Hot-dip plated steel sheet

By forming patterned parts and non-patterned parts on the surface of the hot-dip plated steel plate, and using the design of specific element concentration areas and interface alloy layers, the problem of degradation of durability and corrosion resistance when the surface text or design of the hot-dip plated steel plate is solved. , achieves excellent durability and corrosion resistance.

CN119032195AActive Publication Date: 2024-11-26NIPPON STEEL CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380034445.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-06-10
Filing Date
2023-06-09
Publication Date
2024-11-26
Estimated Expiration
2043-06-09

AI Technical Summary

Technical Problem

The prior art is difficult to show text or design on the surface of hot-dip plated steel plate to maintain durability and corrosion resistance, while avoiding the problem of decreasing adhesion of the coating.

Method used

By forming patterned parts and non-patterned parts on the surface of the hot-dip plated steel plate, and having specific element concentration areas and interface alloy layers at the patterned parts, combined with appropriate chemical composition and process processing, the durability and corrosion resistance of the patterned parts are ensured. , and improve the adhesion of the coating.

Benefits of technology

It is achieved with excellent durability and corrosion resistance to display text or design on the surface of the hot-dip plated steel plate, and the adhesion of the patterned portion is the same as that of the non-patterned portion, thereby avoiding peeling of the plating layer and reducing corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005087119970000231
    Figure BDA0005087119970000231
  • Figure BDA0005087119970000241
    Figure BDA0005087119970000241
  • Figure BDA0005087119970000251
    Figure BDA0005087119970000251
Patent Text Reader

Abstract

This hot-dip plated steel sheet is provided with a hot-dip plating layer formed on the surface of a steel sheet, the hot-dip plating layer containing 4-22 mass% of Al and 1.0-10 mass% of Mg, the remainder containing Zn and impurities, a pattern portion and a non-pattern portion being formed in the hot-dip plating layer, and an element concentrated region containing an element M and an interface alloy layer containing Fe and Al being present at the interface between the steel sheet and the hot-dip plating layer at the pattern portion, the average concentration of the element M contained in the hot-dip plating layer present in the pattern portion and the element concentration region is 0.0010-2 mass%, and the element M is concentrated by two times or more or is non-uniform in the element concentration region relative to the hot-dip plating layer present in the pattern portion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to hot-dip coated steel sheets.

[0002] This application claims priority based on Japanese Patent Application No. 2022-094362 filed in Japan on June 10, 2022, and the contents are incorporated herein by reference. Background Art

[0003] Zn-Al-Mg hot-dip galvanized steel sheets, which have higher corrosion resistance than hot-dip galvanized steel sheets, are widely used in various manufacturing industries such as building materials, home appliances, and automobiles, and their usage has been increasing in recent years.

[0004] However, in order to express characters, designs, etc. on the surface of the hot-dip coating layer of the hot-dip coated steel sheet, characters, designs, etc. may be expressed on the surface of the hot-dip coating layer by subjecting the hot-dip coating layer to a process such as printing or painting.

[0005] However, if the hot-dip coating is printed or coated, there is a problem of increased cost and time for applying text or design. Furthermore, when the surface of the coating is made to show text, design, etc. by printing or coating, not only the metallic gloss appearance supported by the demander disappears, but also due to the time-deterioration of the coating itself and the time-deterioration of the adhesion of the coating, the durability is poor, and it is possible that the text, design, etc. disappear over time. In addition, when the surface of the coating is made to show text, design, etc. by printing ink, although the cost and time can be suppressed relatively, it is worried that the corrosion resistance of the hot-dip coating is reduced due to the ink. Furthermore, when the pattern design is shown by the grinding of the hot-dip coating, although the durability of the pattern design, etc. is excellent, it is inevitable that the thickness of the hot-dip coating at the grinding position is greatly reduced, and the reduction of the corrosion resistance is worried about the reduction of the coating characteristics.

[0006] As shown in the following patent documents, various technologies have been developed for Zn-Al-Mg hot-dip plated steel sheets, but there is no known technology for improving the durability when letters, designs, etc. are expressed on the surface of the plated layer.

[0007] Regarding Zn—Al—Mg based hot dip plated steel sheets, there is a conventional technology which aims to make the pear-skin-like plating appearance seen on the Zn—Al—Mg based hot dip plated steel sheets more beautiful.

[0008] For example, Patent Document 1 describes a Zn-Al-Mg hot-dip plated steel sheet having a fine texture and smooth pear-skin appearance with many glossy parts, that is, a good pear-skin appearance with many white parts per unit area and a large proportion of the area of ​​the glossy parts. In addition, Patent Document 1 describes that the unpreferable pear-skin state is a state showing a surface appearance in which amorphous white parts and round glossy parts are mixed and scattered on the surface.

[0009] In addition, Patent Document 2 describes a Zn-Al-Mg based plated steel sheet, which improves the appearance of the plating by making the portion in the thickness direction cross section of the plating layer where no Al crystals exist between the interface between the plating layer and the base metal and the plating surface layer account for 10% to 50% of the width direction length of the cross section.

[0010] Furthermore, Patent Document 3 describes a hot-dip galvanized steel sheet with excellent formability, wherein the center line average roughness Ra of the plated steel sheet surface is 0.5 to 1.5 μm, the PPI (the number of peaks with a size of 1.27 μm or more contained in every 1 inch (2.54 cm)) is 150 to 300, and the Pc (the number of peaks with a size of 0.5 μm or more contained in every 1 cm) is Pc ≥ PPI / 2.54+10.

[0011] In addition, Patent Document 4 describes a highly corrosion-resistant hot-dip galvanized steel sheet in which the glossiness of the entire coating layer is increased and the uniformity of the appearance is improved by refining the ternary eutectic structure of Al / MgZn2 / Zn.

[0012] However, when characters or the like are displayed on the surface of a plating layer, a technique for improving the durability thereof without reducing the corrosion resistance has not been known in the past.

[0013] Prior art literature

[0014] Patent Literature

[0015] Patent Document 1: Japanese Patent No. 5043234

[0016] Patent Document 2: Japanese Patent No. 5141899

[0017] Patent Document 3: Japanese Patent No. 3600804

[0018] Patent Document 4: International Publication No. 2013 / 002358 Summary of the invention

[0019] Problems to be solved by the invention

[0020] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a hot-dip plated steel sheet which can display characters, designs, etc. on the surface of the hot-dip plated layer, has excellent durability and corrosion resistance, and has excellent adhesion of the hot-dip plated layer at the portion where the characters or designs are displayed.

[0021] Means for solving problems

[0022] In order to solve the above-mentioned problems, the present invention adopts the following configuration.

[0023] [1] A hot-dip plated steel sheet comprising a steel sheet and a hot-dip plated layer formed on a surface of the steel sheet,

[0024] The hot-dip coating layer contains, as an average composition, 4 to 22 mass % of Al, 1.0 to 10 mass % of Mg, and the remainder contains Zn and impurities.

[0025] The hot-dip galvanized layer has a pattern portion and a non-pattern portion.

[0026] At the interface between the steel plate and the hot-dip galvanized layer at the pattern portion, there is an element-concentrated region containing any one or two or more elements M selected from the group consisting of Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, Ni, Ti, Zr, Mo, W, REM, Hf, and C, and an interface alloy layer containing Fe and Al.

[0027] The average concentration of the element M contained in the hot-dip coating layer of the pattern portion and the element-concentrated region is 0.0010 to 2% by mass.

[0028] In the element concentrated region, the element M is concentrated at least twice as much as the hot-dip plating layer present in the pattern portion, or the element M is unevenly present.

[0029] [2] The hot-dip plated steel sheet according to [1], further comprising an interface alloy layer containing Fe and Al at an interface between the steel sheet and the hot-dip plated layer in the non-pattern portion.

[0030] [3] The hot-dip plated steel sheet according to [1] or [2], wherein the concentration of the element M at the interface of the pattern portion is 1.5 times or more the concentration of the element M at the interface of the non-pattern portion.

[0031] [4] The hot-dip coated steel sheet according to any one of [1] to [3], wherein the pattern portion is arranged in a shape that is any one of a straight line portion, a curved line portion, a dot portion, a figure, a number, a symbol or a character, or a combination of two or more of these.

[0032] [5] The hot-dip plated steel sheet according to any one of [1] to [4], wherein the hot-dip plated layer further contains Si: 0.0001 to 2 mass % in terms of average composition.

[0033] [6] The hot-dip plated steel sheet according to [5], wherein the interface alloy layer formed in the pattern portion further contains Si.

