Resin composition, dry film, cured product, and electronic component

By optimizing the dynamic viscoelastic characteristics and process processing of the resin composition, the problems of warping and reflectivity after reflow soldering are solved, and a resin layer with low warping and high reflectivity is achieved, supporting the thinning of the display and the optical performance improvement of the display.

CN119032136APending Publication Date: 2024-11-26TAIYO HOLDINGS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034672.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-27
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

After the reflow welding process, it is difficult to take into account low warping and high reflectivity in the conventional white photosensitive resin composition or thermosetting resin composition, which leads to easy warping of the glass substrate and difficult to maintain the thinning and lightweight requirements of the display.

Method used

Using carboxyl-containing urethane resin and white colorant resin composition, the cured coating properties of the resin are optimized by dynamic viscoelastic determination to ensure that the loss tangent peak is within the range of 0.5 to 1.5, combined with screen printing and The thermal curing process forms a resin layer with low warpage and high reflectivity.

Benefits of technology

It realizes that low warpage and high reflectivity are taken into account after the reflow soldering process, reduces warpage of the glass substrate, supports thinner and lighter display, and improves the optical performance of the backlight unit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005089237220000281
    Figure BDA0005089237220000281
Patent Text Reader

Abstract

Provided are a resin composition and the like which can achieve both low warpage and high reflectance after a reflow step. The resin composition is characterized by containing (A) a carboxyl group-containing urethane resin and (E) a white colorant, and in a dynamic viscoelasticity measurement at a frequency of 1 Hz for a cured coating film of the resin composition, the temperature (Tg) of the loss tangent peak is 100 DEG C or less, and the loss tangent peak is in the range of 0.5-1.5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition, a dry film, a cured product and an electronic component. Background Art

[0002] In recent years, the use of printed circuit boards for direct mounting on low-power light-emitting diodes (LEDs) such as backlights of liquid crystal displays of portable terminals, personal computers, and televisions, and light sources of lighting fixtures has gradually increased. For printed circuit boards used in such applications, a solder resist film with high reflectivity and improved brightness as a whole when the LED is mounted on the printed circuit board is sought in order to efficiently utilize the light of the LED. Patent documents 1 to 4 disclose white curable resin compositions that can be used in the solder resist film.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2009-149878

[0006] Patent Document 2: Japanese Patent No. 4538521

[0007] Patent Document 3: Japanese Patent No. 4538484

[0008] Patent Document 4: Japanese Patent No. 4340272 Summary of the invention

[0009] Problem that the invention aims to solve

[0010] Liquid crystal displays are composed of a light attenuator that combines liquid crystals whose polarization state changes when voltage is applied and polarizing filters, and a backlight unit arranged behind it. In existing liquid crystal displays, the backlight unit has long been a type that emits light uniformly across the entire surface, but a split drive method that divides the light-emitting area according to the brightness of the background has been developed to improve contrast by combining it with a regional dimming technology that turns on the LED only in areas where brightness is required. In the split drive method, side-lit LED backlights that use a light guide plate to spread the light of LEDs arranged at one end of the screen throughout the entire screen are implemented, and LEDs are installed directly under the screen. Those with a split number of dozens to about 100 have already been commercialized.

[0011] When the number of divisions is small, light leaks into the area that should be displayed darkly, and the halo effect of blurring the outline of the bright area becomes noticeable, and sufficient image beauty cannot be obtained. Therefore, in recent years, from the perspective of improving contrast, direct-type small LED backlights have been proposed, in which small LEDs with a size of less than about 1 mm are arranged in a manner covering a substrate.

[0012] With the goal of increasing the number of small LEDs installed in the backlight unit, expanding the wiring density, and realizing a thin backlight, in addition to the PCB substrates such as FR4 that have been used in the past, it is expected that in the future there will be more opportunities to use glass substrates that can easily construct TFTs into a flat surface and easily realize active matrix construction, and flexible substrates (FPCs) that can contribute to the realization of curved surfaces and thinning.

[0013] When manufacturing such a direct-type LED backlight unit, a white photosensitive resin composition having insulation and high reflectivity is applied to the entire surface of the above-mentioned glass substrate, and a pattern for setting small LEDs is formed by each process of exposure, development, and thermal curing, or by screen printing a white thermosetting resin composition using a pattern with openings only at the small LED setting position and thermal curing. Thereafter, a thermal process is further performed in order to solder the small LEDs to the openings of the formed pattern by a reflow process.

[0014] For the direct-type LED backlight unit as described above, for example, in order to manufacture multiple chamfers for large liquid crystal displays or small displays, the glass substrate used for the backlight also becomes a size such as the 8th generation (2160mm×2460mm). Therefore, when a white photosensitive resin composition or a white thermosetting resin composition having insulation and high reflectivity is used to form the pattern for the above-mentioned small LED setting, the area on which these resin compositions are applied to the glass substrate also becomes larger. In addition, in order to make the display thinner and lighter, the glass substrate itself is also thinned from the existing 3mm to 0.7mm and 0.5mm, which are less than 1mm. In order to achieve the increase in the coating area and the thinning of the glass, there is a problem that the glass substrate becomes easy to warp due to the shrinkage of the white photosensitive resin composition or the white thermosetting resin composition based on heating in each process during pattern formation and the subsequent reflow process.

[0015] Thus, when the existing white photosensitive resin composition or white thermosetting resin composition is used in a backlight unit of a display, the substrate will bend due to the warping after the reflow process, and therefore, there is a problem that it is not possible to cope with the thinning and lightening of the display. In addition, in the backlight application of the display, it is also required to maintain a high reflectivity after the reflow process, but for the existing white photosensitive resin composition or white thermosetting resin composition, there is a problem that it is difficult to achieve both low warping and high reflectivity after the reflow process.

[0016] The present invention has been made in view of the above problems of the prior art, and an object of the present invention is to provide a resin composition that can achieve both low warpage and high reflectivity after a reflow process, and a dry film, a cured product, and an electronic component using the same.

[0017] Solutions for solving problems

[0018] The present inventors have conducted intensive research to achieve the above-mentioned purpose. As a result, they found that the use of a composition with specific properties in the dynamic viscoelasticity measurement of a cured coating at a frequency of 1 Hz can achieve both high reflectivity and low warpage after the reflow process, thereby solving the above-mentioned problem and completing the present invention.

[0019] That is, the resin composition of the present invention is characterized in that it contains: (A) a carboxyl-containing urethane resin and (E) a white colorant, and in the dynamic viscoelasticity measurement of the cured coating of the resin composition at a frequency of 1 Hz, the temperature of the loss tangent (tanδ) peak (glass transition temperature, hereinafter referred to as Tg) is 100°C or less, and the peak of the loss tangent is in the range of 0.5 to 1.5. It should be noted that the dynamic viscoelasticity measurement in the present invention refers to the value measured using a dynamic viscoelasticity measuring device (DMA, manufactured by TA Instruments Japan Co., Ltd., model: RSA-G2) under the conditions of a temperature range of -60°C to 300°C, a heating rate of 5°C / min, and a frequency of 1 Hz. The details of the method for measuring the peaks of Tg and loss tangent (tanδ) are described below.

[0020] When the resin composition is a photosensitive resin composition, the photosensitive resin composition is applied to the entire surface of the copper foil by screen printing so that the film thickness after drying becomes 30 μm to form a resin layer. After that, the resin layer is dried in a hot air circulation drying oven at 80° C. for 30 minutes, and then exposed to light at 900 mJ / cm using an exposure device equipped with a metal halide lamp (HMW-680-GW20: ORC MANUFACTURING CO., LTD.). 2The resin layer was exposed to an exposure amount of 1000 nm and developed for 60 seconds (30° C., 0.2 MPa, 1 mass % Na 2 CO 3 aqueous solution). The resin layer was then cured in a hot air circulation drying oven at 150° C. for 60 minutes to form a cured coating of the resin layer, thereby preparing an evaluation substrate.

[0021] In addition, when the resin composition is a thermosetting resin composition, the thermosetting resin composition is applied to the entire surface of the copper foil by screen printing in such a manner that the film thickness after drying becomes 30 μm to form a resin layer. Thereafter, the resin layer is cured in a hot air circulation drying oven at 150° C. for 60 minutes to form a cured coating film of the resin layer, thereby preparing an evaluation substrate.

[0022] The peak values ​​of Tg and loss tangent (tanδ) are measured as follows: the cured coating film of the resin layer formed on these evaluation substrates is peeled off from the copper foil, and the cured coating film is measured according to the tensile mode of the dynamic viscoelasticity measuring device (DMA, manufactured by TA Instruments Japan Co., Ltd., model: RSA-G2). The measurement conditions are as follows: the temperature range is -60°C to 300°C, the heating rate is 5°C / min, the frequency is 1Hz, the strain is 0.1%, and the sample size is 5mm in width × 50mm in length. The cured coating film is installed in a manner that the two ends in the width direction are respectively maintained, and the cured coating film overflowing from the chuck is removed. The chuck spacing is set to 10mm.

[0023] The resin composition of the present invention is preferably such that (E) the white colorant is titanium oxide, and further preferably, (A) the carboxyl-containing urethane resin contains a carboxyl-containing urethane resin without an aromatic ring, and further preferably contains (D) an epoxy resin. In addition, it is preferred to contain (F) other carboxyl-containing resins other than (A) the carboxyl-containing urethane resin. In the case where the resin composition of the present invention is a photosensitive resin composition, it preferably contains (B) a difunctional (meth) acrylate, and (C) a photopolymerization initiator. Here, in the present invention, (meth) acrylate is a term collectively referring to acrylates, methacrylates, and mixtures thereof, and the same applies to other similar expressions.

