Negative photosensitive resin composition, dry film, cured product, and electronic component

By optimizing the combination of polyhydroxy amide compounds, oxime sulfonate compounds and crosslinking agents, negative photosensitive resin compositions with higher resolution and insulation reliability are prepared, and resolution and insulation reliability in the prior art are solved. The problem of insufficient performance has achieved higher integrated circuit pattern formation and better insulation performance.

CN119032325APending Publication Date: 2024-11-26TAIYO HOLDINGS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380031054.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-30
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The conventional negative-type photosensitive resin composition has shortcomings in resolution and insulation reliability, making it difficult to achieve sufficiently high-integrated circuit formation, and the insulation reliability evaluation is insufficient.

Method used

By combining the polyhydroxy amide compound with an oxime sulfonate compound and a crosslinking agent, a specific negative photosensitive resin composition is prepared, including phenolic hydroxyl groups and basic compounds, and the structure and proportion of the crosslinking agent are optimized to improve the structure and proportion of the crosslinking agent to improve the Resolution and insulation reliability.

Benefits of technology

The pattern formation of line width/line distance is less than 1.0μm/1.0μm, the aspect ratio reaches more than 3.5, and the insulation reliability is significantly improved, ensuring high resolution and reliability of electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032325A_ABST
    Figure CN119032325A_ABST
Patent Text Reader

Abstract

Provided is a novel negative-type photosensitive resin composition having more excellent resolution and insulation reliability. The negative photosensitive resin composition is characterized by containing (A) a polyhydroxy amide compound containing a structural unit represented by formula (1), (B) an oxime sulfonic acid ester compound, and (C) a cross-linking agent, the weight-average molecular weight of the polyhydroxy amide compound (A) being 2000-20000, the polyhydroxy amide compound (A) not containing a carboxyl group or having a carboxyl group equivalent of 1500 g / eq or more, and the cross-linking agent (C) being a polyhydroxy amide compound having a weight-average molecular weight of 2000-20000. The crosslinking agent (C) contains a plurality of methoxymethyl groups and / or hydroxymethyl groups. (In formula (1), R1 is a divalent organic group, and R2 is a tetravalent organic group. ). # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a negative photosensitive resin composition, a dry film, a cured product and an electronic component. Background Art

[0002] A photosensitive resin composition containing a polyimide precursor exhibits excellent properties such as insulation, heat resistance, and mechanical strength, and therefore is widely used as an insulating film in various fields such as semiconductors and electronic components.

[0003] In the past, with the demand for higher performance and smaller size of electronic components and electrical equipment, semiconductor elements have been required to be highly integrated. In recent years, in order to meet these demands, high performance and smaller size technologies have been developed in the field of semiconductor element packaging such as wafer-level packaging, and the demand for finer pattern formation (resolution) in the insulating film used in the wiring layer has increased.

[0004] Patent Document 1 discloses the use of a negative photosensitive resin composition, which contains: a specific polyamide derivative that is a photosensitive polybenzoxazole precursor, a compound that generates an acid when irradiated with radiation, and a compound that can crosslink the specific polyamide derivative. According to the disclosure of Patent Document 1, an electronic component with excellent sensitivity, resolution and heat resistance, a good shape pattern, and high reliability is provided.

[0005] Patent document 2 discloses that pattern formation with excellent sensitivity and resolution can be performed by using a negative photosensitive resin composition, wherein the negative photosensitive resin composition contains: a polymer component formed by two or more different heat-resistant polymers having reactive terminal groups; a compound that generates an acid when irradiated with active light; and a compound that can be cross-linked or polymerized by the action of the acid.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2001-125267

[0009] Patent Document 2: Japanese Patent Application Publication No. 2008-033159 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] If the negative photosensitive resin composition of Patent Document 1 is used, pattern formation with a resolution of 5 to 8 μm can be achieved, and if the negative photosensitive resin composition of Patent Document 2 is used, pattern formation with a resolution of 5 to 6 μm can be achieved. However, there is a concern that sufficiently highly integrated circuit formation cannot be achieved at the level of resolution when these negative photosensitive resin compositions are used. In addition, insulation reliability is not evaluated in any of the patent documents, and there is a concern that sufficient insulation reliability cannot be obtained.

[0012] Therefore, the object of the present disclosure is to provide a new negative photosensitive resin composition having better resolution and higher insulation reliability. In addition, another object of the present disclosure is to provide a cured product using the negative photosensitive resin composition, and electronic components such as printed circuit boards and semiconductor elements using the same.

[0013] Solutions for solving problems

[0014] The present inventors have found that the above-mentioned problems can be solved by combining a specific polyhydroxyamide compound, a specific oxime sulfonate compound, and a specific crosslinking agent, and have completed the present invention.

