 to CO ratios in the resulting syngas.

[0086] It should be noted that the ratio of H2 to CO in the syngas also depends on the water-gas shift equilibrium. Although the above stoichiometry shows a ratio of about 1 or about 3 for dry reforming and steam reforming, respectively, the balance of H2 and CO in the syngas may differ from the reaction stoichiometry. The balance may be determined based on the water-gas shift equilibrium, which relates the concentrations of H2, CO, CO2, and H2O based on the reaction

[0087] (4) H2O+CO<=>H2+CO2

[0088] Most reforming catalysts, such as rhodium and / or nickel, can also be used as water-gas shift catalysts. Therefore, if the reaction environment for producing H2 and CO also contains H2O and / or CO2, the initial stoichiometry from the reforming reaction can be changed based on the water-gas shift equilibrium. This balance is also temperature-dependent, with higher temperatures being favorable for producing CO and H2O. It should be noted that higher temperatures can also increase the speed for reaching equilibrium. Therefore, the ability to carry out reforming reactions at elevated temperatures can potentially provide several benefits. For example, instead of steam reforming in an environment with excess H2O, CO2 can be added to the reaction environment. This can both reduce the ratio of H2 to CO produced based on dry reforming stoichiometry and reduce the ratio of H2 to CO produced based on water-gas shift equilibrium. Alternatively, if a higher H2 to CO ratio is required, CO2 can be removed from the environment, and the ratio of H2O to CH4 (or other hydrocarbons) can be controlled to produce the desired type of synthesis gas. By selecting appropriate amounts of feed components, this can potentially allow the production of synthesis gas with a H2 to CO ratio of 0.1 to 15, or 0.1 to 3.0, or 0.5 to 5.0, or 1.0 to 10.

[0089] The reforming reaction shown in equations (1) to (3) is an endothermic reaction. One challenge in industrial-scale reforming may be to provide heat for carrying out the reforming reaction in an efficient manner while reducing or minimizing the introduction of additional components into the desired synthesis gas product. A cyclic reaction system, such as a countercurrent reactor system, can provide heat in a desired manner by having a cycle comprising a reforming step and a regeneration step. During the regeneration step, combustion can be carried out in a selected region of the reactor. The gas flow during regeneration can help to transfer this heat from the combustion zone to another part of the reforming zone in the reactor. The reforming step in the cycle can be a separate step, so that the products from combustion can be reduced or minimized from being incorporated into the reactants and / or the products from the reforming. The reforming step may consume heat, which may reduce the temperature of the reforming zone. When the products from the reforming pass through the reactor, the reforming products can pass through a second zone lacking a reforming or water-gas shift catalyst. This can allow the reaction products to cool before leaving the reactor. The heat transferred from the reforming products to the reactor can then be used to increase the temperature of the reactants to carry out the next combustion or regeneration step.

[0090] A common source of methane is natural gas. In some applications, natural gas, including relevant hydrocarbons and impurity gases, can be used as feedstock for reforming reactions. The natural gas supplied can also be desulfurized and / or dehydrated natural gas. Natural gas generally contains associated gases of various concentrations, such as ethane and other alkanes, preferably at a concentration lower than that of methane. The natural gas supplied may contain impurities, such as H2S and nitrogen. More generally, the hydrocarbon feed for reforming can contain any convenient combination of methane and / or other hydrocarbons. Optionally, the reforming feed can also contain some hydrocarbon-containing compounds, such as alcohols or mercaptans, which are similar to hydrocarbons but contain one or more heteroatoms different from carbon and hydrogen. In some aspects, the other components present in the feed can correspond to impurities, such as sulfur that can be adsorbed onto the catalytic monolith during the reduction cycle (such as the reforming cycle). Such impurities can be oxidized to form sulfur oxides in subsequent cycles, and the sulfur oxides are then reduced to release other sulfur-containing components (or other impurity-containing components) in the reaction environment.

[0091] In some aspects, the feed for reforming may contain 5 wt% or more C 2+Compounds (such as ethane or propane), or 10wt% or more, or 15wt% or more, or 20wt% or more, such as up to 50wt% or possibly still higher. It should be noted that nitrogen and / or other gases that are not reactive in the combustion environment, such as H2O and CO2, may also be present in the feed for reforming. In terms of the reformer corresponding to an on-board reforming environment, such non-reactive products may optionally be introduced into the feed, for example, based on exhaust gas recirculation to the reformer. Additionally or alternatively, the feed for reforming may contain 40wt% or more, or 60wt% or more, or 80wt% or more or 95wt% or more of methane, such as a feed having essentially composed of methane (98wt% or more). In terms of reforming corresponding to steam reforming, the molar ratio of steam molecules to carbon atoms in the feed may be 0.3 to 4.0. It should be noted that methane has 1 carbon atom per molecule, while ethane has 2 carbon atoms per molecule. In aspects where the reforming corresponds to dry reforming, the molar ratio of CO2 molecules to carbon atoms in the feed may range from 0.05 to 3.0.

[0092] In the reforming zone of a countercurrent reactor, due to the nature of the way heat is added to the reactor and / or due to the kinetics of the reforming reaction, the temperature can vary throughout the zone. The highest temperature portion of the zone can usually be found near the middle portion of the reactor. This middle portion can be referred to as a mixing zone, and combustion begins in the mixing zone during regeneration. If the monolith with the reforming catalyst extends into the mixing zone, at least a portion of the mixing zone may correspond to a portion of the reforming zone. Therefore, the position where combustion begins during regeneration is usually close to the end of the reforming zone in the reactor. Moving from the center of the reactor to the end of the reactor, the temperature may decrease. Therefore, the temperature at the beginning of the reforming zone (at the end of the reactor) may be lower than the temperature at the end of the reforming zone (the middle portion of the reactor).

[0093] As the reforming reaction occurs, the temperature in the reforming zone can be reduced. The rate at which the temperature is reduced can be related to the amount of hydrocarbons that can be used for reforming and / or the kinetic factors of the temperature at a given position in the reforming zone. When the reforming feed moves through the reforming zone, the reactants in the feed may be consumed, which can reduce the amount of reforming that occurs at the downstream position. However, when reactants move through the reforming zone, the temperature increase in the reforming zone can increase the reaction rate.

[0094] In some aspects, at about 500 ℃, the reaction rate for reforming can be sufficiently reduced so that little or no additional reforming occurs. Therefore, in some aspects, as the reforming reaction is carried out, the beginning part of the reforming zone can be sufficiently cooled to effectively stop the reforming reaction in a part of the reforming zone. This can move the position where the reforming starts in the reactor to a position further downstream relative to the starting point of the reforming zone. When the temperature of a sufficient part of the reforming zone is lower than 500 ℃ or lower than 600 ℃, the reforming step in the reaction cycle can be stopped to allow regeneration. Alternatively, based on the heat introduced into the reactor during regeneration, the reforming part of the reaction cycle can be stopped based on the amount of reaction time, so that the heat consumed during reforming (plus the heat lost to the environment) is roughly balanced with the heat increased during regeneration. After the reforming process stops, before the regeneration step of the reaction cycle is started, any remaining synthesis gas product still in the reactor can be optionally recovered.