[0034] [7] The hot-dip plated steel sheet according to [5] or [6], wherein the interface alloy layer formed in the non-pattern portion further contains Si.

[0035] [8] The hot-dip coated steel sheet according to any one of [1] to [7], characterized in that the hot-dip coated layer excluding the element-concentrated region further contains any one or more of Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C in an average composition amounting to 0.0001 to 1 mass %.

[0036] [9] The hot-dip coated steel sheet according to any one of [1] to [8], wherein the total amount of the hot-dip coating on both sides of the steel sheet is 30 to 600 g / m 2 .

[0037] Effects of the Invention

[0038] According to the present invention, it is possible to provide a hot-dip plated steel sheet in which characters, designs, etc. can be expressed on the surface of the hot-dip plated layer, the durability and corrosion resistance thereof are excellent, and the adhesion of the hot-dip plated layer at the portion where the characters or designs are expressed is excellent. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a schematic cross-sectional view illustrating a pattern portion and a non-pattern portion of a hot-dip plated steel sheet according to an embodiment of the present invention. DETAILED DESCRIPTION

[0040] A hot-dip plated steel sheet according to an embodiment of the present invention will be described.

[0041] The hot-dip plated steel sheet of the present embodiment includes a steel sheet and a hot-dip plated layer formed on the surface of the steel sheet.

[0042] The hot-dip coating layer contains, as an average composition, 4 to 22% by mass of Al, 1.0 to 10% by mass of Mg, and the remainder includes Zn and impurities.

[0043] In the hot-dip plating layer, a pattern portion and a non-pattern portion are formed.

[0044] An element-concentrated region and an interface alloy layer are present at the interface between the steel plate in the pattern portion and the hot-dip galvanized layer.

[0045] An interface alloy layer is present at the interface between the steel plate in the non-pattern portion and the hot-dip coating layer.

[0046] The pattern portion is arranged so as to have any one of a straight line portion, a curved line portion, a dot portion, a figure, a number, a symbol, or a character, or a shape formed by combining two or more of them.

[0047] The pattern portion is a portion formed intentionally.

[0048] The material of the steel plate that serves as the base of the hot-dip coating is not particularly limited. Although the details will be described below, as the material, general steel can be used without particular limitation, and Al-killed steel and some high-alloy steel can also be used, and the shape is not particularly limited. The hot-dip coating of this embodiment can be formed by applying the hot-dip coating method described later to the steel plate.

[0049] Next, the chemical composition of the hot-dip coating will be described.

[0050] The hot-dip coating layer contains Al: 4-22 mass %, Mg: 1.0-10 mass %, and the remainder contains Zn and impurities as an average composition. It is further preferred that the hot-dip coating layer contains Al: 4-22 mass %, Mg: 1.0-10 mass %, and the remainder is composed of Zn and impurities as an average composition. In addition, the hot-dip coating layer may also contain Si: 0.0001-2 mass % as an average composition. Furthermore, the hot-dip coating layer may also contain any one or more of Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C in a total of 0.0001-1 mass %.

[0051] The content of Al is in the range of 4 to 22 mass % based on the average composition. It is preferable that Al is contained in order to ensure corrosion resistance. If the content of Al in the hot-dip coating is 4 mass % or more, the effect of improving corrosion resistance is further improved. If Al exceeds 22 mass %, the effect of improving corrosion resistance is saturated. From the viewpoint of corrosion resistance, the lower limit is preferably 5 mass %, more preferably 6 mass %. The upper limit is preferably 18 mass %, more preferably 16 mass %.

[0052] The content of Mg is in the range of 1.0 to 10% by mass based on the average composition. It is preferable to contain Mg in order to improve corrosion resistance. If the content of Mg in the hot-dip coating is 1.0% by mass or more, the effect of improving corrosion resistance is further improved. However, if Mg exceeds 10% by mass, the dross generation in the coating bath becomes significant, and it becomes difficult to stably manufacture the hot-dip coated steel sheet, so the content of Mg is set to 10% by mass or less. From the viewpoint of the balance between corrosion resistance and dross generation, the lower limit of the Mg content is preferably 1.5% by mass, and more preferably 2.0% by mass. The upper limit is preferably 6.0% by mass, and more preferably 5.0% by mass.

[0053] It is also possible to contain 0.0001 to 2 mass % Si in the hot-dip coating in terms of average composition. Si is an effective element for improving the adhesion of the hot-dip coating. In order to show the effect of improving adhesion by making the hot-dip coating contain more than 0.0001 mass % Si, it is preferred to contain more than 0.0001 mass % Si. On the other hand, even if more than 2 mass % Si is contained, the effect of improving the adhesion of the coating is saturated, so even when the hot-dip coating contains Si, the content of Si is set to less than 2 mass %. From the viewpoint of coating adhesion, the lower limit of the Si content in the hot-dip coating can also be set to 0.0010, or 0.0100 mass %. The upper limit can also be set to 1.0 mass %, or 0.8 mass %.

[0054] The hot-dip coating may contain one or more of Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C in an average composition of 0.0001 to 1 mass %. By containing these elements, the corrosion resistance of the hot-dip coating can be further improved. REM is one or more of the rare earth elements with atomic numbers of 57 to 71 in the periodic table. These elements may be contained in the hot-dip coating by adding them to the hot-dip coating bath, and may be contained in the hot-dip coating by diffusion from the solidification nucleus, but in the present embodiment, as long as the above elements are in the coating layer other than the element-concentrated area, the total amount is in the range of 0.0001 to 1 mass %.

[0055] The remainder of the chemical composition of the hot-dip coating is zinc and impurities. The impurities include substances other than zinc that are inevitably contained in the base metal and substances that are contained by dissolving the steel in the plating bath.

[0056] It should be noted that the average composition of the hot-dip coating can be measured by the following method. First, it can be obtained by the following method: after removing the surface coating with a coating stripper that does not corrode the coating (for example, NEOREVER SP-751 manufactured by Sancai Chemical Co., Ltd.), the hot-dip coating is dissolved with hydrochloric acid to which an inhibitor (for example, HIBIRON manufactured by SUGIMURA Chemical Industrial Co., Ltd.) is added, and the resulting solution is subjected to inductively coupled plasma (ICP) emission spectrometry analysis. In addition, in the case of not having a surface coating, the removal operation of the surface coating can be omitted.

[0057] Next, the structure of the hot-dip coating is described. The structure of the hot-dip coating of the present embodiment may also have the following structure, for example. As a result, the appearance of the surface of the hot-dip coating becomes a pear-skin-like appearance, and the aesthetics become excellent. It should be noted that the structure of the hot-dip coating can be obtained as long as the coating has the above-mentioned chemical composition, so it is not necessary to limit the structure of the hot-dip coating in the present invention.

[0058] The hot-dip galvanized layer containing Al, Mg and Zn includes [Al phase] and [ternary eutectic structure of Al / Zn / MgZn2]. Specifically, it has a form in which [Al phase] is included in the matrix of [ternary eutectic structure of Al / Zn / MgZn2]. Furthermore, [MgZn2 phase] and [Zn phase] may also be included in the matrix of [ternary eutectic structure of Al / Zn / MgZn2]. In addition, in the case of containing Si, [Mg2Si phase] may also be included in the matrix of [ternary eutectic structure of Al / Zn / MgZn2].

[0059] [Ternary eutectic structure of Al / Zn / MgZn2]

[0060] [Ternary eutectic structure of Al / Zn / MgZn2] refers to the ternary eutectic structure of Al phase, Zn phase and intermetallic compound MgZn2 phase. The Al phase forming the ternary eutectic structure is equivalent to, for example, the "Al" phase at high temperature in the ternary equilibrium state diagram of Al-Zn-Mg (which is an Al solid solution with solid dissolved Zn, containing a small amount of Mg).

[0061] The Al" phase at high temperature usually separates into a fine Al phase and a fine Zn phase at room temperature. The Zn phase in the ternary eutectic structure is a Zn solid solution in which a small amount of Al and, depending on the situation, a small amount of Mg is further dissolved. The MgZn2 phase in the ternary eutectic structure is an intermetallic compound phase that exists near Zn: about 84 mass% in the Zn-Mg binary system equilibrium state diagram.

[0062] From the state diagram, it is believed that: no other added elements are dissolved in each phase, or even if dissolved, they are only in very small amounts. However, since their amounts cannot be clearly distinguished by ordinary analysis, the ternary eutectic structure containing these three phases is represented as [ternary eutectic structure of Al / Zn / MgZn2] in this specification.