[0024] The dry film of the present invention is characterized in that it has a resin layer obtained by applying the resin composition of the present invention to a film and drying it. In addition, the cured product of the present invention is characterized in that it is obtained from the resin composition of the present invention or the dry film of the present invention. Further, the electronic component of the present invention is characterized in that it has the cured product of the present invention.

[0025] Effects of the Invention

[0026] According to the present invention, there can be provided a resin composition that can achieve both low warpage and high reflectivity after a thermal process, and a dry film, a cured product, and an electronic component using the same. DETAILED DESCRIPTION

[0027] As mentioned above, the resin composition of the present invention comprises: (A) a carboxyl-containing urethane resin and (E) a white colorant. In the dynamic viscoelasticity measurement of the cured coating of the resin composition at a frequency of 1 Hz, Tg is below 100°C and the peak of the loss tangent is in the range of 0.5 to 1.5, thereby being able to achieve both high reflectivity and low warpage after the reflow process.

[0028] The loss tangent (tanδ) is the ratio of the loss modulus to the storage modulus, and indicates the degree of contribution of viscosity at that temperature. A loss tangent of 1 indicates that viscosity and elasticity are the same. When it is above 1, it indicates that the viscosity is large, and when it is below 1, it indicates that the elasticity is increased. The larger the peak of the loss tangent, the more components of energy generated by force and strain diffuse to the outside, so it becomes easier to relax the generated stress and strain.

[0029] Generally, the lower the crosslinking density of the resin, the more flexible the formed coating is, and the less warpage after curing. By mixing the components of the resin composition of the present invention in the amounts described in (1) to (3) below and adjusting the loss tangent (tan δ) to a peak between 0.5 and 1.5, low warpage after the reflow process, which is difficult to achieve with conventional methods, can be achieved.

[0030] (1) 75 to 90 parts by weight of (A) carboxyl-containing urethane resin having an effect on stress relaxation is compounded with respect to a total of 100 parts by weight of carboxyl-containing resins including (F) other carboxyl-containing resins. (2) When the resin composition of the present invention is a photosensitive resin composition, 20 to 100 parts by weight of (B) difunctional (meth)acrylate is compounded with respect to a total of 100 parts by weight of (meth)acrylates so that the crosslinking density does not become excessively high. (3) 50 to 500 parts by weight of (E) a white colorant is compounded with respect to a total of 100 parts by weight of (A) carboxyl-containing urethane resin and a carboxyl-containing resin including (F) other carboxyl-containing resins. Here, the range of the peak of the loss tangent (tan δ) is more preferably 0.6 to 1.1, and further preferably 0.8 to 1.0 to reduce warpage.

[0031] It should be noted that a state in which the peak of the loss tangent (tan δ) exceeds 1.5 indicates that the material has a fairly strong viscosity, but with such a material, it is difficult to maintain characteristics such as solder heat resistance and plating resistance.

[0032] The Tg of the cured coating film of the resin composition of the present invention in the dynamic viscoelasticity measurement at a frequency of 1 Hz is more preferably 30° C. to 90° C., and further preferably 40° C. to 70° C. The Tg can be adjusted to the above range by blending the components of the resin composition of the present invention in the amounts described in the following (1) to (2).

[0033] (1) 75 to 90 parts by mass, more preferably 80 to 90 parts by mass, of (A) a carboxyl group-containing urethane resin having an effect on stress relaxation is added to 100 parts by mass of a total of carboxyl group-containing resins including (F) other carboxyl group-containing resins. (2) When the resin composition of the present invention is a photosensitive resin composition, 20 to 100 parts by mass of (B) a difunctional (meth)acrylate having a small number of functional groups is added to 100 parts by mass of a total of (meth)acrylates so that the crosslinking density does not become excessively high.

[0034] The resin composition of the present invention is a resin composition comprising (A) a carboxyl-containing urethane resin and (E) a white colorant. Specifically, as (A) a carboxyl-containing urethane resin, it is preferred to contain at least some of a carboxyl-containing urethane resin having no aromatic ring, (B) a bifunctional (meth)acrylate, (C) a photopolymerization initiator, and (D) an epoxy resin. These components are described in detail below.

[0035] When the resin composition of the present invention is a thermosetting resin composition, it preferably contains (D) an epoxy resin. When the resin composition of the present invention is a photosensitive resin composition, it preferably contains (B) a bifunctional (meth)acrylate and (C) a photopolymerization initiator.

[0036] [(A) Carboxyl group-containing urethane resin]

[0037] The resin composition of the present invention contains (A) a carboxyl group-containing urethane resin having an effect on stress relaxation.

[0038] The (A) carboxyl group-containing urethane resin of the present invention preferably contains at least one of (A-1) a carboxyl group-containing urethane resin having no aromatic ring and (A-2) a carboxyl group-containing urethane resin derived from a diol having an aromatic ring and an aliphatic diisocyanate.

[0039] The resin composition of the present invention preferably contains (A-1) a carboxyl-containing urethane resin having no aromatic ring. By containing (A-1) a carboxyl-containing urethane resin having no aromatic ring, discoloration caused by heat can be suppressed, and a coating film with high reflectivity can be obtained.

[0040] The carboxyl-containing urethane resin (A-1) having no aromatic ring preferably includes a carboxyl-containing urethane resin obtained by reacting a polyisocyanate (a) which is an aliphatic diisocyanate compound having an isocyanate group and a compound having two or more alcoholic hydroxyl groups in one molecule and a compound having one alcoholic hydroxyl group in one molecule. The carboxyl-containing urethane resin (A-1) having no aromatic ring does not contain, in its materials, a diol (b) having an aromatic ring, a polycarbonate diol (c-2) having a repeating unit derived from an alicyclic diol as a structural unit, and a polycarbonate diol (c-3) having a repeating unit derived from both a linear aliphatic diol and an alicyclic diol as a structural unit, but other than this, it can be synthesized by the same method as the carboxyl-containing urethane resin (A-2) derived from a diol having an aromatic ring and an aliphatic diisocyanate.

[0041] As the polyisocyanate (a) of aliphatic diisocyanate, various polyisocyanates known in the past can be used, and are not limited to specific compounds. As a specific example of the polyisocyanate (a) of aliphatic diisocyanate, for example, diisocyanates such as hexamethylene diisocyanate and trimethyl hexamethylene diisocyanate can be cited. These polyisocyanates can be used in one or in combination of two or more. Among these, trimethyl hexamethylene diisocyanate is preferred. When using these diisocyanates, a cured product with excellent resistance to welding heat can be obtained.

[0042] The polyisocyanate is not limited to the polyisocyanate (a) of aliphatic diisocyanate as long as it has an aromatic ring, and for example, polyisocyanates of isophorone diisocyanate, cyclohexane-1,3-dimethylene diisocyanate, and cyclohexane-1,4-dimethylene diisocyanate may be used.

[0043] As the compound having two or more alcoholic hydroxyl groups in one molecule, polycarbonate diol and a compound having a carboxyl group and two or more alcoholic hydroxyl groups are preferred. As the polycarbonate diol, polycarbonate diol (c-1) containing one or more repeating units derived from a linear aliphatic diol as a structural unit is preferred, as a specific example, as described later. As the compound having a carboxyl group and two or more alcoholic hydroxyl groups, dimethylol alkanoic acid (d) is preferred, as a specific example, as described later.

[0044] As the compound having one alcoholic hydroxyl group in one molecule, the monohydroxy compound (e) described below is preferred, and specific examples thereof are described below.

[0045] When a carboxyl-containing urethane resin obtained by reacting a polyisocyanate having no aromatic ring with a polycarbonate diol (c-1) containing one or more repeating units derived from a linear aliphatic diol as a structural unit, a dimethylol alkanoic acid (d) and a monohydroxy compound (e) is used as the carboxyl-containing urethane resin having no aromatic ring (A-1), discoloration due to heat can be suppressed, and a coating film with a higher reflectivity can be obtained, so it is preferred.

[0046] The resin composition of the present invention preferably contains (A-2) a carboxyl-containing urethane resin derived from a diol having an aromatic ring and an aliphatic diisocyanate. Low warpage can be achieved by containing (A-2) a carboxyl-containing urethane resin derived from a diol having an aromatic ring and an aliphatic diisocyanate and a difunctional (meth)acrylate.

[0047] (A-2) The carboxyl group-containing urethane resin derived from a diol having an aromatic ring and an aliphatic diisocyanate preferably has a urethane bond formed by a reaction of a polyisocyanate (a) of an aliphatic diisocyanate and a diol (b) having an aromatic ring, and further has a urethane bond formed by a reaction of a polycarbonate polyol (c) and a dimethylol alkanoic acid (d), and has a carboxyl group introduced from the dimethylol alkanoic acid (d). During the reaction, a monohydroxy compound (e) may be added as a reaction terminator (capping agent).

[0048] (A-2) The carboxyl group-containing urethane resin derived from a diol having an aromatic ring and an aliphatic diisocyanate may be prepared by, for example, simultaneously mixing a polyisocyanate (a) of an aliphatic diisocyanate with a diol (b) having an aromatic ring, a polycarbonate polyol (c), a dimethylol alkanoic acid (d), and a monohydroxy compound (e) to react. Alternatively, the polyisocyanate (a) of an aliphatic diisocyanate with a diol (b) having an aromatic ring, a polycarbonate polyol (c), and a dimethylol alkanoic acid (d) may be reacted, and then reacting the monohydroxy compound (e) which functions as a reaction terminator.

[0049] For example, the polycarbonate polyol (c), the diol (b) having an aromatic ring, the dimethylol alkanoic acid (d), and the monohydroxy compound (e) functioning as a reaction terminator may be mixed together and reacted with the polyisocyanate (a) of the aliphatic diisocyanate.