[0095] In other aspects, the conditions for switching from reforming to regeneration can be based on the temperature in the region where Pd is at least a part of the catalyst system. In such aspects, the reforming step can be stopped so that the lowest temperature in the region where Pd is at least a part of the catalyst system is 900°C or higher, or 950°C or higher, or 1000°C or higher, such as up to 1200°C or possibly still higher. In this type of aspect, when the region where Pd is at least a part of the catalyst system is exposed to oxidation conditions, the region is maintained at a temperature of 900°C or higher. It should be noted that in some aspects, a region containing Pd in ​​the catalyst system can be maintained at 900°C or higher temperatures (such as up to 1300°C), while the second region can also contain Pd, but when the second region is exposed to the regeneration process (and / or other oxidation conditions), the temperature in the second region can be allowed to drop below 900°C. In other aspects, when all regions containing Pd in ​​the catalyst system are exposed to regeneration process / oxidation conditions, the region can be maintained at 900°C (and up to 1300°C).

[0096] Then the regeneration process can be started. During regeneration, fuels such as methane, natural gas or H2 and oxygen can be introduced into the reactor and burned. The position allowing the fuel and oxidant to mix can be controlled in any convenient way (such as by introducing fuel and oxidant through a separate channel). By delaying combustion during regeneration until the reactants reach the center of the reactor, the non-reforming end of the reactor can be maintained at a lower temperature. This may also produce a temperature peak in the middle of the reactor. The temperature peak may be located in a part of the reactor that also includes a reforming catalyst. During the regeneration cycle, the temperature in the reforming reactor can be increased to be enough to allow reforming during the reforming part of the cycle. This may cause the peak temperature in the reactor to be 1100°C or higher, or 1200°C or higher, or 1300°C or higher or potentially still higher temperatures. In some aspects, for the region where Pd is a part of the catalyst system, the peak temperature may be between 1100°C and 1300°C.

[0097] The relative time length and reactant flow rate of the reforming part and the regeneration part of the process cycle can be selected to balance the heat provided during the regeneration period and the heat consumed during the reforming period. For example, a selection can be to select a reforming step with a similar length to the regeneration step. Based on hydrocarbons, H2O and / or CO2 flow rate during the reforming step, the endothermic demand of the reforming reaction can be determined. This heat demand can then be used to calculate the flow rate of the combustion reactants during the regeneration step. Of course, in other aspects, the heat balance between reforming and regeneration can be determined in other ways, such as by determining the expected flow rate of the reactants, and then select the cycle length so that the heat provided by the regeneration is balanced with the heat consumed during the reforming period.

[0098] In addition to providing heat, the reactor regeneration step during the reaction cycle can also allow coke to be removed from the catalyst in the reforming zone. In various fields, one or more types of catalyst regeneration may occur during the regeneration step. A type of catalyst regeneration may correspond to removing coke from the catalyst. During reforming, a part of the hydrocarbon introduced into the reforming zone can form coke, rather than forming CO or CO2. This coke may hinder the catalytic sites (such as metal sites) entering the catalyst. In some aspects, in the part of the reforming zone exposed to higher temperatures, such as the part of the reforming zone exposed to 800 ℃ or higher or 900 ℃ or higher or 1000 ℃ or higher temperatures, the formation rate can increase. During the regeneration step, as the temperature of the reforming zone increases, oxygen may be present. At the temperature reached during the regeneration period, at least a portion of the coke generated during the reforming period can be removed as CO or CO2.

[0099] Due to the temperature variation in the entire reactor, several options can be used to characterize the temperature in the reactor and / or the reforming zone of the reactor. One option for characterizing the temperature can be based on the average bed temperature or average monolith temperature in the reforming zone. In a practical setting, it is necessary to have a measuring device, such as a thermocouple, to determine the temperature in the reactor. Instead of trying to measure the temperature in the reforming zone, the average (bed or monolith) temperature in the reforming zone can be defined based on the average value of the temperature at the beginning of the reforming zone and the temperature at the end of the reforming zone. Another option can be to characterize the peak temperature in the reforming zone after the regeneration step in the reaction cycle. Typically, the peak temperature can occur at or near the end of the reforming zone and can depend on the position where combustion starts in the reactor. Still another option can be to characterize the temperature difference at a given position in the reaction zone at different times in the reaction cycle. For example, the temperature difference between the temperature at the end of the regeneration step and the temperature at the end of the reforming step can be determined. Such temperature differences can be characterized at the peak temperature position in the reactor, the inlet of the reforming zone, the outlet of the reforming zone, or any other convenient position.

[0100] In various aspects, the reaction conditions for reforming the hydrocarbons may include one or more of the following: an average reforming zone temperature in the range of 400°C to 1200°C (or higher); a peak temperature within the reforming zone of 800°C to 1500°C; a temperature difference at the peak temperature location between the end of the regeneration step and the end of the subsequent reforming step of 25°C or more, or 50°C or more, or 100°C or more, or 200°C or more, such as up to 800°C or possibly still higher; a temperature difference at the inlet of the reforming zone between the end of the regeneration step and the end of the subsequent reforming step of 25°C or more, or 50°C or more, or 100°C or more, or 200°C or more, such as up to 800°C or possibly still higher; and / or a temperature difference at the outlet of the reforming zone between the end of the regeneration step and the end of the subsequent reforming step of 25°C or more, or 50°C or more, or 100°C or more, or 200°C or more, such as up to 800°C or possibly still higher. Additionally or alternatively, at least one zone containing Pd as part of the catalyst system may be maintained at a temperature between 900°C and 1300°C.

[0101] With respect to the average reforming zone temperature, in various aspects, the average temperature of the reforming zone can be from 500° C. to 1500° C., or from 400° C. to 1200° C., or from 800° C. to 1200° C., or from 400° C. to 900° C., or from 600° C. to 1100° C., or from 500° C. to 1000° C. In some aspects where the entire catalyst system comprises Pd, the average temperature in the reforming zone can be from 900° C. to 1200° C. Additionally or alternatively, with respect to the peak temperature of the reforming zone (which may correspond to a location in the reforming zone close to the location for combustion of the regeneration reactants), the peak temperature can be from 1000° C. to 1400° C., or from 1200° C. to 1500° C., or from 1200° C. to 1400° C., or from 1000° C. to 1300° C., or from 1100° C. to 1300° C.

[0102] Additionally or alternatively, the reaction conditions for reforming the hydrocarbons may include a pressure of 0 psig to 1500 psig (10.3 MPa), or 0 psig to 1000 psig (6.9 MPa), or 0 psig to 550 psig (3.8 MPa); and 1000 hr -1 Up to 50,000hr -1 The gas hourly space velocity of the reforming reactants. The space velocity corresponds to the volume of the reactants per unit time relative to the volume of the monolith. The volume of the monolith is defined as the volume of the monolith as if it were a solid cylinder.