[0063] 〔Al phase〕

[0064] [Al phase] refers to a phase that has clear boundaries and appears to be island-shaped in the matrix of [ternary eutectic structure of Al / Zn / MgZn2], which is equivalent to the "Al" phase at high temperature in the ternary equilibrium state diagram of Al-Zn-Mg, for example (which is an Al solid solution with dissolved Zn, containing a small amount of Mg). Regarding this Al" phase at high temperature, the amount of dissolved Zn and Mg varies depending on the Al and Mg concentrations of the plating bath. This high-temperature Al" phase is usually separated into fine Al phase and fine Zn phase at room temperature, but it is believed that the island shape seen at room temperature is caused by the shape of the Al" phase at high temperature.

[0065] From the state diagram, it is believed that no other added elements are dissolved in this phase, or even if dissolved, they are only in very small amounts. However, it is not possible to clearly distinguish them through conventional analysis, so the phase derived from the Al" phase at high temperature and the shape of the Al" phase is referred to as "Al phase" in this specification.

[0066] The [Al phase] and the Al phase forming the [ternary eutectic structure of Al / Zn / MgZn2] can be clearly distinguished by microscopic observation.

[0067] 〔Zn phase〕

[0068] The [Zn phase] refers to a phase that has a clear boundary and appears to be an island in the matrix of the [ternary eutectic structure of Al / Zn / MgZn2], but in fact, a small amount of Al and a small amount of Mg may be dissolved in the phase. From the state diagram, it is believed that no other added elements are dissolved in the phase, or even if dissolved, they are extremely small.

[0069] The [Zn phase] can be clearly distinguished from the Zn phase that forms the [ternary eutectic structure of Al / Zn / MgZn2] in microscopic observation. In the hot-dip coating of the present embodiment, the [Zn phase] may be included depending on the manufacturing conditions, but the influence on the corrosion resistance caused by the [Zn phase] is basically not observed. Therefore, even if the [Zn phase] is included in the hot-dip coating, there is no particular problem.

[0070] 〔MgZn2 phase〕

[0071] The [MgZn2 phase] refers to a phase that has a clear boundary and appears to be an island in the matrix of the [ternary eutectic structure of Al / Zn / MgZn2], but in fact, a small amount of Al may be dissolved in it. From the state diagram, it is believed that no other added elements are dissolved in this phase, or even if they are dissolved, they are extremely small.

[0072] The [MgZn2 phase] can be clearly distinguished from the MgZn2 phase that forms the [ternary eutectic structure of Al / Zn / MgZn2] in microscopic observation. In the hot-dip galvanized layer of this embodiment, the [MgZn2 phase] may not be contained depending on the manufacturing conditions, but it will be included in the hot-dip galvanized layer under most manufacturing conditions.

[0073] 〔Mg2Si phase〕

[0074] [Mg2Si phase] refers to a phase that has a clear boundary and appears to be an island in the solidified structure of the Si-added coating. From the state diagram, it is believed that there is no solid solution of Zn, Al, or other added elements in the [Mg2Si phase], or even if they are solid-dissolved, they are extremely small amounts. [Mg2Si phase] can be clearly distinguished from other phases in the hot-dip coating under microscopic observation.

[0075] The hot-dip coating of this embodiment is formed by immersing the steel sheet in a coating bath, then scooping it up, and then solidifying the molten metal attached to the surface of the steel sheet. At this time, the [Al phase] is formed first, and then as the temperature of the molten metal decreases, the [ternary eutectic structure of Al / Zn / MgZn2] is formed. Depending on the chemical composition of the hot-dip coating (i.e., the chemical composition of the coating bath), in the matrix of the [ternary eutectic structure of Al / Zn / MgZn2], [Mg2Si phase], [MgZn2 phase], or [Zn phase] may also be formed.

[0076] Next, the pattern portion and the non-pattern portion of the hot-dip plated layer will be described.

[0077] On the surface of the hot-dip coating layer of the present embodiment, a pattern portion and a non-pattern portion are formed so as to be arranged in a prescribed shape. From the viewpoint of ensuring the beauty of the pattern portion, the pattern portion is preferably arranged so as to be in a prescribed shape. Further, from the viewpoint of ensuring the visual recognition of the pattern portion, the larger the size of the pattern portion, the more preferable. For example, the pattern portion preferably has an artificial shape. The pattern portion is preferably arranged in an intentional shape. The pattern portion is preferably arranged so as to be in a shape that is any one of a straight line portion, a curved line portion, a dot portion, a figure, a number, a symbol, or a character, or a shape formed by combining two or more of them. For example, on the surface of the hot-dip coating layer, a character string, a number string, a symbol, a mark, a line drawing, a design drawing, or a combination thereof formed by the pattern portion appears. The straight line portion and the curved line portion in the pattern portion are preferably each 1 mm or more in length. It can be said that the pattern portion is intentionally formed by showing these shapes. The straight line portion and the curved line portion in the pattern portion preferably have a width that can be recognized by visual inspection as described later, and are each 1 mm or more in length. The equivalent circle diameter of the dot portion in the pattern portion is preferably 1 mm or more and less than 10 mm, and a plurality of dot portions are more preferably arranged regularly. Further, when the pattern portion is a figure, a number, a symbol, or a character, it is preferable that these shapes can be recognized by visual inspection as described later. It can be said that it is further intentionally formed by showing such dimensions and shapes. Further, the non-pattern portion is an area other than the pattern portion. Further, even if a part of the shape of the pattern portion is missing, such as dot omission, as long as it can be recognized as a whole, it is also allowed. Further, the non-pattern portion may also be in a shape that trims the boundary of the pattern portion.

[0078] When a shape formed by combining any one of a straight line portion, a curved line portion, a dot portion, a figure, a number, a symbol, or a character, or two or more of them is arranged on the surface of the hot-dip coating layer, these regions can be regarded as the pattern portion, and the regions other than these can be regarded as the non-pattern portion. This shape is an intentionally or artificially formed shape by the manufacturing method described later, and is not a naturally formed shape. As long as a person skilled in the art who is familiar with the appearance of a normal hot-dip coating layer, it is possible to easily distinguish the pattern portion having an artificial shape from the non-pattern portion.

[0079] The pattern portion is preferably formed with a size that can distinguish the existence of the pattern portion by visual observation with the naked eye or by visual observation with a magnifying glass or a microscope. In addition, the non-pattern portion is an area that occupies most of the hot-dip coating (the surface of the hot-dip coating), and the pattern portion is configured in a specified shape in the non-pattern portion. Specifically, the pattern portion is configured in the non-pattern portion in a manner that forms a shape that is any one of a straight line portion, a curved line portion, a figure, a dot portion, a figure, a number, a symbol or a text, or a shape that is a combination of two or more of them. By intentionally adjusting the shape of the pattern portion, any one of a straight line portion, a curved line portion, a figure, a dot portion, a figure, a number, a symbol or a text, or a shape that is a combination of two or more of them, is shown on the surface of the hot-dip coating. For example, a character column, a number column, a symbol, a mark, a line diagram, a design drawing or a combination thereof formed by the pattern portion is shown on the surface of the hot-dip coating. The shape is a shape that is intentionally or artificially formed by the manufacturing method described later, and is not naturally formed. Those skilled in the art who are familiar with the appearance of a common hot-dip coating can easily distinguish between a patterned portion having an artificial shape and a non-patterned portion. In particular, an area having an artificial shape and having a size of at least one side of a square of 1 mm (this size may be less than 1 mm or greater than 1 mm) can be easily determined as a patterned portion.

[0080] It should be noted that, from the viewpoint of improving the visual recognition of the pattern portion, the area ratio of the pattern portion on the surface of the hot-dip galvanized layer is preferably significantly smaller than that of the non-pattern portion. For example, the area ratio of the pattern portion on the surface of the hot-dip galvanized layer is preferably less than 30%, less than 25%, less than 20%, or less than 15%.

[0081] The pattern part is a region with high metallic gloss on the surface. In addition, the non-pattern part is a region with low metallic gloss on the surface, showing white or gray, and is a region showing the pear-skin appearance seen on Zn-Al-Mg hot-dip plated steel sheets. Therefore, the pattern part and the non-pattern part can be distinguished by naked eyes.

[0082] Furthermore, the pattern portion and the non-pattern portion can also be identified under a microscope. Specifically, the shape formed by the pattern portion can be identified with a viewing field of less than 50 times. As long as it is a viewing field of less than 50 times, the pattern portion and the non-pattern portion can be identified by the difference in their surface states.