[0050] The reaction is carried out without a catalyst by stirring / mixing at room temperature to 100° C., but it is preferably heated to 70 to 100° C. to increase the reaction rate. In addition, as the reaction ratio (molar ratio) of the above-mentioned (a) to (d) components, suitable ones are (b): (c) = 1:9 to 9:1, preferably 2:8 to 8:2, (b+c): (d) = 95:5 to 5:95, preferably 80:20 to 15:85, (a): (b+c+d) = 1:1 to 2:1, preferably 1:1 to 1.5:1, and (a+b+c+d): (e) = 1:0.01 to 0.5, preferably 1:0.02 to 0.3.

[0051] As the polyisocyanate (a) of the aliphatic diisocyanate, various conventionally known polyisocyanates can be used, and the polyisocyanate is not limited to a specific compound. Specific examples are as described above.

[0052] As the diol (b) having an aromatic ring, bisphenol A type alkylene oxide adduct diol is preferred. Specifically, ethylene oxide adducts, propylene oxide adducts, butylene oxide adducts, etc. of bisphenol A are mentioned. Among these, propylene oxide adducts of bisphenol A are preferred from the viewpoint of improving solder heat resistance.

[0053] As the polycarbonate polyol (c), polycarbonate diol is preferred. As the polycarbonate diol, there can be mentioned a polycarbonate diol (c-1) comprising as a structural unit a repeating unit derived from one or more linear aliphatic diols, a polycarbonate diol (c-2) comprising as a structural unit a repeating unit derived from one or more alicyclic diols, or a polycarbonate diol (c-3) comprising as a structural unit a repeating unit derived from these two diols.

[0054] Specific examples of the polycarbonate diol (c-1) containing a repeating unit derived from a linear aliphatic diol as a structural unit include, for example, a polycarbonate diol derived from 1,6-hexanediol, a polycarbonate diol derived from 1,5-pentanediol and 1,6-hexanediol, a polycarbonate diol derived from 1,4-butanediol and 1,6-hexanediol, and a polycarbonate diol derived from 3-methyl-1,5-pentanediol and 1,6-hexanediol.

[0055] As a specific example of the polycarbonate diol (c-2) containing a repeating unit derived from an alicyclic diol as a structural unit, for example, a polycarbonate diol derived from 1,4-cyclohexanedimethanol can be mentioned.

[0056] Specific examples of the polycarbonate diol (c-3) containing repeating units derived from both linear aliphatic diol and alicyclic diol as structural units include polycarbonate diols derived from 1,6-hexanediol and 1,4-cyclohexanedimethanol.

[0057] Polycarbonate diols containing repeating units derived from linear aliphatic diols as structural units tend to have low warpage and excellent flexibility. In addition, polycarbonate diols containing repeating units derived from alicyclic diols as structural units have higher crystallinity and tend to have excellent tinning resistance and soldering heat resistance. From the above viewpoints, these polycarbonate diols can be used in combination of two or more, or polycarbonate diols containing repeating units derived from both linear aliphatic diols and alicyclic diols as structural units can be used. In order to achieve low warpage, flexibility, soldering heat resistance, and tinning resistance in a well-balanced manner, it is preferred to use a polycarbonate diol having a copolymerization ratio of linear aliphatic diol to alicyclic diol of 3:7 to 7:3 by mass ratio.

[0058] The polycarbonate diol preferably has a number average molecular weight of 200 to 5000. The polycarbonate diol contains repeating units derived from a linear aliphatic diol and an alicyclic diol as structural units. When the copolymerization ratio of the linear aliphatic diol to the alicyclic diol is 3:7 to 7:3 by mass ratio, the number average molecular weight is preferably 400 to 2000.

[0059] The dimethylolalkanoic acid (d) is a dihydroxyaliphatic carboxylic acid having a carboxyl group, and specific examples thereof include dimethylolpropionic acid, dimethylolbutanoic acid, etc. By using the dimethylolalkanoic acid (d), a carboxyl group can be easily introduced into the urethane resin.

[0060] The monohydroxy compound (e) may be any compound having one hydroxyl group in the molecule as a terminal blocking agent for polyurethane, and examples thereof include aliphatic alcohols (e-1) and monohydroxy mono(meth)acrylate compounds (e-2).

[0061] Specific examples of the aliphatic alcohol (e-1) include methanol, ethanol, propanol, isobutyl alcohol, and the like. Specific examples of the monohydroxy mono(meth)acrylate compound (e-2) include 2-hydroxyethyl acrylate, and the like.

[0062] As described above, when (A) a carboxyl group-containing urethane resin obtained by reacting (a) a polyisocyanate, (b) a bisphenol A-based alkylene oxide adduct diol, (c) a polycarbonate diol, and (d) a dimethylolalkanoic acid is used as the carboxyl group-containing urethane resin (A-2) derived from a diol having an aromatic ring and an aliphatic diisocyanate, it is preferred to use it in combination with a difunctional (meth)acrylate because a low warpage effect of further suppressing warpage is achieved.

[0063] The weight average molecular weight of the carboxyl group-containing urethane resin (A) is preferably 500 to 100,000, and more preferably 8,000 to 50,000. Here, the weight average molecular weight is a value measured by gel permeation chromatography in terms of polystyrene. When the weight average molecular weight of the carboxyl group-containing urethane resin (A) is less than 500, the elongation, flexibility and strength of the cured film may be impaired. On the other hand, when it exceeds 100,000, the cured film may become hard, and there is a concern that the flexibility may be reduced.

[0064] The acid value of the (A) carboxyl-containing urethane resin is preferably in the range of 5 to 150 mgKOH / g, and more preferably 10 to 100 mgKOH / g. When the acid value is less than 5 mgKOH / g, the reactivity with the thermosetting component is reduced, and the heat resistance is sometimes impaired. On the other hand, if the acid value exceeds 150 mgKOH / g, the alkali resistance, electrical properties, etc. of the cured film as a resist are sometimes reduced. It should be noted that the acid value of the resin is a value measured in accordance with JIS K5407.

[0065] The amount of the (A-1) carboxyl-containing urethane resin having no aromatic ring is 50 to 95 parts by mass, more preferably 60 to 70 parts by mass, based on 100 parts by mass of the total amount of the (A) carboxyl-containing resin and the (F) other carboxyl-containing resin.

[0066] The amount of the carboxyl-containing urethane resin (A-2) derived from a diol having an aromatic ring and an aliphatic diisocyanate is 5 to 90 parts by mass, more preferably 10 to 20 parts by mass, based on 100 parts by mass of the total amount of the carboxyl-containing resin (A) and the other carboxyl-containing resin (F).

[0067] [(B) Difunctional (meth)acrylate]

[0068] The resin composition of the present invention comprises a difunctional (meth)acrylate. The (meth)acrylate has an ethylenically unsaturated group, and therefore, by irradiating active energy rays and performing photocuring, it contributes to the insolubility of the resin composition of the present invention in alkaline aqueous solution. The (B) difunctional (meth)acrylate of the present invention is difunctional, and therefore forms a cross-linked structure, and in particular, by being used in combination with the (A) component, the opposite physical properties of the softness and hardness of the cured coating film are satisfied. It should be noted that when the number of functional groups per unit molecular weight increases, such as trifunctional or higher (meth)acrylates, the polymerization shrinkage becomes larger, and therefore, the compounding amount must be within a specified range.

[0069] Specifically, when the (meth)acrylate contained in the photosensitive resin composition of the present invention is set to 100 parts by mass as a whole, the compounding amount of the (B) difunctional (meth)acrylate is preferably 20 parts by mass to 100 parts by mass, and more preferably 40 parts by mass to 100 parts by mass. For the compounding amount of trifunctional or higher (meth)acrylate, if it is 40 parts by mass to 80 parts by mass when the (meth)acrylate contained in the photosensitive resin composition of the present invention is set to 100 parts by mass as a whole, warping can be suppressed even if it is included. When the (meth)acrylate contained in the photosensitive resin composition of the present invention is set to 100 parts by mass as a whole, if the (meth)acrylate of tetrafunctional or higher is 5 parts by mass or less, warping can be suppressed.

[0070] In particular, in the case of hexafunctional or higher (meth)acrylates, the polymerization shrinkage increases and the warpage worsens as the number of functional groups per unit molecular weight increases. Therefore, in the photosensitive resin composition of the present invention, when the total amount of the (meth)acrylate contained in the photosensitive resin composition of the present invention is 100 parts by mass, it is preferably less than 1 part by mass.

[0071] (B) The difunctional (meth)acrylate specifically includes diacrylates of diols such as ethylene glycol, methoxytetraethylene glycol, polyethylene glycol, and propylene glycol; diacrylates of polyols such as hexanediol, trimethylolpropane, pentaerythritol, dipentaerythritol, trishydroxyethyl isocyanurate, or ethylene oxide adducts, propylene oxide adducts, or ε-caprolactone adducts thereof; and diacrylates such as phenoxy acrylate, bisphenol A diacrylate, and ethylene oxide adducts or propylene oxide adducts of these phenols. Esters; diacrylates of glycidyl ethers such as glycerol diglycidyl ether, glycerol triglycidyl ether, trimethylolpropane triglycidyl ether, and isocyanuric acid triglycidyl ether; not limited to the above, diacrylates and melamine diacrylates obtained by directly acrylateing polyols such as polyether polyols, polycarbonate diols, hydroxyl-terminated polybutadiene, and polyester polyols, or urethane acrylated with diisocyanates, and / or dimethacrylates corresponding to the above diacrylates.