[0103] In some aspects, the advantage of operating the reforming reaction at elevated temperatures can be that substantially all of the methane and / or other hydrocarbons in the reforming feed can be converted. For example, for a reforming process (i.e., steam reforming or double reforming) in which water is present in the reforming reaction environment, reaction conditions can be suitable for converting 10wt% to 100wt%, or 20wt% to 80wt%, or 50wt% to 100wt%, or 80wt% to 100wt%, or 10wt% to 98wt% or 50wt% to 98wt% of methane in the reforming feed. Additionally or alternatively, reaction conditions can be suitable for converting 10wt% to 100wt%, or 20wt% to 80wt%, or 50wt% to 100wt%, or 80wt% to 100wt%, or 10wt% to 98wt% or 50wt% to 98wt% of hydrocarbons in the reforming feed.

[0104] In other aspects, for reforming processes in which carbon dioxide is present in the reforming reaction environment (i.e., dry reforming or dual reforming), the reaction conditions may be suitable for converting 10 wt% to 100 wt%, or 20 wt% to 80 wt%, or 50 wt% to 100 wt%, or 80 wt% to 100 wt%, or 10 wt% to 98 wt% or 50 wt% to 98 wt% of the methane in the reforming feed. Additionally or alternatively, the reaction conditions may be suitable for converting 10 wt% to 100 wt%, or 20 wt% to 80 wt%, or 50 wt% to 100 wt%, or 80 wt% to 100 wt%, or 10 wt% to 98 wt% or 50 wt% to 98 wt% of the hydrocarbons in the reforming feed.

[0105] In some alternative aspects, the reforming reaction can be carried out under dry reforming conditions, wherein the reforming is carried out with CO2 as a reactant, but the amount of H2O in the reaction environment is reduced or minimized. In such alternative aspects, the goal of the reforming reaction can be to produce a synthesis gas having a ratio of H2 to CO of 1.0 or less. In some aspects, the temperature during reforming can correspond to the temperature range described for steam reforming. Optionally, in some aspects, the dry reforming reaction can be carried out at a lower temperature of 500°C to 700°C or 500°C to 600°C. In such aspects, the ratio of H2 to CO can be 0.3 to 1.0, or 0.3 to 0.7 or 0.5 to 1.0. Carrying out a dry reforming reaction under these conditions may also result in a large amount of coke being produced, which may require removal of coke during regeneration to maintain catalytic activity.

[0106] Example of a countercurrent reactor configuration

[0107] For endothermic reactions operating at elevated temperatures, such as hydrocarbon reforming, a countercurrent reactor can provide a suitable reaction environment to provide heat for the endothermic reaction.

[0108] In a countercurrent reactor, the heat required for the endothermic reaction can be provided by generating high temperature hot bubbles in the middle of the reactor. A two-step process can then be used, in which (a) heat is added to the reactor bed or monolith by in-situ combustion, and then (b) heat is removed from the bed in situ by an endothermic process such as reforming, pyrolysis or steam cracking. This type of configuration can provide the ability to consistently manage and limit high temperature bubbles in a reactor region that can tolerate such conditions for a long time. A countercurrent reactor system can allow the main endothermic and regeneration processes to be carried out in a substantially continuous manner.

[0109] The countercurrent reactor system can include a first reactor and a second reactor, which are oriented in a mutually serial relationship relative to a common flow path, and are optionally but preferably oriented along a common axis. The common axis can be horizontal, vertical, or other directions. During the regeneration step, reactants (e.g., fuel and oxygen) are allowed to combine or mix in the reaction zone to burn in situ therein, and produce a high temperature zone or hot bubbles in the middle of the reactor system. Hot bubbles can correspond to a temperature that is at least about the initial temperature of the reaction of endothermic reaction. Typically, the temperature of the hot bubbles can be higher than the initial temperature of the endothermic reaction, because as heat is transferred from the hot bubbles in the middle of the reactor to the end of the reactor, the temperature will be reduced. In some aspects, the combination can be enhanced by a reactant mixer of mixed reactants to promote substantially complete combustion / reaction at a desired position, wherein the mixer is optionally located between the first reactor and the second reactor. The combustion process can continue for a sufficiently long duration that the flow of the first reactant and the second reactant through the first reactor also serves to displace most of the heat generated by the reaction (e.g., hot bubbles) into the second reactor as desired and at least partially through the second reactor, but preferably not all the way through the second reactor to avoid heat waste and overheating of the second reactor. The flue gas can be exhausted through the second reactor, but preferably most of the heat is retained within the second reactor. The amount of heat displaced into the second reactor during the regeneration step can also be limited or determined by the desired exposure time or space velocity of the hydrocarbon feed gas in the endothermic reaction environment.

[0110] After regenerating or heating the second reactor medium (such as the phase-stable monolith described herein), in the next / reverse step or cycle, the reactant methane (and / or natural gas and / or another hydrocarbon) for the endothermic reaction can be supplied or flowed through the second reactor from a direction opposite to the flow direction during the heating step. For example, in a reforming process, methane (and / or natural gas and / or another hydrocarbon) can be supplied or flowed through the second reactor. The methane can contact the hot second reactor and mixer medium in the hot bubble region to transfer heat to the methane as reaction energy.

[0111] For some aspects, the basic two-step asymmetric cycle of the countercurrent regenerative bed reactor system is described in Figures 1 (a) and 1 (b) of Figure 1 according to a reactor system with two zones / reactors; the two zones / reactors are the first or recuperator / quench zone (7) and the second or reaction zone (1). Both the reaction zone (1) and the recuperator zone (7) can contain regeneration monoliths and / or other regeneration structures. As used herein, regeneration monoliths or other regeneration structures include materials that can effectively store and transfer heat and can effectively carry out chemical reactions. Regeneration monoliths and / or other structures can correspond to any convenient type of material suitable for storing heat, transferring heat and catalyzing reactions. Examples of structures can include mats or packing materials, ceramic beads or balls, ceramic honeycomb materials, ceramic tubes, extruded monoliths, etc., provided that they can maintain integrity, functionality, and can withstand long-term exposure to temperatures exceeding 1200°C, or exceeding 1400°C, or exceeding 1600°C, which can allow some operating margin.

[0112] For ease of describing Figure 1, the reactor is described herein with reference to a reforming reaction. It should be understood that other convenient types of endothermic reactions may generally be performed using a countercurrent reactor such as the reactor shown in Figure 1.

[0113] As shown in FIG. 1( a) of FIG. 1 , at the beginning of the "reacting" step of the cycle, the secondary end 5 of reaction zone 1 (also referred to herein as the second reactor) can be at an elevated temperature compared to the primary end 3 of reaction zone 1, and at least a portion (including the first end 9) of the recuperator or quench zone 7 (also referred to herein as the first reactor) can be at a lower temperature than reaction zone 1 to provide a quenching effect on the resulting product. In one aspect where the reactor is used to perform countercurrent reforming, a reactant feed containing methane (or other hydrocarbon-containing reactant feed) can be introduced into the primary end 3 of the reforming or reaction zone 1 via conduit 15. In various aspects, the hydrocarbon-containing reactant feed can also contain H2O, CO2, or a combination thereof.

[0114] The feed stream from inlet 15 can absorb heat from reaction zone 1 and react endothermically to produce the desired synthesis gas product. As this step proceeds, as indicated by the arrows, a movement of the temperature distribution 2 can be generated based on the heat transfer characteristics of the system. When the ceramic catalyst monolith / other catalyst structure is designed to have sufficient heat transfer capacity, this distribution can have a relatively steep temperature gradient, which can move through reaction zone 1 as the reforming step proceeds. In some aspects, a steeper temperature gradient distribution can provide improved control of reaction conditions. In terms of carrying out another type of endothermic reaction, a similar temperature distribution change can occur so that as the reaction step proceeds, the temperature gradient moves through reaction zone 1.