[0083] The pattern portion and the non-pattern portion are distinguishable at a magnification of preferably 20 times or less, more preferably 10 times or less, and even more preferably 5 times or less.

[0084] The pattern portion and the non-pattern portion may further satisfy any one of the following (a), (b), and (c).

[0085] (a) The pattern portion is a region where the exposure ratio of the [Al phase] on the surface of the hot-dip galvanized layer is 30 area % or less, and the non-pattern portion is a region where the exposure ratio of the [Al phase] on the surface of the hot-dip galvanized layer exceeds 30 area %.

[0086] (b) The pattern portion is a region where the arithmetic mean surface roughness Sa is 1.0 μm or less, and the non-pattern portion is a region where the arithmetic mean surface roughness Sa exceeds 1.0 μm.

[0087] (c) The relationship between the reflected light from the pattern part in the normal direction and the reflected light from the non-pattern part in the normal direction and the incident light having an incident angle in the range of greater than 0° and less than 90° relative to the normal direction of the steel plate surface satisfies the following equations (1) and (2).

[0088] |I PH -I BH | / |I PM -I BM |<1.0 (1)

[0089] |I PL -I BL | / |I PM -I BM |<1.0 (2)

[0090] In formulas (1) to (2), I PH : Reflection intensity of the pattern portion in the normal direction relative to incident light with an incident angle of 0° or more and less than 35°, I BH : Reflection intensity of the non-pattern portion in the normal direction relative to incident light with an incident angle of 0° or more and less than 35°, I PM : Reflection intensity of the pattern portion in the normal direction relative to incident light with an incident angle of 35° to 80°, I BM : Reflection intensity of the non-pattern part in the normal direction relative to the incident light with an incident angle of 35° to 80°, I PL : Reflection intensity of the pattern portion in the normal direction relative to incident light with an incident angle of more than 80° and less than 90°, I BL : Reflection intensity of the non-pattern portion in the normal direction with respect to incident light having an incident angle of more than 80° and less than 90°.

[0091] In the hot-dip coating, at least [Al phase] and [ternary eutectic structure of Al / Zn / MgZn2] exist, but in the pattern part, [Al phase] is unevenly present on the steel sheet side in the thickness direction of the hot-dip coating, while on the surface side in the thickness direction, [Al phase] is relatively small, and structures or phases other than [Al phase] are more present. Therefore, in the pattern part, the exposure ratio of [Al phase] at the surface of the hot-dip coating is less than 30 area%.

[0092] In addition, there is a relatively large amount of [ternary eutectic structure of Al / Zn / MgZn2] on the surface of the pattern part, but since the [ternary eutectic structure of Al / Zn / MgZn2] forms a relatively flat surface during the solidification of the hot-dip coating, the arithmetic mean surface roughness Sa of the pattern part becomes below 1.0 μm.

[0093] In this way, it is presumed that in the pattern portion, the exposure ratio of the [Al phase] is 30 area % or less, or the arithmetic mean surface roughness Sa is relatively small, 1.0 μm or less, and thus a metallic luster is exhibited.

[0094] On the other hand, in the hot-dip coating, at least [Al phase] and [ternary eutectic structure of Al / Zn / MgZn2] exist, but in the non-patterned portion, [Al phase] is not unevenly present on the steel sheet side of the hot-dip coating in the thickness direction, but is relatively widely distributed in the entire thickness direction. Therefore, in the non-patterned portion, the exposure ratio of [Al phase] at the surface of the hot-dip coating exceeds 30% by area.

[0095] In addition, in this way, the exposed area of ​​the [Al phase] is larger in the non-patterned portion than in the first region. The [Al phase] is a phase formed in the early stage of solidification of the hot-dip galvanized layer and crystallizes in a dendrite shape. Since the [Al phase] crystallized in a dendrite shape is relatively present on the surface of the hot-dip galvanized layer, the arithmetic mean surface roughness Sa of the non-patterned portion becomes a range exceeding 1.0 μm.

[0096] In this way, it is estimated that in the non-pattern portion, since the exposure ratio of the [Al phase] exceeds 30 area % or the arithmetic mean surface roughness Sa is relatively large and exceeds 1.0 μm, light incident on the non-pattern portion is diffusely reflected and appears white to gray.

[0097] The exposure ratio of the [Al phase] is measured by the following method. First, the surface of the hot-dip galvanized layer is photographed with a scanning electron microscope at 100 times magnification, and the surface analysis of the element distribution is performed using an energy dispersive X-ray element analyzer (EDS) attached to the scanning electron microscope. For example, 5 photographs of 1 mm2 of the pattern part are prepared. 2 Field of view images, 5 images of the non-patterned area 1mm 2Image of the field of view. For each image, commercially available image analysis software is used to measure the area of ​​the [Al phase] exposed to the surface of the hot-dip galvanized layer. The [Al phase] can be obtained by observing the morphology of the [Al phase] using the Al-concentrated area in the surface analysis and the reflected electron image. The [Al phase] exists in the form of dendrites in most cases. In each of the patterned part and the non-patterned part, the average value of the exposed area of ​​the [Al phase] in 5 images is obtained. Then, by dividing the average value of the exposed area of ​​the [Al phase] by the total area of ​​the observation field of view, the average exposed area ratio (%) of the [Al phase] in the observation field of view is obtained in the patterned part and the non-patterned part, respectively. The average exposed area ratio (%) of the [Al phase] obtained in this way is used as the exposure ratio of the [Al phase]. It should be noted that, for example, the field of view to be photographed can be set to be larger than 1 mm. 2 The field of view is smaller than 1mm. 2 In the case of a field of view of 5 mm, as long as the total area is 5 mm 2 That's it.

[0098] The arithmetic mean surface roughness Sa is measured by the following method. Using a 3D laser microscope (manufactured by KEYENCE Co., Ltd.), the height Z is measured at a measurement interval of 50 μm with a 20x standard lens installed. The number of measurement points is preferably set to 100 points, 10 points in the vertical direction and 10 points in the horizontal direction. When the number of measurement points is set to 100 points and the obtained height Z100 points are set to height Z1 to height Z100, Sa is calculated using the following formula. Zave is set to the average of the height Z100 points. Sa = 1 / 100 × Σ[x = 1→100] (|height Zx-Zave|)

[0099] The [Al phase] generated during the solidification of the hot-dip galvanized layer usually crystallizes in the entire thickness direction of the hot-dip galvanized layer. However, if a substance that serves as a solidification nucleus is pre-configured on the surface of the steel plate, in the area where the solidification nucleus is configured, when the molten metal attached to the surface of the steel plate solidifies, a large amount of [Al phase] is crystallized using the solidification nucleus on the surface of the steel plate as the nucleus. The generated [Al phase] is formed on the side closer to the steel plate. In addition, in the area where the solidification nucleus exists, since the [Al phase] is generated at a relatively high density, the [Al phase] itself will not coarsen but will be in a fine state. Therefore, in the area where the solidification nucleus is configured, the [Al phase] will not grow to the surface side of the hot-dip galvanized layer, and the exposure ratio of the [Al phase] becomes smaller.

[0100] In this way, the area where the solidification nuclei exist on the surface of the steel plate becomes easy to become the above-mentioned pattern part of the hot-dip coating, and the area where the solidification nuclei do not exist becomes easy to become the non-pattern part of the hot-dip coating. In addition, since the pattern part is formed by the above-mentioned mechanism, there is an element concentration area derived from the solidification nuclei at the interface between the base steel plate and the hot-dip coating of the pattern part. More specifically, there is an element concentration area containing any one or more elements M of Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, Ni, C, Ti, Zr, Mo, W, REM, Hf, and C at the interface between the steel plate and the hot-dip coating of the pattern part.

[0101] In the element concentrated region, the element M is concentrated at least twice as much as the hot-dip coating layer existing in the pattern portion, or the element M is unevenly present. Here, the element M being unevenly present means that the element M originating from the solidification nucleus is present in the element concentrated region, and the element M is not detected in the pattern portion other than the element concentrated region.

[0102] In the process of forming the hot-dip coating, part of the solidification nuclei may diffuse into the hot-dip coating. When such diffusion occurs, the element M constituting the solidification nuclei is also included in the hot-dip coating. In this case, the element M contained in the element-concentrated region has a concentration of more than twice that of the element M contained in the hot-dip coating.

[0103] On the other hand, in the process of forming the hot-dip coating, it is possible that the solidification nuclei hardly diffuse into the hot-dip coating. In this case, the element M constituting the solidification nuclei is not contained in the hot-dip coating, but is contained only in the element-concentrated region. That is, the element-concentrated region becomes a region where the element M is unevenly present with respect to the hot-dip coating of the pattern portion.