[0015] That is, according to one embodiment of the disclosed technology, there can be provided a negative photosensitive resin composition, characterized in that it contains:

[0016] (A) a polyhydroxyamide compound comprising a structural unit represented by the following formula (1);

[0017] (B) an oxime sulfonate compound; and

[0018] (C) a cross-linking agent,

[0019] The weight average molecular weight of the polyhydroxyamide compound (A) is 2,000 to 20,000.

[0020] The aforementioned (A) polyhydroxyamide compound does not contain a carboxyl group or has a carboxyl group equivalent of 1500 g / eq or more,

[0021] The aforementioned (C) cross-linking agent contains a plurality of methoxymethyl groups and / or hydroxymethyl groups.

[0022]

[0023] (In formula (1), R 1 is a divalent organic group, R 2 is a tetravalent organic group.)

[0024] The (A) polyhydroxyamide compound preferably has a carboxyl group or a phenolic hydroxyl group at a terminal.

[0025] The (B) oxime sulfonate compound preferably has a structure represented by the following formula (2).

[0026]

[0027] (In formula (2), X is a hydrocarbon group or a halogen atom, m is an integer from 0 to 3, and R 3 is a hydrogen atom, a hydrocarbon group, an organic group containing a keto group, or a halogen atom. )

[0028] It is preferred that the cross-linking agent (C) contains a heterocyclic ring.

[0029] The (C) cross-linking agent is preferably a compound having a triazine ring.

[0030] It is preferred that the negative photosensitive resin composition contains (D) a compound containing a phenolic hydroxyl group.

[0031] The (D) compound containing a phenolic hydroxyl group preferably contains a polyhydroxystyrene polymer or a polyhydroxystyrene copolymer.

[0032] It is preferred that the negative photosensitive resin composition contains (E) a basic compound.

[0033] According to another aspect of the present disclosure, there is provided a dry film characterized by comprising a resin layer formed from the negative photosensitive resin composition.

[0034] According to another embodiment of the present disclosure, there is provided a cured product characterized in that it is formed from the negative photosensitive resin composition or from the resin layer of the dry film.

[0035] According to another aspect of the present disclosure, there can be provided an electronic component characterized by comprising the above-mentioned cured product.

[0036] Effects of the Invention

[0037] According to the disclosed technology, a new negative photosensitive resin composition having more excellent resolution and higher insulation reliability can be provided. DETAILED DESCRIPTION

[0038] Hereinafter, embodiments of the disclosed technology will be described in detail. It should be noted that in the present specification, the expression "a to b" in the description of the numerical range means a or more and b or less unless otherwise specified.

[0039] 1. Negative photosensitive resin composition

[0040] The negative photosensitive resin composition disclosed in the present invention contains: a specific (A) polyhydroxyamide compound, a specific (B) oxime sulfonate compound and a specific (C) crosslinking agent as shown below. The negative photosensitive resin composition disclosed in the present invention has a high resolution, and therefore, can form a fine pattern, and its cured product has excellent insulation reliability. Specifically, the negative photosensitive resin composition disclosed in the present invention can make the line width / line spacing (L / S) in the pattern of the semiconductor circuit or circuit substrate lower than 2μm / 2μm, and can be made below 1.5μm / 1.5μm, and further below 1.0μm / 1.0μm. In addition, the aspect ratio (line height / line width) can be made greater than 2.0, and can also be made greater than 3.0, and further greater than 3.5. In addition, through holes with an opening diameter of less than 2.0μm can also be formed.

[0041] 1-1. (A) Polyhydroxyamide compounds

[0042] (A) The polyhydroxyamide compound contains a structural unit represented by the following formula (1).

[0043]

[0044] (In formula (1), R 1 is a divalent organic group, R 2 is a tetravalent organic group.)

[0045] R in formula (1) 1 There are no particular limitations on the divalent organic group as long as it is a divalent organic group, and examples thereof include alkylene groups, cycloalkylene groups, arylene groups, alkyl ether groups, ketone groups, and ester groups. Of these, divalent aromatic hydrocarbon groups having a skeleton of benzene, naphthalene, perylene, biphenyl, diphenyl ether, diphenyl sulfone, diphenyl propane, diphenyl hexafluoropropane, benzophenone, or the like, or divalent aliphatic hydrocarbon groups having a skeleton of butane, cyclobutane, or the like are preferred. From the viewpoint of the resolution of the negative photosensitive resin composition and the insulation reliability of the cured product, R 1 The carbon number of is preferably 4 to 30, and phenyl, biphenyl, diphenyl ether, and diphenylhexafluoropropane are preferred. 1 Two or more of the groups exemplified above.