[0115] The effluent from the reforming reaction, which may contain unreacted feed components (hydrocarbons, H2O, CO2) as well as synthesis gas components, may exit the reaction zone 1 through the secondary end 5 at an elevated temperature and pass through the recuperator reactor 7, entering through the second end 11, and exiting at the first end 9. The recuperator 7 may initially be at a lower temperature than the reaction zone 1. As the products from the reforming reaction (and optionally unreacted feed) pass through the recuperator zone 7, the gas may be quenched or cooled to a temperature close to the temperature of the recuperator zone substantially located at the first end 9, which in some embodiments may be approximately the same as the temperature of the regeneration feed introduced into the recuperator zone 7 through conduit 19 during the second step of the cycle. As the reforming effluent is cooled in the recuperator zone 7, a temperature gradient 4 may be created in the regeneration bed of the zone and may move through the recuperator zone 7 during this step. The quench may heat the recuperator 7 which may be cooled again in a second step to subsequently provide another quench service and prevent the hot bubbles from growing in size and location through the quench reactor 7. After the quench, the reaction gases may exit the recuperator at 9 via conduit 17 and may be processed to separate and recover the various components.

[0116] The second step of the cycle, referred to as the regeneration step, may begin by reintroducing the first regeneration reactant and the second regeneration reactant through conduit 19. The first reactant and the second reactant may be conveyed separately through the hot recuperator 7 toward a second end 11 of the recuperator 7 where they may be combined in or near a central region 13 of the reactor system for an exothermic reaction or combustion.

[0117] FIG. 1( b) of FIG. 1 shows an example of a regeneration step. Regeneration may require transferring recovered sensible heat from the recuperator zone 7 to the reaction zone 1 to thermally regenerate the reaction bed 1 for a subsequent reaction cycle. The regeneration gas / reactant may enter the recuperator zone 7, for example, through conduit 19, and flow through the recuperator zone 7 and into the reaction zone 1. In doing so, the temperature gradients 6 and 8 may move through the bed as shown by the arrows on the exemplary graph in FIG. 1( b), similar to the temperature gradient graph formed during the reaction cycle in FIG. 1( a) of FIG. 1, but in the opposite direction. The fuel and oxidant reactants may be burned in a region near the interface 13 of the recuperator zone 7 and the reaction zone 1. The heat recovered from the recuperator zone together with the combustion heat may be transferred to the reaction zone, thermally regenerating the regeneration reaction monolith and / or bed 1 disposed therein.

[0118] In some respects, due at least in part to a certain mixing at the first end (17) of the first reactor, several conduits in the passage can convey a mixture of the first reactant and the second reactant. However, the number of conduits conveying the combustible mixture of the first reactant and the second reactant can be sufficiently small so that most of the stoichiometric reactants will not react before leaving the second end of the first reactor. In those conduits conveying the mixture of reactants, the axial initiation position of combustion or exothermic reaction can be controlled by a combination of temperature, time and fluid dynamics. Fuel and oxygen generally require temperature dependence and mixture dependence autoignition time to burn. Nevertheless, a certain reaction may occur in the axial portion of the conduit conveying the mixture of reactants. However, this reaction may be acceptable because the number of channels with such reactions may be sufficiently small so that there is only an acceptable or unimportant level of influence on the total heat balance in the reactor. The design details of a specific reactor system may be selected to reasonably avoid the mixing of reactants in the conduit as much as possible.

[0119] Figure 2 Another exemplary reactor system is presented that may be suitable for use in some applications to control and delay the combustion of fuel and oxidant to achieve efficient regeneration heat. Figure 2 A single reactor system operating in a regeneration cycle is depicted. The reactor system can be considered to include two reactor zones. The recuperator 27 can be a zone where quenching mainly occurs, and a substantially isolated flow path or channel is provided to pass two quenching reaction gases through the reactor medium without causing combustion until the gas reaches the vicinity or interior of the reactor core 13 in FIG. The reformer 2 can be a reactor where regeneration heating and methane (and / or hydrocarbon) reforming mainly occur, and can be considered to be a second reactor for the purposes of this article. Although the first reactor and the second reactor in the reactor system are identified as separate distinguishable reactors, it should be understood that the first reactor and the second reactor can be manufactured, provided or otherwise combined into a common single reactor bed, whereby the reactor system can be described as including only a single reactor integrating two cycles in the reactor. The terms "first reactor" and "second reactor" can refer only to the corresponding zones in the reactor system, where each of the steps of regeneration, reforming, quenching, etc. occurs, and there is no need to use separate components for the two reactors. However, various aspects can include a reactor system, whereby the recuperator reactor includes conduits and channels as described herein, and the reformer reactor can similarly have conduits. Additionally or alternatively, some aspects may include a reformer reactor bed that is arranged differently than the recuperator reactor bed, and may even include different materials than the recuperator reactor bed.

[0120] As previously mentioned, the first reactor or recuperator 27 can include various gas conduits 28 for guiding two or more gases to enter the first end 29 of the recuperator 27 separately and pass through the regeneration bed placed therein. The first gas 30 can enter the first end of multiple flow conduits 28. In addition to providing flow channels, conduit 28 can also include an effective flow barrier (e.g., it is effectively used as a conduit wall) to prevent cross-flow or mixing between the first reactant and the second reactant, and maintain most of the reactants to be effectively separated from each other until mixing is allowed. As previously mentioned, each of the first channel and the second channel can include multiple channels or flow paths. The first reactor can also include a plurality of substantially parallel flow segments, each of which includes the first channel and the second channel isolated.

[0121] In some respects, as described above, the recuperator may include one or more extruded honeycomb monoliths. Each monolith may provide flow channel (e.g., flow path) for one of the first reactant or the second reactant. Each channel preferably includes a plurality of conduits. Alternatively, the monolith may include one or more channels for every kind of reactant, wherein one or more channels or conduit groups are dedicated to the flow of one or more reactant streams, and the remainder of the conduit makes one or more streams of another reactant flow. It should be appreciated that at the interface between the channels, many conduits may convey the mixture of the first reactant and the second reactant, but this conduit quantity is proportionally small.

[0122] Alternative embodiments may use reactor media other than monoliths, such as whereby channel conduits / flow paths may include more tortuous paths (e.g., convoluted, complex, winding and / or twisted, but not linear or tubular), including but not limited to labyrinthine, multiple flow paths, conduits, tubes, slots and / or pore structures having channels through a portion of the reactor, and may include barrier portions, such as along the outer surface of a segment or within a subsegment, substantially impermeable to gases, and / or other devices suitable for preventing cross-flow between the reactant gases and maintaining the first reactant gas and the second reactant gas substantially separated from each other as they pass axially through the recuperator 27. Such other types of reactor media may be suitable, provided that at least a portion of such media can be formed by sintering a ceramic catalytic composition as described herein, followed by exposing such media to reducing conditions to activate the catalyst. For such embodiments, complex flow paths may result in extended effective flow paths, increased surface area and improved heat transfer. Such designs may be preferred for reactor embodiments having relatively short axial lengths through the reactor. Longer axial reactor lengths may experience increased pressure drops through the reactor. However, for such embodiments, the porous and / or permeable medium may comprise, for example, at least one of a packed bed, a tile arrangement, a permeable solid medium, a substantially honeycomb type structure, a fiber arrangement, and a grid type lattice structure.