[0104] The element M contained in the element-concentrated region is set to have a concentration of more than twice that of the element M contained in the hot-dip coating layer. If the concentration of the element M contained in the element-concentrated region becomes less than twice that of the hot-dip coating layer of the pattern portion, the solidification nucleus function is not fulfilled, and it becomes difficult to form the pattern portion.

[0105] The average concentration of the element M contained in the hot-dip coating and the element-concentrated region of the pattern portion is 0.0010 to 2% by mass. When the average concentration is lower than 0.0010% by mass, the function of the solidification nucleus is not exerted, and it becomes difficult to form the pattern portion. On the other hand, if the average concentration exceeds 2% by mass, although the shape performance of the pattern portion is sufficient, the adhesion between the hot-dip coating and the steel sheet at the pattern portion may be reduced due to the excessive presence of solidification nuclei, and the hot-dip coating at the pattern portion may peel off. Therefore, the average concentration of the element M contained in the hot-dip coating and the element-concentrated region of the pattern portion is preferably in the range of 0.0010 to 2% by mass. The preferred lower limit is 0.1% by mass, and the preferred upper limit is 1.00% by mass.

[0106] On the other hand, since the non-patterned portion is an area where there is no solidification nucleus, the above-mentioned element M is basically absent (i.e., below the detection limit) at the interface between the steel plate and the hot-dip coating in the non-patterned portion, or even if it exists, it is extremely small. Therefore, the concentration of the element M at the interface of the patterned portion, i.e., the concentration of the element M in the element-concentrated region, becomes at least 1.5 times the concentration of the element M at the interface of the non-patterned portion. Preferably, it is 2 times or more, and more preferably 4 times or more. In addition, at the interface between the steel plate and the hot-dip coating in the non-patterned portion, when the element M is below the detection limit, the ratio of the concentration of the element M becomes impossible to calculate.

[0107] In order to confirm the presence and concentration ratio of the above elements at the interface between the steel plate and the hot-dip coating at the patterned portion and the non-patterned portion, it can be confirmed by the following method: the cross section of the hot-dip coated steel plate in the plate thickness direction is exposed, and the interface between the hot-dip coated layer and the steel plate appearing in the cross section is analyzed by an electron beam probe microanalyzer (EPMA) to measure the surface distribution of the elements. In addition, for the presence of the interface alloy layer described later, the presence of the interface alloy layer can also be confirmed by the same method. The thickness of the interface alloy layer can be confirmed by observing the reflected electron image of a scanning electron microscope (SEM).

[0108] As described above, before immersing the steel sheet in the hot-dip coating bath, by arranging solidification nuclei on the surface of the steel sheet in the shape of any one of straight lines, curved lines, graphics, numbers, symbols and letters, or a combination of two or more of them, a pattern portion having these shapes can be formed on the hot-dip coating layer.

[0109] Next, the interface alloy layer is described. In the hot-dip plated steel sheet of the present embodiment, an interface alloy layer exists between the hot-dip plated layer and the steel sheet. The interface alloy layer exists in both the formation area of ​​the pattern portion and the formation area of ​​the non-pattern portion. At the interface between the hot-dip plated layer and the steel sheet at the pattern portion, there is an element-concentrated region and an interface alloy layer. In the hot-dip plated steel sheet of the present embodiment, by also forming an interface alloy layer in the pattern portion having the element-concentrated region, the adhesion of the hot-dip plated layer at the pattern portion becomes equal to the adhesion of the hot-dip plated layer at the non-pattern portion. As a result, there is no risk of peeling off of the pattern portion of the hot-dip plated layer, and the corrosion resistance of the hot-dip plated steel sheet is improved over the entire surface of the hot-dip plated layer.

[0110] The interface alloy layer contains at least Fe and Al. When the hot-dip galvanized layer contains Si, the interface alloy layer contains at least Fe, Si and Al.

[0111] The interface alloy layer is formed on the surface of the base steel plate (specifically, between the base steel plate and the hot-dip coating), and is a layer in which the Al5Fe2 phase is the main phase in terms of organization. Generally speaking, the interface alloy layer is formed by mutual atomic diffusion of the base metal (steel plate) and the plating bath. When the hot-dip coating method is used as the manufacturing method, an interface alloy layer containing Fe and Al is easily formed in the hot-dip coating containing Al. Since Al above a certain concentration is contained in the plating bath, the Al5Fe2 phase is formed the most. However, atomic diffusion takes time, and there is also a part where the Fe concentration becomes high near the base metal. Therefore, the interface alloy layer may also partially contain a small amount of AlFe phase, Al3Fe phase, etc. In addition, since a certain concentration of Zn is also contained in the plating bath, Zn is also contained in a small amount in the Al-Fe alloy phase.

[0112] When Si is contained in the hot-dip coating, it is easy to take in Si in the interface alloy layer, and it is possible to dissolve in the Al-Fe alloy phase or form an Al-Fe-Si intermetallic compound phase. As an example of an Al-Fe-Si intermetallic compound phase, there are α, β, q1, q2 phases, etc. Therefore, these Al-Fe-Si intermetallic compound phases may be detected in the interface alloy layer.

[0113] In the present embodiment, since no solidification nuclei are arranged on the surface of the steel plate in the predetermined area of ​​the non-patterned portion, mutual atomic diffusion of the base metal (parent steel plate) and the plating bath is easy to be performed in the non-patterned portion, and an interface alloy layer is easy to be formed. On the other hand, since solidification nuclei are arranged on the surface of the steel plate in the predetermined area of ​​the patterned portion, mutual atomic diffusion of the base metal (parent steel plate) and the plating bath will not be performed in the patterned portion, and an interface alloy layer will not be formed at all, or even if it is formed, its thickness becomes very thin to the extent that it cannot be detected. Therefore, in the present embodiment, in particular, in order to promote the growth of the interface alloy layer in the patterned portion, it is necessary to perform a reheating treatment after the hot dip plating process.

[0114] The thickness of the interface alloy layer is preferably set to a range of 10 to 500 nm, more preferably 10 to 100 nm, in each of the pattern portion and the non-pattern portion. This can further improve the adhesion between the pattern portion and the non-pattern portion.

[0115] Figure 1 A schematic cross-sectional view of the pattern portion 1 and the non-pattern portion 2 is shown in FIG. In the non-pattern portion 2, an interface alloy layer 5 exists between the steel plate 3 and the coating 4. In the pattern portion 1, an interface alloy layer 5 and a concentrated region 6 exist between the steel plate 3 and the coating 4. It is believed that in the pattern portion 1, the element concentrated region 6 does not dissolve in the interface alloy layer 5 but exists in an independent state. However, since each has a fine structure, it is difficult to distinguish even by cross-sectional analysis such as EPMA. In the element distribution map of the cross section obtained by EPMA, etc., an element distribution image is obtained as if the interface alloy layer 5 and the concentrated region 6 exist in the same part.

[0116] The hot-dip plated steel sheet of this embodiment may also have a chemical conversion coating layer or a coating layer on the surface of the hot-dip plated layer. Here, the types of the chemical conversion coating layer or the coating layer are not particularly limited, and known chemical conversion coating layers or coating layers may be used.

[0117] As an example of a chemical conversion coating, a chemical conversion coating containing a phthalocyanine pigment coated with at least one of a resin and a surfactant can be exemplified. The hot-dip coating provided with such a chemical conversion coating can be colored with a phthalocyanine pigment to impart a preferred pattern design to the coating surface, and the visual recognition of the pattern portion is further improved. Furthermore, the corrosion resistance and weather resistance of the chemical conversion coating can be improved.

[0118] Next, a method for producing the Zn—Al—Mg based hot dip coated steel sheet according to the present embodiment will be described.

[0119] First, a hot-rolled steel sheet is manufactured, and the hot-rolled sheet is annealed as needed. After pickling, the sheet is cold-rolled to form a cold-rolled sheet. The cold-rolled sheet is degreased and washed with water, and then annealed (cold-rolled sheet annealing). The annealed cold-rolled sheet is immersed in a hot-dip coating bath to form a hot-dip coating layer.

[0120] Here, during the period from cold rolling to immersion in a hot dip coating bath, solidification nuclei are attached to the surface of the steel sheet to form a pattern portion in the shape of a straight line portion, a curved line portion, a figure, a number, a symbol, and a character, or a combination of two or more of them. The attachment of solidification nuclei is carried out at any stage between cold rolling and cold rolled sheet annealing, between cold rolled sheet annealing and immersion in a hot dip coating bath, or immediately before the final annealing of cold rolled sheet annealing. The solidification nuclei can be attached in a solution dispersed state or by evaporation.