[0072] Furthermore, there can be mentioned epoxy diacrylate resins obtained by reacting a multifunctional epoxy resin such as a cresol novolac epoxy resin with diacrylic acid; epoxy urethane diacrylate compounds obtained by reacting a hydroxyl group of the epoxy diacrylate resin with an acrylic acid hydroxyl ester such as pentaerythritol triacrylate and a half urethane compound of a diisocyanate such as isophorone diisocyanate, etc. Such epoxy diacrylate resins can improve photocurability without reducing dryness to touch.

[0073] The amount of the (B) difunctional (meth)acrylate is preferably 5 to 100 parts by mass, more preferably 5 to 70 parts by mass, relative to 100 parts by mass of the total amount of the (A) carboxyl group-containing urethane resin and the (F) other carboxyl group-containing resin. When the amount is within the above range, the photocurability is good, pattern formation can be performed by alkali development after active energy ray irradiation, and the solubility in alkaline aqueous solution is good.

[0074] [(C) Photopolymerization initiator]

[0075] The resin composition of the present invention can use a known and commonly used (C) photopolymerization initiator. (C) The photopolymerization initiator can be used alone or in combination of two or more, but preferably has a photobleaching effect. The photobleaching effect means that when the photopolymerization initiator absorbs light and generates free radicals, cleavage occurs and the conjugated bonds of the molecules are cut, thereby reducing the absorbance in the ultraviolet region and not hindering the transmission of ultraviolet rays to the interior. Preferred examples of the (C) photopolymerization initiator having a photobleaching effect include monoacylphosphine oxide-based photopolymerization initiators and bisacylphosphine oxide-based photopolymerization initiators.

[0076] Examples of the monoacylphosphine oxide-based photopolymerization initiator include 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, methyl 2,4,6-trimethylbenzoylphenylphosphinate, 2-methylbenzoyldiphenylphosphine oxide, isopropyl pivaloylphenylphosphinate, etc. Among them, 2,4,6-trimethylbenzoyldiphenylphosphine oxide is easily available.

[0077] Examples of the bisacylphosphine oxide-based photopolymerization initiator include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and (2,5,6-trimethylbenzoyl)-2,4,4-trimethylpentylphosphine oxide. Among them, bis-(2,4,6-trimethylbenzoyl)phenylphosphine oxide (manufactured by BASF Japan Co., Ltd., trade name: Irgacure 819) is easily available.

[0078] The total amount of the photopolymerization initiator is preferably 1 to 30 parts by mass, more preferably 2 to 25 parts by mass, relative to 100 parts by mass of the total amount of the (A) carboxyl group-containing urethane resin and the (F) other carboxyl group-containing resin. If the amount is within the above range, the photocurability of the coating film is good, and pattern formation after exposure / development is also good.

[0079] [(D) Epoxy resin]

[0080] In order to improve the heat resistance of the cured product, the curable resin composition of the present invention may use a known and commonly used (D) epoxy resin. The (D) epoxy resin may be used alone or as a mixture of two or more.

[0081] As specific examples of epoxy resins, for example, bisphenol A type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, novolac type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, N-glycidyl type epoxy resins, novolac type epoxy resins of bisphenol A, bixylenol type epoxy resins, biphenol type epoxy resins, chelate type epoxy resins, glyoxal type epoxy resins, amino-containing epoxy resins, rubber modified epoxy resins, dicyclopentadienol type epoxy resins, diglycidyl phthalate resins, heterocyclic epoxy resins, tetraglycidyl ditoluoyl ethane resins, silicone modified epoxy resins, ε-caprolactone modified epoxy resins, etc. In addition, in order to impart flame retardancy, those having halogens such as chlorine and bromine, atoms such as phosphorus, etc. introduced into their structures can also be used.

[0082] The amount of the epoxy resin (D) in the resin composition of the present invention is preferably 5 to 150 parts by mass, preferably 10 to 80 parts by mass, relative to 100 parts by mass of the total amount of the carboxyl group-containing urethane resin (A) and the other carboxyl group-containing resin (F). If the amount is within the above range, the cured coating film of the photosensitive resin composition has good resistance to solder heat, and also has good properties, especially electrical insulation, when used as an insulating protective film for a printed circuit board.

[0083] [(E) White coloring agent]

[0084] In the resin composition of the present invention, the colorant (E) in white is used to make the cured coating white, and titanium oxide, zinc oxide, potassium titanate, zirconium oxide, antimony oxide, white lead, zinc sulfide, lead titanate, barium titanate, etc. can be cited. As the colorant (E) in white of the present invention, titanium oxide is preferred because of the high inhibitory effect of discoloration caused by heat. As titanium oxide, titanium oxide can be used: titanium oxide manufactured by sulfuric acid method, chlorine method, rutile titanium oxide, anatase titanium oxide, or titanium oxide obtained by surface treatment based on hydrous metal oxide and surface treatment based on organic compound. Among these titanium oxides, rutile titanium oxide is preferred. Anatase titanium oxide has a high whiteness compared with rutile type, so it is often used, but because it has photocatalytic activity, it sometimes causes discoloration of the resin in the curable resin composition. In contrast, the whiteness of rutile titanium oxide is slightly worse than that of anatase type, but it is basically not photoactive, so a stable cured coating can be obtained. As rutile titanium oxide, known rutile titanium oxide can be used. Specifically, TR-600, TR-700, TR-750, TR-840 manufactured by Fuji Titanium Industry Co., Ltd., R-550, R-580, R-630, R-820, CR-50, CR-60, CR-90 manufactured by Ishihara Industry Co., Ltd., KR-270, KR-310, KR-380 manufactured by Titanium Industry Co., Ltd., etc. can be used. Among these rutile titanium oxides, from the viewpoint of dispersibility and storage stability in the composition, it is particularly preferred to use titanium oxide whose surface has been treated with hydrous aluminum oxide or aluminum hydroxide.

[0085] The amount of the white colorant (E) is preferably in the range of 50 to 500 parts by mass, preferably 100 to 450 parts by mass, and more preferably 150 to 450 parts by mass, relative to 100 parts by mass of the total amount of the carboxyl group-containing urethane resin (A) and the other carboxyl group-containing resin (F). If the amount of the white colorant (E) is less than 50 parts by mass, it becomes difficult to form a good white cured coating film. If the amount of the white colorant (E) is within the above range, a good white cured coating film can be formed, the viscosity of the composition does not become excessively high, the coating and moldability are good, and the cured product does not become brittle.

[0086] [(F) Other carboxyl group-containing resins (carboxyl group-containing resins other than (A) carboxyl group-containing urethane resins)]

[0087] The resin composition of the present invention preferably contains a carboxyl group-containing resin other than the (A) carboxyl group-containing urethane resin as (F) other carboxyl group-containing resin.

[0088] The amount of the other carboxyl-containing resin (F) in the resin composition of the present invention is preferably 5 to 50 parts by mass, more preferably 10 to 20 parts by mass in a total of 100 parts by mass of the other carboxyl-containing resin (F) and the carboxyl-containing urethane resin (A). By mixing the amount of the other carboxyl-containing resin (F) within the above range, the peaks of Tg and loss tangent (tan δ) can be easily adjusted.

[0089] As the (F) other carboxyl group-containing resin, a known and commonly used carboxyl group-containing resin can be used. The following carboxyl group-containing resins are preferred because they can further suppress discoloration due to heat and provide a coating film with high reflectivity by using them in combination with the (A) carboxyl group-containing urethane resin.

[0090] (1) A copolymer resin having a carboxyl group obtained by reacting (a) a carboxyl group-containing (meth)acrylic copolymer resin with (b) a compound having an ethylene oxide ring and an ethylenically unsaturated group in one molecule.

[0091] (2) A carboxyl group-containing resin having a styrene skeleton (either an oligomer or a polymer) obtained by copolymerizing an unsaturated carboxylic acid such as (meth)acrylic acid with a compound containing an unsaturated group selected from styrene, α-methylstyrene, a lower alkyl (meth)acrylate, isobutylene, etc. It should be noted that the lower alkyl group refers to an alkyl group having 1 to 5 carbon atoms.

[0092] [Other thermosetting ingredients]

[0093] The resin composition of the present invention may further be mixed with a thermosetting component to improve heat resistance. As the thermosetting component, known and commonly used thermosetting resins such as melamine resin, benzoguanamine resin and other amine resins, blocked isocyanate compounds, cyclic carbonate compounds, multifunctional oxetane compounds, episulfide resins, melamine derivatives, bismaleimide, oxazine compounds, oxazoline compounds, etc. may be used, preferably, a thermosetting component having multiple cyclic (thio) ether groups in a molecule that can react with a carboxyl-containing resin represented by (A) a carboxyl-containing urethane resin (or further a phenolic hydroxyl group).

[0094] In the resin composition of the present invention, the aforementioned thermosetting component can be used alone or in combination of two or more. Its blending amount is preferably 5 to 150 parts by mass, preferably 10 to 80 parts by mass, relative to 100 parts by mass of the total amount of (A) carboxyl-containing urethane resin and (F) other carboxyl-containing resins. If it is within the above blending amount range, the cured coating of the resin composition has good resistance to soldering heat, and various properties when used as an insulating protective film, especially electrical insulation, also become good.