[0123] In some aspects, a countercurrent reactor can include some type of apparatus or method to direct the flow stream of one reactant into a selected portion of a conduit. Figure 2 In an exemplary embodiment of the present invention, the gas distributor 31 can direct the second gas flow 32 to a second gas flow channel that is substantially isolated from or not in fluid communication with the first gas channel (here shown as channel 33). As a result, at least a portion of the gas flow 33 remains separated from the gas flow 30 during the axial passage of the recuperator 27. In some aspects, the regeneration bed and / or monolith of the recuperator zone may include a channel having a gas or fluid barrier that isolates the first reactant channel from the second reactant channel. Thus, at least two reactant gases passing through the channel arrangement can pass completely through the regeneration bed, thereby quenching the regeneration bed and absorbing heat into the reactant gases before combining and reacting with each other in the combustion zone.

[0124] In various aspects, gas (including fluid) 30 and 32 can each include components reacting with components in another reactant 30 and 32, to produce exothermic reaction when combined.For example, each of the first reactant and the second reactant can include one of fuel gas and oxidant gas, one of fuel gas and oxidant gas burns or burns when combined with another in fuel and oxidant.By keeping reactants basically separated, the position of heat release occurring due to exothermic reaction can be controlled.In some aspects, "basically separated" can be defined as meaning between the first reactant stream and the second reactant stream, at least 50%, or at least 75%, or at least 90% of the reactants with minimum or limited stoichiometric reactive amount, before these gases have completed the point of their axial passage of the recuperator 27, have not been consumed by reaction.In this way, most of the first reactant 30 can be kept isolated from most of the second reactant 32, and most of the heat release from the reaction of the combined reactants 30 and 32 can occur after the reactants begin to leave the recuperator 27. The reactants may be gases, but optionally some reactants may include a liquid phase, a mixture phase, or a vapor phase.

[0125] The reaction percentages of these regeneration streams mean the possible reaction percentages based on the stoichiometry of the overall feed. For example, if gas 30 includes 100 volumes of air (80 volumes of N2 and 20 volumes of O2), and gas 32 includes 10 volumes of hydrogen, then the maximum stoichiometric reaction will be the combustion of 10 volumes of hydrogen (H2) with 5 volumes of oxygen (O2) to produce 10 volumes of H2O. In this case, if 10 volumes of hydrogen are actually burned in the recuperator zone (27), this will indicate 100% reaction of the regeneration stream. Although there is residual unreacted oxygen, this is because in this example, unreacted oxygen exists in an amount exceeding the stoichiometric requirement. Therefore, in this example, hydrogen is the stoichiometrically limited component. Using this definition, during the axial passage of the recuperator (27), less than 50% of the reaction of the regeneration stream, or less than 25% of the reaction, or less than 10% of the reaction can occur.

[0126] In various aspects, channels 28 and 33 may comprise ceramic (including zirconia), alumina, or other refractory materials capable of withstanding temperatures in excess of 1200° C., or 1400° C., or 1600° C. Additionally or alternatively, the wetted area of ​​channels 28 and 33 may be 50 ft -1 Up to 3000ft -1 , or 100ft -1 Up to 2500ft -1 or 200ft -1 Up to 2000ft -1 .

[0127] Referring briefly again to FIG. 1 , the reactor system may include a first reactor 7 and a second reactor 1 , wherein the first reactor has a first end 9 and a second end 11 , and the second reactor has a primary end 3 and a secondary end 5 . The embodiments shown in FIGS. 1 and 2 are simple illustrations provided for explanatory purposes only and are not intended to represent comprehensive embodiments. Reference to the "end" of a reactor refers only to the distal portion of the reactor relative to the axial midpoint of the reactor. Thus, to say that a gas enters or leaves the "end" of a reactor, such as end 9, simply means that the gas may enter or leave at substantially any point along the axis between the respective end face of the reactor and the midpoint of the reactor, but more preferably closer to the end face than the midpoint. Thus, one or both of the first reaction gas and the second reaction gas may enter at the respective end face, while the other may be supplied to the respective end of the reactor through a slot or port on the circumferential or peripheral outer surface on the respective end of the reactor.

[0128] Example 1 - Activity for reforming at elevated temperatures

[0129] The following example demonstrates that a Pd-based catalyst system can provide suitable reforming activity under high temperature conditions. In this example, the catalyst system was tested by loading the catalytic metal on particles of a thermally stable oxide layer. The particles were then placed in a quartz reactor and exposed to a methane stream under steam reforming conditions. The weight hourly space velocity of methane relative to the catalyst particles was approximately 2.0 hr -1 The volume ratio of water to methane was approximately 2.0. The exposure was conducted at atmospheric pressure (approximately 100 kPa-a). No monoliths were used. After exposure of the methane stream to the catalyst, a flame ionization detector (FID) was used to detect any unreacted methane.

[0130] The first catalyst system corresponds to NiO supported on NiAl2O4. The second catalyst system corresponds to Rh supported on α-Al2O3. The third catalyst system corresponds to Pd on α-Al2O3.

[0131] For the first catalyst system (NiO / NiAl2O4), 12.5 mg of the catalyst was placed in a quartz reactor. The catalyst system was initially exposed to a hydrogen stream at 900°C to activate the catalyst. The activated catalyst system was then exposed to a methane stream under steam reforming conditions at 900°C. Figure 5 The FID results of the exhaust gas from the reactor are shown. Figure 5 As shown, a small amount of methane was detected in the reactor off-gas. This corresponds to a methane conversion of approximately 96% over the catalyst exposure.

[0132] In the second run, 5.2 mg of the first catalyst system was placed in a quartz reactor and activated using hydrogen. This smaller amount of activated first catalyst system was then exposed to a methane stream under steam reforming conditions at 900°C. Figure 6 As shown, after exposure to a relatively small portion of the first catalyst system, a large portion of the methane remains unreacted. This corresponds to a methane conversion of approximately 11% over the exposure to the catalyst.

[0133] For the second catalyst system (Rh / α-Al2O3, 4.0 wt% Rh relative to the weight of the catalyst system), 14.7 mg of the catalyst system was placed in a quartz reactor. Rhodium catalysts are usually used at lower temperatures, so the second catalyst system was exposed to a methane stream under steam reforming conditions at 550°C. Figure 7 As shown, only a small amount of unreacted methane was detected by the FID. This corresponds to a methane conversion of approximately 96% for the exposure to the second catalyst system.

[0134] For the third catalyst system (Pd / α-Al2O3, 5.0 wt% Pd relative to the weight of the catalyst system), 5.5 mg of the catalyst system was placed in a quartz reactor. The catalyst system was initially exposed to a hydrogen stream at 900°C to ensure that the Pd was in the metallic form (to activate the catalyst). The activated catalyst system was then exposed to a methane stream under steam reforming conditions at 900°C. Figure 8 The FID results are shown, corresponding to essentially no unreacted methane exiting the reactor. This demonstrates that Pd can provide suitable reforming activity at elevated temperatures (eg, 900°C or higher) to be used as a reforming catalyst.