[0121] As a component that forms a solidification nucleus (hereinafter, sometimes referred to as a solidification nucleus forming component), it is not particularly limited as long as it is a component that forms a solidification nucleus during the solidification process of the coating. As a solidification nucleus forming component, for example, any one or more of Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, Ni, Ti, Zr, Mo, W, REM, Hf, C, or a compound containing any one or more of the above elements, etc. can be listed. The above components can also be used in combination of one or more. As an example of a method for attaching a solidification nucleus to the surface of a steel plate, the following method can be listed: in addition to containing the solidification nucleus forming component itself, an alloy foil or resin, a surfactant, ink, an oil, etc. contains a solidification nucleus forming component and is attached to the surface of the steel plate. These solidification nucleus forming components can be solids themselves, or they can be dissolved or dispersed in water or an organic solvent. Alternatively, they can also be included in the ink as a pigment or dye.

[0122] As a method for attaching the solidification nuclei to the surface of the steel plate, for example, there can be exemplified methods such as transferring, coating, and blowing a material containing a solidification nucleus-forming component onto the surface of the steel plate. For example, a general printing method such as a foil transfer method using hot stamping or cold stamping, a printing method using various plates (gravure printing, flexographic printing, offset printing, screen printing, etc.), an inkjet method, and a thermal transfer method using an ink ribbon can be used.

[0123] As an example of the transfer method using alloy foil, there is a method in which alloy foil containing a solidification nucleus forming component is bonded to the surface of a steel sheet and a heated silicon roller is pressed against the alloy foil to transfer the alloy foil to the surface of the steel sheet.

[0124] As an example of a printing method using a plate, there is a method in which ink or a surfactant containing a component that becomes a solidification nucleus is attached to a rubber roller or a rubber stamp having a printed pattern formed on the circumference, and the rubber roller or the rubber stamp is pressed against the surface of a steel plate to transfer the ink or the surfactant. According to this method, for a steel plate that is continuously passed through, the solidification nucleus-forming component can be efficiently attached to the surface of the steel plate.

[0125] The amount of coagulation nuclei deposited is preferably 50 mg / m 2 ~5000mg / m 2 When the adhesion is less than 50mg / m 2 In the case of an adhesion amount exceeding 5000 mg / m 2 In the case of , there is a possibility that the adhesion of the hot-dip coating layer will decrease, which is not preferred.

[0126] Next, the steel sheet having the patterned portion formed on the surface is immersed in a hot dip coating bath. The hot dip coating bath preferably contains 4 to 22 mass % of Al, 1.0 to 10 mass % of Mg, and the remainder contains Zn and impurities. In addition, the hot dip coating bath may also contain 0.0001 to 2.0 mass % of Si. Furthermore, the hot dip coating bath may also contain any one or more of Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C in a total amount of 0.0001 to 1 mass %.

[0127] It should be noted that the composition of the hot-dip galvanized layer can be measured by the following method. It can be obtained by first removing the surface coating with a coating stripper that does not corrode the coating (e.g., NEOREVER SP-751 manufactured by Sancai Chemical Industry Co., Ltd.), dissolving the hot-dip galvanized layer with hydrochloric acid to which an inhibitor (e.g., HIBIRON manufactured by SUGIMURA Chemical Industrial Co., Ltd.) is added, and the resulting solution is subjected to inductively coupled plasma (ICP) emission spectrometry.

[0128] The temperature of the hot-dip coating bath is preferably in the range of 400 to 500° C. This is because a desired hot-dip coating layer can be formed when the temperature of the hot-dip coating bath is in this range.

[0129] The amount of hot-dip coating can be adjusted by gas wiping or other means on the steel sheet taken out of the hot-dip coating bath. The amount of hot-dip coating is preferably adjusted to a total of 30 to 600 g / m2 on both sides of the steel sheet. 2 When the adhesion is less than 30g / m2 In the case of Zn-Al-Mg hot-dip plated steel sheet, the corrosion resistance is reduced, which is not preferred. 2 In the case of , the molten metal attached to the steel sheet will drip, making it impossible to smooth the surface of the hot-dip coating, which is not preferred.

[0130] After adjusting the adhesion amount of the hot-dip coating, a reheating treatment is performed, and then the steel plate is cooled. The reheating treatment is performed under the condition that the interface alloy layer of the pattern part becomes more than 10nm and the interface alloy layer of the non-pattern part becomes less than 500nm. Although the specific reheating treatment conditions vary depending on the coating composition, for example, it is appropriate to stay in the temperature range of (Tw+15)℃ to (Tw+50)℃ for 1 to 10 seconds relative to the surface temperature Tw of the coating in the molten state just after wiping. The cooling conditions after the reheating treatment are preferably set to a cooling rate of more than 3℃ / second and less than 30℃ / second, preferably at a cooling rate of 3 to 25℃ / second to a range of 300 to 340℃. It should be noted that if the reheating temperature is too low or the reheating time is short, an interface alloy layer of sufficient thickness cannot be formed in the pattern part, and the adhesion of the hot-dip coating at the pattern part will not be improved. If the reheating temperature is too high or the reheating time is too long, diffusion of Fe into the hot-dip plating layer in the pattern portion becomes excessive, and alloying of the hot-dip plating layer proceeds, making it difficult to realize the pattern design by the pattern portion.

[0131] The cooling of the molten metal attached to the steel plate begins after the steel plate is taken out of the hot-dip coating bath. Although it also varies depending on the composition of the hot-dip coating bath, for example, [Al phase] begins to crystallize at around 430°C. Then, [MgZn2] begins to crystallize at around 370°C, and [ternary eutectic structure of Al / Zn / MgZn2] crystallizes at around 340°C, completing solidification.

[0132] At this time, in the area where the solidification nuclei are attached to the surface of the steel plate, the [Al phase] begins to crystallize with the solidification nuclei as the nuclei, and the [Al phase] crystallizes in large quantities near the interface between the steel plate and the molten metal. Since the [Al phase] is generated at a relatively high density by the solidification nuclei, the [Al phase] itself does not coarsen but is in a fine state. Therefore, the [Al phase] does not grow to the surface side of the hot-dip galvanizing layer, and the exposure ratio of the [Al phase] becomes relatively small. It is speculated that: in this way, the area where the solidification nuclei exist on the surface of the steel plate becomes the pattern part of the hot-dip galvanizing layer.

[0133] On the other hand, in the area where no solidification nuclei are attached to the surface of the steel plate, the [Al phase] crystallizes in the entire thickness direction of the molten metal. That is, since the crystal density of the [Al phase] is relatively low, the crystallization of the [Al phase] is not hindered. As a result, the [Al phase] coarsens. Therefore, the [Al phase] grows to the surface side of the hot-dip galvanizing layer, so the exposure ratio of the [Al phase] at the surface of the hot-dip galvanizing layer becomes relatively large.

[0134] It is presumed that, by such a mechanism, a region where no solidification nuclei exist on the surface of the steel sheet becomes a non-pattern portion of the hot-dip galvanizing layer.

[0135] When a chemical conversion treatment layer is formed on the surface of the hot-dip coating layer, the hot-dip coated steel sheet after the hot-dip coating layer is formed is subjected to a chemical conversion treatment. The type of chemical conversion treatment is not particularly limited, and a known chemical conversion treatment can be used.

[0136] When a coating layer is formed on the surface of the hot-dip coating layer or the surface of the chemical conversion treatment layer, the hot-dip coated steel sheet after the hot-dip coating layer or the chemical conversion treatment layer is subjected to a coating treatment. The type of coating treatment is not particularly limited, and a known coating treatment can be used.

[0137] As an example of chemical conversion treatment, a chemical conversion treatment using a chemical conversion treatment agent containing a phthalocyanine pigment coated with at least one of a resin and a surfactant can be exemplified. As a chemical conversion treatment agent, specifically, the following aqueous coating agent can be used: polyurethane resin particles and ethylene-unsaturated carboxylic acid copolymer resin particles containing at least one of a silanol group and an alkoxysilyl group, silicon oxide particles, an organic titanium compound and the above-mentioned phthalocyanine pigment, the content of the phthalocyanine pigment relative to the total of 100 parts by mass of the polyurethane resin particles and the ethylene-unsaturated carboxylic acid copolymer resin particles, and the primary particle size of the phthalocyanine pigment is 0.01 to 1.0 μm. The hot-dip coating subjected to such chemical conversion treatment can impart a preferred pattern design to the coating surface by coloring with the phthalocyanine pigment, and further, the corrosion resistance and weather resistance of the formed chemical conversion treatment coating can be improved.