[0095] (Other ingredients)

[0096] The resin composition of the present invention may be mixed with a thermosetting catalyst in order to promote the thermosetting reaction and further improve the properties such as adhesion, chemical resistance, and heat resistance. Examples of such thermosetting catalysts include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazine compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. In addition, as commercially available products, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, 2P4MHZ (all are trade names of imidazole compounds) manufactured by Shikoku Chemical Industry Co., Ltd., U-CAT (registered trademark) 3503N, U-CAT3502T (all are trade names of blocked isocyanate compounds of dimethylamine), DBU, DBN, U-CATSA102, U-CAT5002 (all are bicyclic amidine compounds and salts thereof) manufactured by San-Apro Ltd., etc. are mentioned. It is not particularly limited to these, as long as it is a heat curing catalyst for epoxy resins and oxetane compounds, or a catalyst that promotes the reaction of epoxy groups and / or oxetane groups with carboxyl groups, and it can be used alone or in combination of two or more. In addition, s-triazine derivatives such as guanamine, methylguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-s-triazine, 2-vinyl-2,4-diamino-s-triazine, 2-vinyl-4,6-diamino-s-triazine / isocyanuric acid adduct, and 2,4-diamino-6-methacryloyloxyethyl-s-triazine / isocyanuric acid adduct can also be used. It is preferred that these compounds which also function as adhesion-imparting agents are used in combination with a thermosetting catalyst.

[0097] These thermosetting catalysts may be used alone or in combination of two or more, and the amount thereof blended is sufficient in a conventional amount ratio, for example, preferably 0.1 to 20 parts by mass, more preferably 0.5 to 15.0 parts by mass, relative to 100 parts by mass of the total amount of (A) the carboxyl group-containing urethane resin and (F) other carboxyl group-containing resins, or relative to 100 parts by mass of the total amount of (D) the epoxy resin and other thermosetting components.

[0098] In the resin composition of the present invention, in order to make (A) to (F) and other components as needed easily dissolved or dispersed or to adjust to a viscosity suitable for coating, an organic solvent can be used. As an organic solvent, for example, toluene, xylene, ethylbenzene, nitrobenzene, cyclohexane, isophorone, diethylene glycol dimethyl ether, ethylene glycol diethyl ether, carbitol acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, dipropylene glycol methyl ether acetate, methyl methoxypropionate, ethyl methoxypropionate, methyl ethoxypropionate, ethyl ethoxypropionate, ethyl acetate, n-butyl acetate, isoamyl acetate, ethyl lactate, acetone, methyl ethyl ketone, cyclohexanone, N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, γ-butyrolactone, dimethylformamide, chloroform and dichloromethane can be cited. The blending amount of the organic solvent can be appropriately set according to the desired viscosity.

[0099] The resin composition of the present invention may contain a known commonly used mercapto compound and a close-fitting accelerator as required to improve the close-fitting property with a substrate such as polyimide. As mercapto compounds, mercapto-containing silane coupling agents such as 2-mercaptopropionic acid, trimethylolpropane tris(2-thiopropionate), 2-mercaptoethanol, 2-aminothiophenol, 3-mercapto-1,2,4-triazole, and 3-mercapto-propyltrimethoxysilane may be cited. As a close fit accelerator, for example, there are: benzimidazole, benzoxazole, benzothiazole, 2-mercaptobenzimidazole, 2-mercaptobenzoxazole, 2-mercaptobenzothiazole, 3-morpholinomethyl-1-phenyl-triazole-2-thione, 5-amino-3-morpholinomethyl-thiazole-2-thione, 2-mercapto-5-methylthio-thiadiazole, triazole, tetrazole, benzotriazole, carboxylbenzotriazole, amino-containing benzotriazole, vinyl triazine, etc. They can be used alone or in combination of two or more. Its blending amount is relative to the total amount of 100 parts by mass of (A) carboxyl-containing urethane resin and (F) other carboxyl-containing resins, and it is suitable to be the range of less than 10 parts by mass. When the blending amount of these compounds is within the above range, the consumption of the epoxy group based on the reaction of the epoxy group of the epoxy resin (D) required for the crosslinking reaction is made to be an appropriate range, and the crosslinking density also becomes good, so it is preferred.

[0100] Most polymer materials are as follows: once oxidation begins, oxidative degradation will occur successively, resulting in a reduction in the function of the polymer raw materials. Therefore, in order to prevent oxidation, the curable resin composition of the present invention may be added with (1) a free radical scavenger that invalidates the generated free radicals and / or (2) an antioxidant such as a peroxide decomposer that decomposes the generated peroxide into harmless substances so that it does not generate new free radicals.

[0101] Examples of the antioxidant that functions as a radical scavenger include phenolic compounds such as 4-tert-butylcatechol, 2-tert-butylhydroquinone, hydroquinone monomethyl ether, 2,6-di-tert-butyl-p-cresol, 2,2-methylene-bis(4-methyl-6-tert-butylphenol), 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, and 1,3,5-tris(3',5'-di-tert-butyl-4-hydroxybenzyl)-s-triazine-2,4,6-(1H,3H,5H)trione; quinone compounds such as menadione and benzoquinone; and amine compounds such as bis(2,2,6,6-tetramethyl-4-piperidinyl)-sebacate.

[0102] The radical scavenger may be a commercially available product, for example, ADK STAB (registered trademark) AO-30, ADK STAB AO-330, ADK STAB AO-20, ADK STAB LA-77, ADK STAB LA-57, ADK STAB LA-67, ADK STAB LA-68, ADK STAB LA-87 (all manufactured by ADEKA Co., Ltd.), Irganox (registered trademark) 1010, Irganox 1035, Irganox 1076, Irganox 1135, Tinuvin (registered trademark) 111FDL, Tinuvin 123, Tinuvin 144, Tinuvin 152, Tinuvin 292, Tinuvin 5100 (all manufactured by BASF Japan Co., Ltd.), etc.

[0103] As an antioxidant that functions as a peroxide decomposer, for example, phosphorus compounds such as triphenyl phosphite, pentaerythritol tetralauryl thiopropionate, dilauryl thiodipropionate, 3,3'-distearyl thiodipropionate, etc. can be cited. The peroxide decomposer can be a commercially available product, for example, ADK STAB TPP (manufactured by ADEKA Co., Ltd.), ADK STAB AO-412S (manufactured by ADEKA Co., Ltd.), SUMILIZER (registered trademark) TPS (manufactured by Sumitomo Chemical Co., Ltd.), etc. The antioxidant can be used alone or in combination of two or more.

[0104] The resin composition of the present invention may contain an ultraviolet absorber in addition to the antioxidant. Examples of such ultraviolet absorbers include benzophenone derivatives, benzoate derivatives, benzotriazole derivatives, triazine derivatives, benzothiazole derivatives, cinnamate derivatives, anthranilic acid derivatives, and dibenzoylmethane derivatives.

[0105] Examples of the benzophenone derivatives include 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, 2,2′-dihydroxy-4-methoxybenzophenone, and 2,4-dihydroxybenzophenone.

[0106] Examples of the benzoate derivatives include 2-ethylhexyl salicylate, phenyl salicylate, p-tert-butylphenyl salicylate, 2,4-di-tert-butylphenyl 3,5-di-tert-butyl-4-hydroxybenzoate, and hexadecyl 3,5-di-tert-butyl-4-hydroxybenzoate.

[0107] Examples of benzotriazole derivatives include 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, and 2-(2'-hydroxy-3,5'-di-tert-amylphenyl)benzotriazole.

[0108] Examples of the triazine derivatives include hydroxyphenyltriazine and bis-ethylhexyloxyphenol methoxyphenyl triazine.

[0109] The ultraviolet absorber may be a commercially available product, and examples thereof include Tinuvin PS, Tinuvin 99-2, Tinuvin 109, Tinuvin 384-2, Tinuvin 900, Tinuvin 928, Tinuvin 1130, Tinuvin 400, Tinuvin 405, Tinuvin 460, and Tinuvin 479 (all manufactured by BASF Japan Co., Ltd.).

[0110] In the resin composition of the present invention, as required, for the purpose of improving the characteristics such as adhesion, hardness, heat resistance, etc., at least one filler selected from the group consisting of inorganic fillers and organic fillers can be further contained. As inorganic fillers, barium sulfate, calcium carbonate, silicon oxide, amorphous silica, talc, clay, hydrotalcite, mica powder, etc. can be cited, and as organic fillers, silicon powder, nylon powder, fluorine powder, etc. can be cited. Among the above-mentioned fillers, silicon dioxide is particularly excellent in low hygroscopicity and low volume expansion. Regardless of melting and crystallinity, silicon dioxide can be a mixture of them, especially in the case of silicon dioxide surface-treated with coupling agents, etc., electrical insulation can be improved, so it is preferred. In addition, in the case of the resin composition of the present invention is a thermosetting resin composition, it is necessary to adjust the thixotropic properties for pattern printing, preferably containing silicon dioxide. The average particle size of the filler is expected to be less than 25 μm, more preferably less than 10 μm, and further preferably less than 3 μm. The amount of these inorganic and / or organic fillers is preferably 300 parts by mass or less, preferably 5 to 150 parts by mass, relative to 100 parts by mass of the total amount of (A) carboxyl-containing urethane resin and (F) other carboxyl-containing resins. If the amount of the filler exceeds the above ratio, the flexibility of the cured coating film is reduced, which is not preferred.

[0111] In the resin composition of the present invention, other additives other than the aforementioned components can be added as long as the effect of the present invention is not impaired. As additives, known commonly used thickeners such as organobentonite and montmorillonite, defoamers and / or leveling agents of silicone, fluorine, polymer, fiber-reinforced materials such as glass fiber, carbon fiber, boron nitride fiber, etc. can be cited. And then, as required, silane coupling agents, dispersants, defoamers, plasticizers, foaming agents, flame retardants, antistatic agents, antioxidants, antibacterial / mildew-proof agents, etc. of known commonly used thermal inhibitors, imidazoles, thiazoles, triazoles, etc. can be added.

[0112] (Adjustment and use of resin composition)

[0113] The resin composition having the above composition is obtained by dissolving or dispersing the aforementioned components or the components described later as required using a mixer, such as a disperser, a kneader, a three-roll mill, a ball mill, etc. At this time, a solvent that is inactive to epoxy groups and phenolic hydroxyl groups can also be used. As such an inactive solvent, the aforementioned organic solvent is preferred.