[0135] Example 2 - Stability of Pd in ​​an oxidizing environment at 900°C to 1300°C

[0136] To demonstrate the oxidation resistance of Pd at temperatures above 900°C, a catalyst system corresponding to 5.0 wt% Pd supported on alumina was placed in a flow cell. The Pd-containing catalyst system was exposed to a flow of 5.0 vol% O2 in a He carrier gas. The catalyst system was initially exposed to the gas flow at 1050°C for 60 minutes. The temperature was then ramped down to a temperature of approximately 100°C over approximately 2 hours.

[0137] During exposure of the catalyst system to the gas stream, the output of the flow cell is analyzed using a thermal conductivity detector (TCD). TCD allows detection of oxygen loss based on changes in conductivity in the output gas stream. Because the alumina in the catalyst system is stable against further oxidation, the oxygen loss in the output gas stream corresponds to the amount of O2 consumed by Pd oxidation.

[0138] Fig.10 The results of exposure of a Pd-containing catalyst system to a gas stream are shown. Fig.10 , the horizontal axis corresponds to the time the catalyst system is exposed to the gas flow. Data line 1010 corresponds to the temperature of the catalyst system during exposure to the gas flow. Data line 1020 represents the TCD signal. It should be noted that for O2 in helium, the consumption of O2 will result in a decrease in the conductivity of the gas flow. To simplify Fig.10 , data line 1020 corresponds to the TCD signal multiplied by -1, so that the position of maximum O2 consumption (and therefore maximum Pd oxidation) corresponds to Fig.10 The peak value in .

[0139] like Fig.10 As shown, during the initial exposure at 1050°C, the TCD signal changes minimally during the first hour of exposure time. This indicates that Pd resists oxidation at temperatures above 900°C, as little or no consumption of O2 occurs. After the initial hour, the temperature was allowed to decrease. Fig.10 As shown, the TCD signal shows a small shoulder peak near 900°C, followed by a large peak. Fig.10 For the gas exposure conditions in the data, maximum oxidation occurs at approximately 540°C. This peak position can vary depending on the reaction conditions. However, the onset of significant oxidation at temperatures below 900°C is a consistent feature of Pd exposed to O2, regardless of the specific gas flow conditions. Fig.10 As shown, O2 consumption ends at a temperature of about 400°C.

[0140] The oxidation resistance of Pd at temperatures above 900°C is unexpected. Traditionally, it is expected that oxidation of a metal in the presence of O2 would increase with increasing temperature. Additionally, even if the metallic form had a higher stability, it would be expected that some oxidation would occur as an equilibrium process. However, as Fig.10 As shown, Pd is unexpectedly resistant to oxidation at temperatures above 900° C. Based on this unexpected resistance, the volatility of the Pd-containing catalyst system can be unexpectedly reduced by avoiding exposure of the Pd-containing catalyst system to oxidative conditions at temperatures between 600° C. and 900° C. Avoiding Pd loss due to catalyst volatility can significantly extend the useful life of the Pd-containing catalyst system.

[0141] Examples 3A, 3B and 3C - Catalyst systems with different starting alumina phases

[0142] This example and the following examples illustrate the benefits of using a thermally stable oxide support layer as part of a catalyst system.The monolith used to support the catalyst system described in this example corresponds to a monolith having 400 cpsi (cells per square inch) and an open frontal area of ​​35% or 52%.

[0143] Three different types of catalyst system washcoat formulations were used to prepare a multi-zone catalyst system for hydrocarbon reforming. In this example, a multi-zone catalyst system was used, with two catalyst zones. The first zone (higher temperature) corresponded to a Ni-containing catalyst, while the second zone (lower temperature) corresponded to a Rh-containing catalyst. In each zone of the pilot scale reactor, two monoliths were used to fill the desired catalyst bed volume, so each catalyst system corresponded to a total of four monoliths.

[0144] For Example 3A, the first two monoliths with a Ni-containing catalyst system were prepared using NiO as the catalytic metal and α-Al2O3 as the oxide support layer. The molar ratio of Al to Ni in the catalyst system was approximately 1.5:1. This type of catalyst system may result in the in-situ formation of NiAl2O4 after exposure to cyclic high temperature reforming conditions. Sufficient carrier coating was applied so that the weight of the NiO / α-Al2O3 catalyst system was approximately 5wt% of the total weight of the washed monolith. For Example 3A, the last two monoliths with a Rh-containing catalyst system were also prepared using α-alumina as the oxide support layer. The Rh / Al2O3 catalyst system contained approximately 4.0wt% Rh relative to the weight of the catalyst system. Sufficient carrier coating was applied so that the weight of the Rh2O3 / α-Al2O3 catalyst system was approximately 4wt% of the total weight of the washed monolith.

[0145] For Examples 3B and 3C, rather than using a catalyst system comprising a phase-stable material, a washcoat containing a higher surface area material was deposited on the monolith. Thus, the washcoat used in Examples 3B and 3C did not comprise a thermally stable metal oxide support layer.

[0146] In Example 3B, the catalyst system used for the first two washcoats corresponds to θ-Al2O3 doped with 4 wt% La and 30% Ni as a catalyst, which is formed at 1200°C. This type of composition can be referred to as 30% Ni-4%-La-θ-Al2O3. This catalyst system corresponds to an Al:Ni molar ratio of 3.7:1. It should be noted that this ratio has a significant amount of excess Al relative to the stoichiometric ratio of NiAl2O4. After the washcoats were deposited, the first two monoliths in Example 3B were calcined at 500°C. For the last two monoliths in Example 3B, a washcoat of 5% Rh on 4%-La-γ-Al2O3 was washcoated onto the alumina-rich monolith. It should be noted that the last two washcoats contain γ-Al2O3, rather than the θ-Al2O3 of the first two washcoats. After the washcoats were deposited, the last two monoliths in Example 3B were calcined at 500°C.

[0147] In Example 3C, the first two washcoats and the last two washcoats were prepared in a similar manner to Example 3B, but the calcination temperature of the first two monoliths was different. In Example 3C, a calcination temperature of 1200°C was used after the washcoat was applied (compared to 500°C for calcination in Example 3B).

[0148] Example 4 - Reforming with Monoliths Having Different Starting Alumina Phases

[0149] The washed monoliths described in Examples 3A, 3B, and 3C were used in a pilot scale reactor to study the change in catalytic activity over time and to determine the structural stability of the washed monoliths. The monoliths were used to steam reform a methane feed under cyclic high temperature conditions. The reaction conditions included a regeneration step and a reforming step. During the regeneration step, air was used to provide a source of oxygen for the combustion of the hydrocarbon fuel. The amount of air was sufficient to provide 10% excess O2 relative to the amount of hydrocarbon fuel used for heating. The regeneration step during each cycle was carried out at a pressure of 150 psig (about 1.0 MPa-g) for approximately 15 seconds. The combustion during the regeneration step was carried out to provide a temperature similar to that of the reforming step. Figure 4 The temperature profile of the temperature profile shown, but at the end of the regeneration step / beginning of the reforming step, the target peak temperature was 1150°C. The reforming step during each cycle was carried out at a pressure of 300 psig (about 2.1 MPa-g) for about 15 seconds, with methane as the hydrocarbon for reforming. The molar ratio of H2O to CH4 in the reforming step feed was 1.3.