[0138] According to the present embodiment, it is possible to provide a hot-dip plated steel sheet having excellent corrosion resistance, high durability of a pattern portion showing characters or designs, and excellent adhesion of the hot-dip plated layer in the pattern portion.

[0139] In particular, in the present embodiment, by attaching solidified nuclei to the surface of the steel sheet in a manner that forms an arbitrary pattern, the range of the pattern portion can be intentionally determined, and the pattern portion can be configured in a manner that forms a shape that forms any one of a straight line portion, a curved line portion, a figure, a number, a symbol, and a character, or a combination of two or more of them. Thus, various pattern designs can be implemented on the surface of the hot-dip coating layer without coating or grinding, and the recognition and design of the steel sheet can be improved. In addition, by forming an interface alloy layer at the pattern portion together with the element-concentrated region, the adhesion of the hot-dip coating of the pattern portion can be improved to the same degree as the adhesion of the hot-dip coating of the non-pattern portion.

[0140] In addition, according to this embodiment, various patterns, trademarks, and other identification marks can be expressed on the surface of the hot-dip plated layer without printing or painting, which can improve the identification and design of the origin of the steel plate. In addition, the pattern portion can also be used to provide the hot-dip plated steel plate with information required for process management or inventory management, or any information required by the customer. This can also help improve the productivity of the hot-dip plated steel plate.

[0141] Example

[0142] Next, examples of the present invention will be described.

[0143] (No.1~71)

[0144] First, the cold-rolled steel sheet is degreased and washed with water. The ink containing the solidification nucleus forming component shown in Table 1 is attached to a rubber plate having a shape with a checkerboard pattern with a spacing of 50 mm transferred thereto. Here, the checkerboard pattern is formed in a linear shape, and the line width is set to 10 mm. By pressing the rubber plate against the washed steel sheet, the ink containing the solidification nucleus forming component is attached to the surface of the steel sheet in a checkerboard shape with a spacing of 50 mm. Thereafter, the steel sheet is subjected to cold-rolled sheet annealing. The steel sheet after cold-rolled sheet annealing is immersed in a hot-dip plating bath at 400 to 500°C to form a hot-dip plating layer on the surface of the steel sheet. Thereafter, the adhesion amount is controlled by a wiping nozzle, and a reheating treatment is performed, and further cooling is performed. For the reheating treatment, the wiped steel sheet is heated to the reheating temperature described in Tables 2A and 2B, retained at this temperature, and cooled to a range of 300 to 340°C at the average cooling rate described in Tables 2A and 2B. Thus, Zn—Al—Mg-based hot-dip plated steel sheets Nos. 1 to 71 shown in Tables 3A to 4B were produced.

[0145] (No.72)

[0146] A Zn-Al-Mg hot-dip plated steel sheet was produced in the same manner as above except that the coating amount was controlled by the wiping nozzle and then cooled without reheating. The results are shown as No. 72 in Tables 3B and 4B.

[0147] (No.73)

[0148] A Zn-Al-Mg hot-dip plated steel sheet was produced in the same manner as above except that the transfer of ink using the rubber plate was not performed. Then, a checkerboard pattern with a spacing of 50 mm was printed on the surface of the hot-dip plated layer by an inkjet method. The result is shown as No. 73 in Tables 3B and 4B.

[0149] (No.74)

[0150] A Zn-Al-Mg hot-dip plated steel sheet was produced in the same manner as above except that the transfer of the ink using the rubber plate was not performed. Thereafter, the surface of the hot-dip plated layer was ground to form a checkerboard pattern with a spacing of 50 mm. The result is shown as No. 74 in Tables 3B and 4B.

[0151] [Evaluation method of exposure ratio of [Al phase]]

[0152] The surface of the hot-dip galvanized layer was photographed using a 100x scanning electron microscope, and the element distribution was measured using an energy dispersive X-ray element analyzer (EDS) attached to the scanning electron microscope. Five images of the 1 mm2 area of ​​the pattern were prepared. 2 Field of view images, 5 images of the non-patterned area 1mm 2 Image of the viewing field. For each image, commercially available image analysis software is used to measure the area of ​​the [Al phase] exposed to the surface of the hot-dip galvanized layer. The [Al phase] is obtained by combining the Al-concentrated area in the surface analysis with the morphological observation of the [Al phase] using the reflected electron image. In each of the patterned portion and the non-patterned portion, the average value of the exposed area of ​​the [Al phase] in the 5 images is obtained. Then, by dividing the average value of the exposed area of ​​the [Al phase] by the total area of ​​the observed field of view, the average exposed area ratio (%) of the [Al phase] in the observed field of view is obtained in the patterned portion and the non-patterned portion, respectively. The average exposed area ratio (%) of the [Al phase] obtained in this way is used as the exposure ratio of the [Al phase].

[0153] [Method for measuring arithmetic mean surface roughness Sa]

[0154] On the surface of the hot-dip galvanized layer, imaginary grid lines are drawn at intervals of 0.5 mm, and in the multiple areas divided by the imaginary grid lines, the arithmetic mean surface roughness Sa of each area is measured. The area with an arithmetic mean surface roughness Sa of 1 μm or more becomes a non-pattern part, and the area with an arithmetic mean surface roughness Sa of less than 1 μm becomes a pattern part. The measurement of the arithmetic mean surface roughness Sa is performed using a 3D laser microscope (manufactured by KEYENCE Co., Ltd.). In this embodiment, a 20x standard lens is used, and in the multiple areas divided by the imaginary grid lines, the height Z within the area is measured at a measurement interval of 50 μm. When the measurement is performed on the grid, 100 measurement points are obtained in the area. The obtained height Z100 points are set as height Z1 to height Z 100 When Z is , Sa is calculated using the following formula. ave Set to the average of the height Z100 points.

[0155] Sa=1 / 100×Σ[x=1→100](|height Z x -Z ave |)

[0156] It should be noted that the location for measuring the arithmetic mean surface roughness Sa is set to a location different from the location for measuring the exposure ratio of the Al phase. This is also set similarly for both the pattern portion and the non-pattern portion.

[0157] [Element-concentrated region and interface alloy layer]

[0158] The cross section of the hot-dip plated steel sheet in the thickness direction was exposed, and the interface between the hot-dip plated layer and the steel sheet in the cross section was subjected to surface analysis for element distribution by an electron probe microanalyzer (EPMA), and the element concentration region and the interface alloy layer were confirmed. At the same time, the concentration and concentration ratio of the element M were measured. The thickness of the interface alloy layer was measured by a reflected electron image of a scanning electron microscope (SEM).

[0159] [Pattern design]

[0160] For the test plates of the embodiments and comparative examples, whether the checkerboard pattern can be visually recognized is evaluated based on the following criteria. The evaluation is performed on the test plates immediately after manufacture and after 6 months of outdoor exposure. A or B is set as acceptable for both the initial state and the timed state. If at least one of the initial state or the timed state is C, it is set as unacceptable.

[0161] A: The checkerboard can be visually identified from 5m ahead.

[0162] B: The checkerboard cannot be visually recognized from 5m ahead, but it is highly visible from 2m ahead.

[0163] C: The checkerboard cannot be visually discerned from 2 m ahead.

[0164] [Corrosion resistance]

[0165] The test plate cut into 150×70 mm was subjected to 30 cycles of the accelerated corrosion test CCT according to JASO-M609. Thereafter, the corrosion resistance was evaluated as follows based on the rusting condition. A or B was regarded as passing.

[0166] A: No rust, maintain beautiful pattern appearance.

[0167] B: The design appearance is slightly damaged due to rust.

[0168] C: The appearance quality is significantly degraded due to rust.

[0169] [Plating Adhesion]

[0170] The test plate cut into 150×70 mm was subjected to 2T bending at the portion where the grid pattern was formed, and the plating adhesion was evaluated based on the following criteria: A or B was regarded as acceptable.

[0171] A: The plating layer does not come off even when the tape is peeled off. B: The plating layer comes off when the tape is peeled off, but does not come off when the tape is not peeled off. C: The plating layer comes off even when the tape is not peeled off.