[0114] The resin composition of the present invention can be applied to a printed circuit board by various conventional methods such as curtain coating, roll coating, spray coating, and dip coating, and can also be used in various forms and applications such as dry film or prepreg. Various solvents can be used according to the method of use and application, and not only good solvents but also poor solvents can be used depending on the situation.

[0115] In addition, the resin composition of the present invention is applied to a glass substrate or a flexible printed circuit board having a circuit formed thereon by screen printing, and is heated to a temperature of, for example, 120 to 180° C. for thermal curing, thereby forming a white cured coating film which has no warping due to curing shrinkage and cooling shrinkage, and which achieves properties such as adhesion to the substrate, folding resistance, low warping, chemical gold plating resistance, soldering heat resistance, and electrical insulation, and also achieves flexibility and high reflectivity at a high level with good balance, and has little decrease in reflectivity over time.

[0116] The resin composition of the present invention is adjusted to a viscosity suitable for the coating method using the aforementioned organic solvent, and then coated on a substrate by a method such as dip coating, flow coating, roller coating, rod coating, screen printing, curtain coating, etc. The organic solvent contained in the composition is evaporated and dried (dried) at a temperature of about 60 to 100° C., thereby forming a non-sticky coating film.

[0117] In the case where the resin composition is a photosensitive resin composition, after drying, it is selectively exposed using active energy rays or directly exposed using a laser direct exposure machine through a photomask having a pattern, and the unexposed portion is developed using a dilute alkali aqueous solution to form an anti-etching pattern. Furthermore, in the case where the resin composition is a photosensitive thermosetting composition that also contains a thermosetting component, for example, it is heated for 5 minutes to 120 minutes at a temperature of about 140 to 180° C. for thermosetting (post-curing). Through this thermosetting, the carboxyl group (or further phenolic hydroxyl group) of the carboxyl-containing urethane resin (A) reacts with the (D) epoxy resin (or, when contained, the cyclic (thio) ether group of other thermosetting components) of the thermosetting component to form a white cured coating film that realizes adhesion to the substrate, folding resistance, low warpage, chemical gold plating resistance, solder heat resistance, electrical insulation and other characteristics, and also realizes flexibility and high reflectivity with a high level of balance, and the decrease in reflectivity caused by time is small.

[0118] When the resin composition is a thermosetting resin composition without photosensitivity, after drying, it is heated at a temperature of about 140 to 180° C. for 5 to 120 minutes for thermal curing (post-curing) to form a white cured coating film that exerts the same effect as the above-mentioned photosensitive resin composition.

[0119] As the above-mentioned substrate, in addition to glass substrates, printed circuit boards and flexible printed circuit boards with pre-formed circuits, copper-clad laminates of all grades (FR-4, etc.) using composite materials such as paper-phenolic resin, paper-epoxy resin, glass cloth-epoxy resin, glass-polyimide, glass cloth / non-woven fabric-epoxy resin, glass cloth / paper-epoxy resin, synthetic fiber-epoxy resin, fluororesin / polyethylene / PPO / cyanate ester, polyimide films, PET films, ceramic substrates, wafer plates, etc. can also be used.

[0120] The volatilization drying or thermal curing (post-curing) after coating the resin composition of the present invention can be carried out using a hot air circulation drying furnace, an IR furnace, a hot plate, a convection oven, etc. (using a device with a heat source using steam to heat the air, a method of making the hot air in the dryer contact by convection, and a method of blowing it onto the support using a nozzle).

[0121] As the exposure machine used in the above-mentioned active energy ray irradiation, a direct drawing device (for example, a laser direct imaging device that directly draws an image with a laser using CAD data from a computer), an exposure machine equipped with a metal halide lamp, an exposure machine equipped with a (ultra) high pressure mercury lamp, an exposure machine equipped with a mercury short arc lamp, or a direct drawing device using an ultraviolet lamp such as a (ultra) high pressure mercury lamp can be used. As the active energy ray, it is sufficient to use a laser beam with a maximum wavelength in the range of 350 to 450 nm, which can be a gas laser or a solid laser. In addition, the exposure amount varies depending on the film thickness, etc., and can usually be set to 5 to 800 mJ / cm 2 , preferably 5 to 500 mJ / cm 2 As the direct drawing device, for example, a product manufactured by Japan Orbotech Co., Ltd. can be used, and any device can be used as long as it oscillates a laser beam having a maximum wavelength of 350 to 450 nm.

[0122] As the above-mentioned development method, an immersion method, a shower method, a spray method, a brush method, etc. can be used, and as the developer, an alkaline aqueous solution of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, etc. can be used.

[0123] In addition to the method of directly applying the resin composition of the present invention to the substrate in a liquid state, it can also be used in the form of a dry film having a resin layer formed by applying the resin composition in advance on a film (first film) such as polyethylene terephthalate and drying it. The following shows the case where the resin composition of the present invention is used as a dry film.

[0124] The dry film has a structure in which a first film and a resin layer and a second film that can be peeled off are sequentially laminated as needed. The resin layer is, for example, a layer obtained by coating a resin composition on a carrier film or a protective film and drying it. After forming a resin layer on a first film, a second film is laminated thereon, or a resin layer is formed on the second film, and the laminate is laminated on the first film to obtain a dry film.

[0125] As the first film, a thermoplastic film such as a polyester film having a thickness of 2 to 150 μm is used.

[0126] The resin layer is formed by uniformly applying the resin composition to a thickness of 10 to 150 μm on the first film or the second film using a blade coater, a lip coater, a comma coater, a film coater, or the like, and drying the coating.

[0127] As the second film, a polyethylene film, a polypropylene film or the like can be used, but it is preferable that the second film has a lower adhesiveness to the resin layer than the first film.

[0128] When a protective film (permanent protective film) is made on a substrate using a dry film, the second film is peeled off, the resin layer is overlapped with the substrate on which the circuit is formed, and the resin layer is formed on the substrate on which the circuit is formed by laminating the resin layer with a laminator or the like. The formed resin layer can be exposed, developed, and heat-cured in the same manner as described above to form a cured coating film. The first film can be peeled off before exposure, after exposure, or before heat curing.

[0129] Example

[0130] Hereinafter, the present invention will be specifically described with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0131] (Synthesis of Varnish A-1-1)

[0132] In a reaction container equipped with a stirring device, a thermometer, and a condenser, 2400 g (3 mol) of polycarbonate diol derived from 1,5-pentanediol and 1,6-hexanediol (TJ5650J manufactured by Asahi Kasei Corporation, number average molecular weight 800), 603 g (4.5 mol) of dimethylol propionic acid, and 238 g (2.6 mol) of 2-hydroxyethyl acrylate as a monohydroxy compound were added. Next, 1887 g (8.5 mol) of isophorone diisocyanate as a polyisocyanate was added, and the mixture was heated to 60°C while stirring and then stopped. When the temperature in the reaction container began to decrease, the mixture was heated again and stirred continuously at 80°C. The absorption spectrum of the isocyanate group (2280 cm-1) was confirmed in the infrared absorption spectrum. -1) disappears, and the reaction is terminated. Carbitol acetate is added in a manner that the solid content becomes 50% by mass to obtain varnish A-1-1. The weight average molecular weight of the carboxyl-containing urethane resin is 17,000, and the acid value of the solid content is 50 mgKOH / g.

[0133] (Synthesis of Varnish A-1-2)

[0134] In a reaction container equipped with a stirring device, a thermometer, and a condenser, 2400 g (3.0 mol) of polycarbonate diol derived from 1,5-pentanediol and 1,6-hexanediol (T5650J, Asahi Kasei Corporation, number average molecular weight 800) as a compound having two or more alcoholic hydroxyl groups, 603 g (4.5 mol) of dimethylolbutyric acid, and 238 g (2.6 mol) of 2-hydroxyethyl acrylate as a monohydroxy compound were added. Next, 1512 g (6.5 mol) of hexamethylene diisocyanate as a non-aromatic compound having an isocyanate group was added, and the mixture was heated to 60°C while stirring and then stopped. When the temperature in the reaction container began to drop, the mixture was heated again and stirred continuously at 80°C. The absorption spectrum of the isocyanate group (2280 cm-1) was confirmed in the infrared absorption spectrum. -1 ) disappears, and the reaction is terminated. Then, carbitol acetate is added in a manner that the solid content becomes 50% by mass to obtain a carboxyl-containing urethane resin and varnish A-1-2 that are a viscous liquid containing a diluent. The acid value of the solid content of the obtained carboxyl-containing urethane resin is 49.8 mgKOH / g.

[0135] (Synthesis of Varnish A-2-1)

[0136] In a reaction vessel equipped with a stirrer, a thermometer, and a condenser, 288 g (0.36 mol) of a polycarbonate diol (number average molecular weight 800) derived from 1,5-pentanediol and 1,6-hexanediol as a polyol component, 45 g (0.09 mol) of bisphenol A propylene oxide adduct diol (BPX33, number average molecular weight 500, manufactured by ADEKA Corporation), 81.4 g (0.55 mol) of dimethylolbutyric acid as dimethylolalkanoic acid, 11.8 g (0.16 mol) of n-butanol as a molecular weight modifier (reaction terminator), and 250 g of carbitol acetate (manufactured by Daicel Corporation) as a solvent were charged, and all the raw materials were dissolved at 60° C. While the polyol component was stirred, 200.9 g (1.08 mol) of trimethylhexamethylene diisocyanate as a polyisocyanate was added dropwise using a dropping funnel. After the dropwise addition was completed, the reaction was continued while stirring at 80°C. The absorption spectrum of the isocyanate group (2280 cm -1) disappears, and the reaction is terminated. Carbitol acetate is added in a manner that the solid content becomes 50% by mass, and a carboxyl-containing urethane resin varnish A-2-1 containing a viscous liquid of a diluent is prepared. The weight-average molecular weight of the obtained carboxyl-containing urethane resin is 18300, and the acid value of the solid content is 50.3 mgKOH / g. It should be noted that the average molecular weight is determined by gel-supported liquid chromatography (HLC-8120GPC manufactured by Tosoh Corporation) and the value converted to polystyrene.