[0150] Fig. 9 The average conversion of methane during the reforming step is shown as the process proceeds over a period of 4-6 weeks (right graph). The conversion rate at the end of the reforming step in each cycle is slightly lower due to the effects of cooling in the reactor near the end of the reforming step during a single cycle. This is shown by averaging over the first 10 seconds of each reforming step ( Fig. 9 ) and averaged over the first 15 seconds of each renormalization step ( Fig. 9 It should be noted that shorter reforming steps can be used if it is desired to maintain a higher overall conversion throughout the reforming step.

[0151] like Fig. 9 As shown in the right figure of , both Example 3B and Example 3C initially provided higher conversion than Example 3A. This matches the expected effect of using a higher surface area alumina phase as a support in Examples 3B and 3C. However, as Fig. 9As shown in the right figure of , the conversion activity of the catalysts in Examples 3B and 3C is unstable. Although the data is noisy, it is clear that in Example 3C, the conversion activity of the catalyst begins to decline almost immediately after the start of the run. This decline in activity continues until about 300 hours of cyclic reaction. At this point, the reaction in Example 3C stops due to the rapid loss of activity. The catalytic activity of Example 3B declines more slowly, but Example 3B also experiences a significant decline in activity that begins before 400 hours of operation. Between 400 and 800 hours, an alternative set of cyclic reforming conditions is used that does not Figure 7 3A, but a similar decrease in activity over time was observed. At 800 hours, the process conditions were returned to the initial reforming conditions. By 800 hours, the degradation of the catalyst appeared to have stabilized, although the activity level was significantly lower than the catalyst of Example 3A. Again, this loss of activity is believed to be due to degradation of the catalyst system on the monolith in the reactor, resulting in a loss of available surface area for exposing the methane feed to the catalyst.

[0152] Compared with Example 3B and Example 3C, Fig. 9 The middle right figure shows that the catalyst system in Example 3A maintains similar activity throughout the process run. Without being bound by any particular theory, it is believed that this is because Example 3A corresponds to a) a monolith made of a material that is phase stable under cyclic high temperature reforming conditions and b) the monolith includes an oxide support layer, so that any interaction between the catalyst metal (such as Ni) and the oxide material (such as Al2O3) occurs in the oxide support layer and does not affect the structural integrity of the underlying monolith or other support structures.

[0153] Fig. 9 The left graph in shows similar results. Again, Example 3C initially showed higher activity than Example 3A, but the activity of Example 3C began to decline almost immediately. Examples 3A and 3B initially had similar activities, but only Example 3A maintained the activity. Fig. 9 As shown in the two figures in FIG. 1 , Example 3A maintained substantially the same activity over the 750 hours of operation.

[0154] To further characterize the results of cyclic reforming for the catalyst system and monolith of Example 3A, at the end of the run, alternating oxidation and reduction cycles were maintained while the peak temperature in the reactor was cooled to 1000° C. The reactor was then cooled to room temperature using a N2 stream. After cooling, additional characterization was then performed.

[0155] After cooling, it was initially noted that for the first and second monoliths of Example 3A, the catalyst system was difficult to remove from the underlying monolith. Due to structural decomposition, it is generally relatively easy to separate the catalyst or catalyst system from the monolith when the catalyst or catalyst system does not include a thermally stable metal oxide. However, it was unexpectedly discovered that by using a thermally stable support metal oxide in the catalyst system, strong adhesion of the catalyst system to the monolith can be maintained after long-term exposure to a cyclic high temperature reforming environment.

[0156] After removal, the catalyst systems from Example 3A were characterized using X-ray diffraction (XRD). The XRD spectra showed that all catalyst systems were in a stable phase. For the first monolith, the catalyst system was primarily in a reduced state. This was indicated by the presence of a large number of peaks based on Ni and α-Al2O3 and the presence of a small amount of NiAl2O4. The catalyst system used for the second monolith was more oxidized, with a mixture of Ni, NiO, α-Al2O3, and NiAl2O4. The XRD spectra of the third and fourth monoliths were similar to each other, with both showing primarily Rh and α-Al2O3. Additional microscopic and elemental analyses of the catalyst systems were consistent with the XRD spectra.

[0157] Other embodiments

[0158] Embodiment 1. A method for reforming hydrocarbons in a cyclic reaction environment, the method comprising: exposing a reactant flow comprising reformable hydrocarbons to a catalyst system in a reaction zone within a reactor to form a product flow comprising H2, the reaction zone comprising the catalyst system supported on one or more surfaces of a support structure, the catalyst system comprising Pd in ​​at least a portion of the reaction zone; and reacting a mixture comprising a fuel and 0.1 vol% or more O2 in a combustion zone within the reactor under combustion conditions to heat one or more surfaces in the reaction zone to a regeneration surface temperature of 1000°C to 1300°C, wherein the minimum temperature in at least a portion of the reaction zone at the end of the exposure is 900°C or higher, or wherein the minimum temperature in at least a portion of the reaction zone at the start of the reaction is 900°C or higher, or a combination thereof.

[0159] Embodiment 2. A method according to embodiment 1, wherein the minimum temperature in at least a portion of the reaction zone at the end of the exposure is 900°C or higher; or wherein the minimum temperature in at least a portion of the reaction zone at the start of the reaction is 950°C; or a combination thereof.

[0160] Embodiment 3. A method according to any one of the preceding embodiments, wherein the peak temperature in at least a portion of the reaction zone at the beginning of the exposure is 1300°C or less, or wherein the peak temperature in at least a portion of the reaction zone at the end of the reaction is 1300°C or less, or a combination thereof.

[0161] Embodiment 4. The method according to any one of the preceding embodiments, wherein the flow direction of the reactant flow in the reaction zone is opposite to the flow direction of the mixture.

[0162] Embodiment 5. The method according to any of the preceding embodiments, wherein the catalyst system comprises Ni, Rh, Ru, Pt, Cu, Ir or a combination thereof in the second portion of the reaction zone.

[0163] Embodiment 6. A method according to any of the preceding embodiments, wherein the at least a portion of the reaction zone includes the one or more surfaces in the reaction zone.

[0164] Embodiment 7. The method according to any one of the preceding embodiments, wherein the catalyst system further comprises a metal oxide support layer, the metal oxide support layer comprising stabilized zirconia, perovskite, pyrochlore, spinel, hirconite, zeolite, corundum oxide or a combination thereof.

[0165] Embodiment 8. The method of embodiment 7, wherein the metal oxide support layer is thermally phase stable at 800°C to 1600°C.

[0166] Embodiment 9. The method according to embodiment 7 or 8, a) wherein the catalyst system in at least a portion of the reaction zone further comprises Ni, Rh, Ru, Pt, Cu, Ir or a combination thereof; b) wherein at least a portion of the catalyst system comprises a mixture of the catalyst and the metal oxide support layer; or c) a combination of a) and b).