[0172] As shown in Table 2A to Table 4B, the manufacturing conditions of No. 1 to 61 meet the preferred conditions, the average composition of the hot-dip coating meets the scope of the invention, a pattern portion and a non-pattern portion are formed in the hot-dip coating, and an element-concentrated region containing element M and an interface alloy layer containing Fe and Al exist at the interface between the base steel plate and the hot-dip coating at the pattern portion. The average concentration of element M contained in the hot-dip coating and the element-concentrated region is 0.0010 to 2% by mass. In the element-concentrated region, element M is concentrated more than twice as much as the hot-dip coating present in the pattern portion, or element M exists unevenly. As a result, No. 1 to 61 are excellent in pattern design, corrosion resistance, and plating adhesion. In addition, Fe and Al are contained in the interface alloy layer of the pattern portion and the non-pattern portion of No. 1 to 61. In addition, when Si is contained in the coating, Fe, Al, and Si are contained in the interface alloy layer of the pattern portion and the non-pattern portion.

[0173] The Al content in the average composition of the hot-dip plating layer of No. 62 was insufficient. Therefore, the corrosion resistance of the hot-dip plating layer was insufficient.

[0174] In No. 63, the Al content in the average composition of the hot-dip coating was excessive, and therefore, the corrosion resistance of the hot-dip coating was insufficient.

[0175] The Mg content in the average composition of the hot-dip plating layer of No. 64 was insufficient. Therefore, the corrosion resistance of the hot-dip plating layer became insufficient.

[0176] The Mg content in the average composition of the hot-dip coating of No. 65 was excessive, so dross was generated in the coating bath and the corrosion resistance of the hot-dip coating was insufficient.

[0177] In No. 66, since the residence time in the reheating treatment exceeded the preferred upper limit, diffusion of the M element added as a solidification nucleus occurred inside the coating layer, and homogenization of the coating layer progressed, resulting in a decrease in pattern design properties.

[0178] In No. 67, since the heating temperature in the reheating treatment was lower than the preferred lower limit, an interface alloy layer was not formed in the pattern portion, and the adhesion was reduced.

[0179] In No. 68, since the residence time in the reheating treatment was less than the preferred lower limit, an interface alloy layer was not formed in the pattern portion, and the adhesion was reduced.

[0180] In No. 69, since the heating time in the reheating treatment exceeded the preferred upper limit, diffusion of the M element added as a solidification nucleus occurred inside the coating layer, and the adhesion was reduced.

[0181] In No. 70, since the average cooling rate in the reheating treatment was lower than the preferred lower limit, diffusion of the M element added as a solidification nucleus occurred inside the coating layer, and homogenization of the coating layer progressed, resulting in a decrease in pattern design properties.

[0182] In No. 71, since the average cooling rate in the reheating treatment exceeded the preferred upper limit, the surface of the plated layer was roughened by the blowing of the cooling gas during cooling, and the pattern design properties were deteriorated.

[0183] In No. 72, since the reheating treatment was not performed, no interface alloy layer was formed in the pattern portion, and the adhesion was reduced.

[0184] In No. 73, since the pattern portion was formed by printing, the pattern design was degraded over time.

[0185] In No. 74, since the pattern portion was formed by grinding, the plating thickness at the pattern portion was reduced, and the corrosion resistance was reduced.

[0186] [Table 1]

[0187]

[0188] [Table 2A]

[0189]

[0190] [Table 2B]

[0191]

[0192] The underlined portion indicates that the conditions are outside the range of the preferred production conditions.

[0193] [Table 3A]

[0194]

[0195] [Table 3B]

[0196]

[0197] The underlined part indicates that it is outside the scope of the present invention.

[0198] [Table 4A]

[0199]

[0200] (*1) Average concentration of the element M contained in the hot-dip plating layer and the element-concentrated region of the pattern portion.

[0201] (*2) The concentration ratio of the element M with respect to the hot-dip plating layer of the pattern portion.

[0202] (*3) The concentration ratio of the element group M at the interface of the pattern portion to the element group M at the interface of the non-pattern portion.

[0203] [Table 4B]

[0204]

[0205] The underlined part indicates that it is outside the scope of the present invention.

[0206] (*1) Average concentration of the element M contained in the hot-dip plating layer and the element-concentrated region of the pattern portion.

[0207] (*2) The concentration ratio of the element M with respect to the hot-dip plating layer of the pattern portion.

[0208] (*3) The concentration ratio of the element group M at the interface of the pattern portion to the element group M at the interface of the non-pattern portion.

[0209] Furthermore, a chemical conversion film was formed on the surface of the hot-dip galvanized steel sheets No. 57 to 59, and the pattern design was confirmed. The chemical conversion film was formed by chemical conversion treatment using a chemical conversion agent containing a phthalocyanine pigment. As the chemical conversion agent, the following aqueous coating agent was used: polyurethane resin particles and ethylene-unsaturated carboxylic acid copolymer resin particles having a silanol group and an alkoxysilyl group, silicon oxide particles, an organic titanium compound and Cu phthalocyanine, the content of the Cu phthalocyanine pigment was 0.01 to 10 parts by mass relative to 100 parts by mass of the total of the polyurethane resin particles and the ethylene-unsaturated carboxylic acid copolymer resin particles, and the primary particle size of the Cu phthalocyanine was 0.01 to 1.0 μm.

[0210] The pattern designability of the hot-dip plated steel sheets No. 57 to 59 formed with a chemical conversion treatment film was evaluated. The results showed that the evaluation was A for both the hot-dip plated steel sheets immediately after manufacture and after 6 months of outdoor exposure. The pattern designability was further improved by providing a chemical conversion treatment film containing Cu phthalocyanine.

[0211] Explanation of symbols

[0212] 1 pattern part, 2 non-pattern part, 3 steel plate, 4 hot-dip coating layer, 5 interface alloy layer, 6 element concentrated area.

Claims

1. A hot-dip plated steel sheet comprising a steel sheet and a hot-dip plated layer formed on a surface of the steel sheet, The hot-dip coating layer contains, as an average composition, 4 to 22 mass % of Al, 1.0 to 10 mass % of Mg, and the remainder contains Zn and impurities. The hot-dip plated layer has a pattern portion and a non-pattern portion, At the interface between the steel sheet and the hot-dip galvanized layer at the pattern portion, there are: an element-concentrated region containing any one or more elements M selected from Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, Ni, Ti, Zr, Mo, W, REM, Hf, and C; and an interface alloy layer containing Fe and Al, The average concentration of the element M contained in the hot-dip plating layer of the pattern portion and the element-concentrated region is 0.0010 to 2% by mass. In the element concentrated region, the element M is concentrated at least twice as much as the hot-dip plating layer present in the pattern portion, or the element M is unevenly present. 2 . The hot-dip plated steel sheet according to claim 1 , further comprising an interface alloy layer containing Fe and Al at an interface between the steel sheet and the hot-dip plated layer in the non-pattern portion.

3. The hot-dip coated steel sheet according to claim 1 or claim 2, wherein: The concentration of the element M at the interface of the pattern portion is 1.5 times or more the concentration of the element M at the interface of the non-pattern portion.

4. The hot-dip coated steel sheet according to claim 1, characterized in that: The pattern portion is arranged so as to have any one of a straight line portion, a curved line portion, a dot portion, a figure, a number, a symbol, or a character, or a shape formed by combining two or more of them.

5. The hot-dip coated steel sheet according to claim 1, characterized in that: The hot-dip coating layer further contains Si: 0.0001 to 2 mass % in terms of average composition. 6 . The hot-dip plated steel sheet according to claim 5 , further comprising Si in the interface alloy layer formed in the pattern portion. 7 . The hot-dip plated steel sheet according to claim 5 , further comprising Si in the interface alloy layer formed in the non-pattern portion.

8. The hot-dip plated steel sheet according to any one of claims 1, 2, 4, 5, 6 and 7, characterized in that: The hot-dip galvanized layer excluding the element-concentrated region further contains any one or more of Ni, Ti, Zr, Sr, Fe, Sb, Pb, Sn, Ca, Co, Mn, P, B, Bi, Cr, Sc, Y, REM, Hf, and C in an average composition of 0.0001 to 1 mass % in total.

9. The hot-dip coated steel sheet according to claim 1, characterized in that: The total amount of hot-dip coating on both sides of the steel plate is 30 to 600 g / m 2 .

Citation Information

Patent Citations

  • Alloyed hot-dip galvanized steel sheet having excellent formability and post-adhesion detachment resistance, and manufacturing method therefor

    CN102666903A

  • Zn-Al-Mg-BASED HOT-DIP PLATED STEEL SHEET AND METHOD FOR PRODUCING SAME

    CN112166206A

  • Plated steel, flux, and manufacturing method of plated steel

    JP2017008387A

  • Plated steel material

    WO2022085386A1