[0137] (Synthesis of Varnish A-2-2)

[0138] In a reaction vessel equipped with a stirrer, a thermometer, and a condenser, 180 g (0.225 mol) of a polycarbonate diol (number average molecular weight 800) derived from 1,5-pentanediol and 1,6-hexanediol as a polyol component, 112.5 g (0.225 mol) of bisphenol A propylene oxide adduct diol (BPX33, number average molecular weight 500, manufactured by ADEKA Corporation), 81.4 g (0.55 mol) of dimethylolbutyric acid as dimethylolalkanoic acid, 11.8 g (0.16 mol) of n-butanol as a molecular weight modifier (reaction terminator), and 250 g of carbitol acetate (manufactured by Daicel Corporation) as a solvent were charged, and all the raw materials were dissolved at 60° C. While the polyol component was stirred, 200.9 g (1.08 mol) of trimethylhexamethylene diisocyanate as a polyisocyanate was added dropwise using a dropping funnel. After the dropwise addition was completed, the reaction was continued while stirring at 80°C. The absorption spectrum of the isocyanate group (2280 cm -1 ) disappears, and the reaction is terminated. Carbitol acetate is added in a manner that the solid content becomes 50% by mass to obtain a carboxyl-containing urethane resin varnish A-2-2 that is a viscous liquid containing a diluent. The weight-average molecular weight of the obtained carboxyl-containing urethane resin is 18,000, and the acid value of the solid content is 50.0 mgKOH / g. It should be noted that the average molecular weight is determined by gel-supported liquid chromatography (HLC-8120GPC manufactured by Tosoh Corporation) and the value converted to polystyrene.

[0139] (Synthesis of Varnish F-1 (Other Carboxyl-containing Resins))

[0140] In a flask equipped with a thermometer, a stirrer, a dropping funnel and a reflux condenser, 325.0 parts by mass of dipropylene glycol monomethyl ether as a solvent was heated to 110° C., and a mixture of 174.0 parts by mass of methacrylic acid, 174.0 parts by mass of ε-caprolactone-modified methacrylic acid (average molecular weight 314), 77.0 parts by mass of methyl methacrylate, 222.0 parts by mass of dipropylene glycol monomethyl ether, and 12.0 parts by mass of tert-butyl peroxy-2-ethylhexanoate (manufactured by NOF Corporation, Perbutyl O) as a polymerization catalyst was added dropwise over 3 hours, and the mixture was further stirred at 110° C. for 3 hours to deactivate the polymerization catalyst, thereby obtaining a resin solution. After cooling the resin solution, 289.0 parts by mass of Cyclomer M100 manufactured by Daicel Corporation, 3.0 parts by mass of triphenylphosphine and 1.3 parts by mass of hydroquinone monomethyl ether were added, and the mixture was heated to 100° C. and stirred to allow a ring-opening addition reaction of the epoxy group to proceed, thereby obtaining a varnish F-1 having a solid content of 45.5% by mass and a solid content acid value of 79.8 mgKOH / g.

[0141] (Synthesis of Varnish F-2 (Other Carboxyl-containing Resins))

[0142] In a 2000 ml flask equipped with a stirrer and a condenser, 377 g of tripropylene glycol monomethyl ether was placed and heated to 90°C under a nitrogen stream. Over 4 hours, 104.2 g of styrene, 246.5 g of methacrylic acid, and 20.7 g of 2,2'-azobis(2-methylpropionic acid) dimethyl ester (manufactured by FUJIFILM Wako Chemicals Corporation: V-601) were added dropwise to the flask to mix and dissolve. In this way, a carboxyl-containing resin solution varnish F-2 was obtained. The carboxyl-containing resin solution was as follows: the solid content acid value was 120 mgKOH / g, the solid content was 50%, and the molecular weight was 20,000. The mass average molecular weight of the obtained carboxyl group-containing resin was measured by high-performance liquid chromatography using a pump LC-6AD manufactured by Shimadzu Corporation and three columns Shodex (registered trademark) KF-804, KF-803, and KF-802 manufactured by Showa Denko K.K.

[0143] (Synthesis of Varnish F-3 (Other Carboxyl-containing Resins))

[0144] In 600 g of diethylene glycol monoethyl ether acetate, 1070 g of o-cresol novolac epoxy resin (manufactured by DIC Corporation, EPICLON N-695, softening point 95°C, epoxy equivalent 214, average number of functional groups 7.6), 360 g of acrylic acid and 1.5 g of hydroquinone were added, heated to 100°C and stirred to dissolve uniformly. Then, 4.3 g of triphenylphosphine was added, heated to 110°C, and after 2 hours of reaction, the temperature was raised to 120°C and the reaction was further carried out for 12 hours. In the obtained reaction solution, 415 g of aromatic hydrocarbon (SOLVESSO150) and 456.0 g of tetrahydrophthalic anhydride were added, and the reaction was carried out at 110°C for 4 hours. After cooling, a varnish F-3 with a solid content acid value of 89 mgKOH / g and a solid content of 65% was obtained.

[0145] (Preparation of resin composition)

[0146] The obtained varnishes (A-1-1), (A-1-2), (A-2-1), (A-2-2), (F-1), (F-2) and (F-3) were used to mix the various components shown in Table 1 in the above ratios (parts by mass), pre-mixed in a mixer, and then kneaded with a three-roll mill to prepare resin compositions of Examples 1 to 11 and Comparative Examples 1 to 7. The values ​​in the table are parts by mass unless otherwise specified. In addition, the values ​​in the table of each varnish and other components are expressed as solid content.

[0147] (Measurement method of Tg and loss tangent (tanδ))

[0148] The peaks of Tg and loss tangent (tanδ) are measured as follows: the cured coating film of the resin layer formed on the evaluation substrate for measuring the peaks of Tg and loss tangent (tanδ) described later is peeled off from the copper foil, and the cured coating film is measured using the tensile mode of the dynamic viscoelasticity measuring device (DMA, manufactured by TA Instruments Japan Co., Ltd., model: RSA-G2). The measurement conditions are as follows: the temperature range is -60°C to 300°C, the heating rate is 5°C / min, the frequency is 1Hz, the strain is 0.1%, and the sample size is 5mm in width × 50mm in length. The cured coating film is installed in a manner that the two ends in the width direction are respectively maintained, and the cured coating film overflowing from the chuck is removed. The chuck spacing is set to 10mm.

[0149] Table 1 shows together the peaks of Tg and loss tangent (tan δ) in the dynamic viscoelasticity measurement at a frequency of 1 Hz of the cured coating films of the resin compositions of Examples 1 to 11 and Comparative Examples 1 to 7.

[0150] (Preparation of an evaluation substrate for measuring Tg and loss tangent (tan δ) peaks (hereinafter referred to as a Tg etc. measurement evaluation substrate))

[0151] The photosensitive resin compositions of Examples 1 to 8 and Comparative Examples 1 to 6 were applied to the entire surface of a copper foil having a thickness of 18 μm by screen printing so that the film thickness after drying was 30 μm to form a resin layer. After that, the resin layer was dried in a hot air circulation drying oven at 80° C. for 30 minutes and then exposed to light at 900 mJ / cm using an exposure device equipped with a metal halide lamp (HMW-680-GW20: ORCMANUFACTURING CO., LTD.). 2 The resin layer was exposed to an exposure amount of 1000 nm and developed for 60 seconds (30° C., 0.2 MPa, 1 mass % Na2CO3 aqueous solution). After that, the resin layer was cured in a hot air circulation drying oven at 150° C. for 60 minutes to form a cured coating film of the resin layer, and a substrate for measuring and evaluating Tg was prepared.

[0152] The thermosetting resin compositions of Examples 9 to 11 and Comparative Example 7 were applied to the entire surface of a copper foil having a thickness of 18 μm by screen printing so that the film thickness after drying was 30 μm to form a resin layer. Thereafter, the resin layer was cured in a hot air circulation drying oven at 150° C. for 60 minutes to form a cured coating film of the resin layer, and a substrate for measuring and evaluating Tg, etc. was prepared.