[0167] Embodiment 10. A method according to any one of Embodiments 7 to 9, i) wherein the metal oxide support layer comprises α-Al2O3, yttria-stabilized zirconia (YSZ), perovskite or a combination thereof; ii) wherein the metal oxide support layer comprises 80 wt% or more of α-Al2O3 relative to the weight of the metal oxide support layer; or iii) a combination of i) and ii).

[0168] Embodiment 11. A method according to any one of Embodiments 7 to 10, further comprising an intermediate bonding layer comprising a metal oxide, wherein a first surface of the intermediate bonding layer contacts at least a portion of the one or more surfaces of the support structure, and the catalyst system is loaded on the surface of the support structure by being at least partially loaded on a second surface of the intermediate bonding layer, and the intermediate bonding layer optionally comprises α-Al2O3.

[0169] Embodiment 12. A method according to any of the preceding embodiments, wherein the support structure comprises a monolith having a cell density of 50 cells / square inch to 900 cells / square inch, or wherein the support structure comprises 80 wt % or more of Al2O3, or a combination thereof.

[0170] Embodiment 13. A method according to any one of the preceding embodiments, further comprising: after the reaction, exposing a second portion of the reactant flow including the reformable hydrocarbon to the catalyst system in the reaction zone within the reactor to form a product flow including H2; and after the exposing of the second portion of the reactant flow, reacting the second portion of the mixture including fuel and 0.1 vol% or more O2 in the combustion zone within the reactor under combustion conditions to heat the one or more surfaces in the reaction zone to a regeneration surface temperature of 1000°C to 1300°C, wherein the lowest temperature in at least a portion of the reaction zone is 900°C or higher at the end of the exposing of the second portion of the reactant flow, or wherein the lowest temperature in at least a portion of the reaction zone is 900°C or higher at the start of the reacting of the second portion of the mixture, or a combination thereof.

[0171] Embodiment 14. A method according to any of the preceding embodiments, wherein the catalyst system comprises 0.1 wt% to 10 wt% Pd relative to the weight of the catalyst system, or wherein the catalyst system comprises 0.5 wt% to 6.0 wt% Pd relative to the weight of the catalyst system.

[0172] Embodiment 15. The method of claim 1, wherein the catalyst system comprises a catalyst system calcined at a temperature of 900°C to 1500°C prior to the reacting.

[0173] While the present invention has been described and illustrated with reference to particular embodiments, those skilled in the art will appreciate that the present invention lends itself to variations not necessarily illustrated herein. Therefore, reference should then be made solely to the appended claims to determine the true scope of the present invention.

Claims

1. A method for reforming hydrocarbons in a cyclic reaction environment, the method comprising: Exposing a reactant stream comprising reformable hydrocarbons to a catalyst system in a reaction zone within a reactor to form a product stream comprising H2, the reaction zone comprising the catalyst system supported on one or more surfaces of a support structure, the catalyst system comprising Pd in ​​at least a portion of the reaction zone; and reacting a mixture comprising a fuel and 0.1 vol% or more O2 in a combustion zone within the reactor under combustion conditions to heat one or more surfaces in the reaction zone to a regeneration surface temperature of 1000°C to 1300°C, wherein the minimum temperature in at least a portion of the reaction zone at the end of the exposure is 900°C or higher, or wherein the minimum temperature in at least a portion of the reaction zone at the start of the reaction is 900°C or higher, or a combination thereof.

2. The method of claim 1, wherein the minimum temperature in at least a portion of the reaction zone at the end of the exposing is 900° C. or higher; or wherein the minimum temperature in at least a portion of the reaction zone at the start of the reaction is 950° C.; or a combination thereof.

3. The method of any one of the preceding claims, wherein the peak temperature in the at least a portion of the reaction zone at the start of the exposing is 1300°C or less, or wherein the peak temperature in the at least a portion of the reaction zone at the end of the reaction is 1300°C or less, or a combination thereof.

4. A method according to any one of the preceding claims, wherein the flow direction of the reactant stream within the reaction zone is reversed relative to the flow direction of the mixture.

5. The process of any one of the preceding claims, wherein the catalyst system comprises Ni, Rh, Ru, Pt, Cu, Ir, or a combination thereof in the second portion of the reaction zone.

6. The method of any one of the preceding claims, wherein the at least a portion of the reaction zone comprises the one or more surfaces in the reaction zone.

7. The method according to any one of the preceding claims, wherein the catalyst system further comprises a metal oxide support layer, the metal oxide support layer comprising stabilized zirconia, perovskite, pyrochlore, spinel, hirconite, zeolite, corundum group oxides or combinations thereof.

8. The method of claim 7, wherein the metal oxide support layer is thermally phase stable at 800°C to 1600°C.

9. The process of claim 7 or 8, a) wherein the catalyst system in at least a portion of the reaction zone further comprises Ni, Rh, Ru, Pt, Cu, Ir or a combination thereof; b) wherein at least a portion of the catalyst system comprises a mixture of a catalyst and the metal oxide support layer; or c) a combination of a) and b).

10. The method of any one of claims 7 to 9, i) wherein the metal oxide support layer comprises α-Al2O3, yttria-stabilized zirconia (YSZ), perovskite, or a combination thereof; ii) wherein the metal oxide support layer comprises 80 wt% or more of α-Al2O3 relative to the weight of the metal oxide support layer; or iii) a combination of i) and ii).

11. The method according to any one of claims 7 to 10, further comprising an intermediate bonding layer comprising a metal oxide, a first surface of the intermediate bonding layer being in contact with at least a portion of the one or more surfaces of the support structure, the catalyst system being supported on the surface of the support structure by being at least partially supported on a second surface of the intermediate bonding layer, the intermediate bonding layer optionally comprising α-Al2O3.

12. The method of any of the preceding claims, wherein the support structure comprises a monolith having a cell density of 50 cells / square inch to 900 cells / square inch, or wherein the support structure comprises 80 wt% or more Al2O3, or a combination thereof.

13. The method according to any one of the preceding claims, further comprising: After said reacting, exposing a second portion of said reactant stream comprising said reformable hydrocarbon to said catalyst system in a reaction zone within said reactor to form a product stream comprising H2; and after said exposing said second portion of said reactant flow, reacting said second portion of said mixture comprising fuel and 0.1 vol % or more O2 in said combustion zone within said reactor under combustion conditions to heat said one or more surfaces in said reaction zone to a regeneration surface temperature of 1000°C to 1300°C, wherein at the end of said exposing said second portion of said reactant flow the minimum temperature in said at least a portion of said reaction zone is 900°C or higher, or wherein at the start of said reacting said second portion of said mixture the minimum temperature in said at least a portion of said reaction zone is 900°C or higher, or a combination thereof.

14. The process according to any one of the preceding claims, wherein the catalyst system comprises 0.1 wt% to 10 wt% Pd relative to the weight of the catalyst system, or wherein the catalyst system comprises 0.5 wt% to 6.0 wt% Pd relative to the weight of the catalyst system.

15. The process according to any one of the preceding claims, wherein the catalyst system comprises a catalyst system calcined at a temperature of 900°C to 1500°C prior to the reacting.