[0153] [Table 1]

[0154]

[0155] (*1) (A) (A-1) Carboxyl-containing urethane resin having no aromatic ring: Varnish A-1-1 synthesized above

[0156] (*2) (A) (A-1) Carboxyl-containing urethane resin having no aromatic ring: Varnish A-1-2 synthesized above

[0157] (*3) (A) (A-2) Carboxyl-containing urethane resin derived from a diol having an aromatic ring and an aliphatic diisocyanate: Varnish A-2-1 synthesized above

[0158] (*4) (A) (A-2) Carboxyl-containing urethane resin derived from a diol having an aromatic ring and an aliphatic diisocyanate: Varnish A-2-2 synthesized above

[0159] (*5) Other carboxyl group-containing resin described in the description (1) of the component (F): Varnish F-1 synthesized above

[0160] (*6) Other carboxyl group-containing resin described in the explanation (2) of the component (F): Varnish F-2 synthesized above

[0161] (*7) (F) Component: Varnish F-3 synthesized above

[0162] (*8) (D) Component: Bisphenol A epoxy resin manufactured by Mitsubishi Chemical Corporation Trade name: jER828

[0163] (*9) (C) Component: 2,4,6-trimethylbenzoyldiphenylphosphine oxide, acylphosphine oxide, acylphosphine oxide-based photopolymerization initiator

[0164] (*10) Thermosetting catalyst: Dicyandiamide manufactured by Mitsubishi Chemical Corporation. Trade name: DICY7

[0165] (*11)Thermosetting catalyst: Nissan Chemical Co., Ltd. Melamine Trade name: Melamine

[0166] (*12) (B) Component: Bisphenol A type difunctional methacrylate manufactured by Shin-Nakamura Chemical Industry Co., Ltd. Trade name: BPE-900

[0167] (*13) Trifunctional (meth)acrylate: Trimethylolpropane EO-modified triacrylate manufactured by Toagosei Co., Ltd. Trade name: M-350

[0168] (*14) Hexafunctional (meth)acrylate: Dipentaerythritol hexaacrylate manufactured by Nippon Kayaku Co., Ltd. Trade name: DPHA

[0169] (*15) Dispersant: BYK Japan Co., Ltd. Wetting dispersant Trade name: Disperbyk-111

[0170] (*16) (E) Component: Rutile titanium oxide (surface treated with alumina + silica) manufactured by Ishihara Sangyo Co., Ltd. Trade name: CR-90

[0171] (*17) Silica manufactured by TOSOH SILICA CORPORATION Trade name: E-743 (average particle size 0.1 μm)

[0172] The resin compositions of Examples 1 to 11 and Comparative Examples 1 to 7 obtained in this manner were evaluated as follows.

[0173] (Preparation of substrate for evaluation of heat resistance, etc.)

[0174] The photosensitive resin compositions of Examples 1 to 8 and Comparative Examples 1 to 6 were applied to the entire surface of a copper solid substrate pre-treated by polishing by screen printing so that the film thickness after drying was 30 μm to form a resin layer. After that, the resin layer was dried in a hot air circulation drying oven at 80° C. for 30 minutes, and then exposed to light at 900 mJ / cm using an exposure device equipped with a metal halide lamp (HMW-680-GW20: ORC MANUFACTURING CO., LTD.). 2 The resin layer was exposed to an exposure amount of 1000 nm and developed for 60 seconds (30° C., 0.2 MPa, 1 mass % Na2CO3 aqueous solution). After that, the resin layer was cured in a hot air circulation drying oven at 150° C. for 60 minutes to form a cured coating film of the resin layer, and a substrate for evaluation of heat resistance was prepared.

[0175] The thermosetting resin compositions of Examples 9 to 11 and Comparative Example 7 were applied to the entire surface of a copper solid substrate pre-treated by polishing by screen printing so that the film thickness after drying was 30 μm to form a resin layer. Thereafter, the resin layer was dried in a hot air circulation drying oven at 80° C. for 30 minutes, and then cured in a hot air circulation drying oven at 150° C. for 60 minutes to form a cured coating film of the resin layer, thereby preparing a substrate for evaluation of heat resistance and the like.

[0176] (Evaluation of heat resistance)

[0177] A rosin-based flux was applied to each of the heat resistance evaluation substrates obtained above, and the substrates were immersed in a solder bath pre-set at 260°C for 5 seconds. The flux was then cleaned with a modified alcohol, and the expansion / peeling of the cured coating was visually evaluated. The evaluation criteria for heat resistance were as follows.

[0178] ○: There is no swelling or peeling in the cured coating film.

[0179] ×: There is swelling and peeling in the cured coating film.

[0180] (Evaluation of reflectivity)

[0181] The reflectance at 450 nm of the resin layer formed on each of the heat resistance evaluation substrates obtained above was measured using a spectrophotometer (manufactured by Konica Minolta, Inc., model: CM-5). The evaluation results are shown in the "After Curing" row in Table 1. The evaluation criteria for the reflectance were as follows.

[0182] ◎: Reflectivity is 90% or more.

[0183] ○: The reflectance is 86% or more and less than 90%.

[0184] ×: The reflectance is less than 86%.

[0185] The reflectance of the resin layer on each evaluation substrate after the above heat resistance evaluation was also measured and evaluated based on the same evaluation criteria as above. The evaluation results are shown in the "After Reflow" row in Table 1.

[0186] (Warp Evaluation)

[0187] When preparing the above-mentioned substrate for measuring and evaluating Tg, etc., in the case of the photosensitive resin composition of Examples 1 to 8 and Comparative Examples 1 to 6, the coating formed on the copper foil obtained after development is cut into 5 cm × 5 cm pieces together with the copper foil, and heat-cured in a hot air circulation drying furnace at 150°C for 60 minutes, and then returned to room temperature. After leaving the cut 5×5 cm pieces of each cured coating with copper foil (hereinafter referred to as a sample) on a workbench for 1 hour, the height of the four ends of the sample from the surface of the workbench is measured with a ruler. For each sample, a total of 3 similar tests are performed, and the average value of the 3 tests is calculated. The evaluation results are shown in the "After Curing" row in Table 1. The evaluation criteria for warping are set as follows.

[0188] When preparing the above-mentioned substrate for measuring and evaluating Tg, etc., in the case of the thermosetting resin composition of Examples 9 to 11 and Comparative Example 7, the coating formed on the copper foil obtained after drying is cut into 5 cm × 5 cm pieces together with the copper foil, and heat-cured in a hot air circulation drying furnace at 150°C for 60 minutes, and then returned to room temperature. After leaving the cut 5×5 cm pieces of each cured coating with copper foil (hereinafter referred to as a sample) on a workbench for 1 hour, the height of the four ends of the sample from the surface of the workbench is measured with a ruler. For each sample, a total of 3 similar tests are performed, and the average value of the 3 tests is calculated. The evaluation results are shown in the "After Curing" row in Table 1. The evaluation criteria for warping are set as follows.

[0189] It should be noted that in the evaluation of the warpage, copper foil was used as the base material of the evaluation substrate instead of the glass listed in the subject of the present invention. Glass is less likely to warp than copper foil, so when the same test is performed with the same size as the above sample, the warpage value is too small and it is very difficult to make an evaluation judgment. Therefore, the test is performed using copper foil with large warpage so that the evaluation judgment becomes clear. If there is a good warpage reduction effect in the evaluation criteria of the warpage, it is considered that there is also a sufficient warpage reduction effect in the case of glass.

[0190] ◎: Total height is less than 40 mm.

[0191] ○: The total height is 40 mm or more and less than 60 mm.

[0192] △: The total height is 60 mm or more and less than 80 mm.

[0193] ×: The total height is 80 mm or more.

[0194] In addition, the evaluation substrate was subjected to a reflow process once at a maximum temperature of 260° C. using a reflow device (NIS-20-82C manufactured by EIGHTECH TECTRON CO., LTD.). After that, the reflectivity was measured and evaluated based on the same criteria as the above evaluation. The evaluation results are shown in the "After Reflow" row in Table 1.

[0195] (Evaluation of resistance to chemical gold plating)

[0196] When preparing the above-mentioned substrate for evaluation of heat resistance, etc., in the case of the photosensitive resin compositions of Examples 1 to 8 and Comparative Examples 1 to 6, a negative film with L / S (line width / line spacing) = 100 / 300 μm is used to form an anti-etching pattern (cured coating film) on a copper circuit pattern substrate with a thickness of 18 μm that has been treated with sulfuric acid.

[0197] When preparing the above-mentioned substrate for evaluating heat resistance, etc., in the case of the thermosetting resin composition of Examples 9 to 11 and Comparative Example 7, an anti-etching pattern (cured coating film) having an opening with a diameter of 2 mm is formed on a copper circuit pattern substrate with a thickness of 18 μm that has been treated with sulfuric acid by pattern printing.

[0198] On this basis, the obtained evaluation substrate was plated with gold using a commercially available chemical nickel plating bath and a chemical gold plating bath under the conditions of 5 μm nickel and 0.03 μm gold, and the presence or absence of peeling of the resist pattern layer and the presence or absence of plating layer penetration were evaluated, and then the presence or absence of peeling of the resist pattern layer was evaluated by tape stripping. The evaluation criteria for chemical gold plating resistance were set as follows.

[0199] ○: No penetration of the plating layer or peeling of the resist pattern layer was observed.

[0200] △: Some penetration was observed after plating, and peeling of the resist pattern layer was also observed after the tape was peeled off.

[0201] ×: The resist pattern layer peeled off after plating.

[0202] As is apparent from the above, according to the present invention, a resin composition capable of achieving both low warpage and high reflectivity after the reflow step can be provided.

Claims

1. A resin composition, characterized in that The invention comprises: (A) a carboxyl-containing urethane resin and (E) a white colorant, In the dynamic viscoelasticity measurement of the cured coating film of the resin composition at a frequency of 1 Hz, The loss tangent peak temperature (Tg) is below 100°C. The peak of the loss tangent is in the range of 0.5 to 1.

5.

2. The fat composition according to claim 1, characterized in that The (E) white coloring agent is titanium oxide.

3. The resin composition according to claim 1, characterized in that The (A) carboxyl group-containing urethane resin includes a carboxyl group-containing urethane resin having no aromatic ring.

4. The resin composition according to claim 1, characterized in that Contains (D) epoxy resin.

5. The resin composition according to claim 1, characterized in that (F) other carboxyl group-containing resin other than the (A) carboxyl group-containing urethane resin is included. 6 . A dry film comprising a resin layer, wherein the resin layer is obtained by applying the resin composition according to claim 1 on a film and drying the film.

7. A solidified product, characterized in that: The resin composition is obtained from the resin composition according to claim 1.

8. A solidified product, characterized in that: It is obtained from the dry film according to claim 6.

9. An electronic component, characterized in that: A cured product according to claim 7.

10. An electronic component, characterized in that: A cured product according to claim 8.