[0046] R in formula (1) 2 The organic group is not particularly limited as long as it is a tetravalent organic group, but is preferably a tetravalent aromatic hydrocarbon group having a skeleton such as diphenyl, diphenyl ether, diphenyl sulfide, benzophenone, diphenylmethane, diphenylpropane, diphenylhexafluoropropane, diphenyl sulfoxide, diphenyl sulfone, biphenyl, or benzene, and more preferably an organic group having a structure represented by the following formula (3).

[0047]

[0048] (In formula (3), a is an integer from 0 to 3, and * represents a bond)

[0049] The terminal structure of the polyhydroxyamide compound (A) is not particularly limited, and examples thereof include terminal structures having a functional group such as an amino group, an alcoholic hydroxyl group, a phenolic hydroxyl group, an acid anhydride group, a carboxyl group, and an isocyanate group. From the viewpoint of solubility in a developer, a terminal structure having a carboxyl group or a phenolic hydroxyl group is preferred.

[0050] Among these terminal structures, it is particularly preferred to have a phenolic hydroxyl group. When the terminal of the polyhydroxyamide compound has a phenolic hydroxyl group, the solubility of the polyhydroxyamide compound in the developer can be improved. Furthermore, since the phenolic hydroxyl group is less reactive than the carboxyl group, excessive reaction with the crosslinking agent is suppressed, and even when the PEB process is performed, the resolution can be maintained, so it is estimated that a negative photosensitive resin composition that can form a finer L / S pattern with a high aspect ratio can be provided.

[0051] In addition, these terminal structures may have the above-mentioned terminal structure as a terminal structure in which the molecular chain terminal of the polyhydroxyamide compound is blocked with a terminal blocking agent.

[0052] The weight average molecular weight (Mw) of the (A) polyhydroxyamide compound is 2000 to 20000, preferably 2000 to 15000, more preferably 3000 to 15000, particularly preferably 4000 to 10000. By setting it as such a range, a finer L / S pattern with a high aspect ratio can be formed.

[0053] The number average molecular weight (Mn) of the (A) polyhydroxyamide compound is preferably 1,000 to 10,000, more preferably 1,500 to 6,000.

[0054] The molecular weight distribution index (PDI) of the (A) polyhydroxyamide compound is preferably 1.5 to 4.0, more preferably 1.5 to 3.5.

[0055] When the weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight dispersion (PDI) of the polyhydroxyamide compound (A) are within the above ranges, the solubility in the developer in the unexposed portion and the reaction with the crosslinking agent (C) during exposure are suitably balanced, and a negative photosensitive resin composition with better resolution can be obtained.

[0056] In this specification, the weight average molecular weight and number average molecular weight are measured by gel chromatography (GPC) (GL7700 manufactured by GL Sience Co., Ltd.), and are values ​​obtained by conversion to standard polystyrene. Specific measurement conditions are as follows.

[0057] Column: TSKgelαM (manufactured by Tosoh Corporation)

[0058] Column temperature: 40°C

[0059] Eluent composition: contains 100mmol / L H 3 PO 4 (Use H 3 PO 4 85% aqueous solution as raw material) and 10mmol / L LiBr in NMP solution

[0060] Eluent flow rate: 0.5 mL / min

[0061] Calibration standard reagent: polystyrene

[0062] Detector wavelength: 260nm and 300nm

[0063] Detector temperature: room temperature

[0064] Analysis time baseline range: 15 minutes to 40 minutes

[0065] Molecular weight calculation range during analysis: 20 to 35 minutes

[0066] In addition, in this specification, molecular weight distribution index (PDI) is calculated according to the following formula (4).

[0067] (Formula 4)

[0068] PDI=Mw / Mn

[0069] (A) The polyhydroxyamide compound does not contain a carboxyl group or contains a carboxyl group, and the carboxyl equivalent is 1500 g / eq or more, preferably does not contain a carboxyl group or contains a carboxyl group, and is 2000 g / eq or more, and more preferably does not contain a carboxyl group. (A) When the polyhydroxyamide compound does not contain a carboxyl group or the carboxyl equivalent is within the above range, a negative photosensitive resin composition with better resolution can be obtained. It should be noted that the carboxyl group has the effect of improving the solubility of the polyhydroxyamide compound in the developer, but it is speculated that the reaction with the cross-linking agent (C) in the heat treatment (also called PEB (Post Exposure Bake)) before the development process is excessive, which deteriorates the resolution, but the details are unclear.

[0070] The hydroxyl equivalent of the (A) polyhydroxyamide compound is not particularly limited, and can be, for example, 100 to 400 g / eq, preferably 150 to 350 g / eq, and more preferably 200 to 300 g / eq.

[0071] The chlorine atom concentration (or chlorine ion concentration) contained in the molecular structure of the (A) polyhydroxyamide compound is not particularly limited, but is preferably 5 ppm by mass or less relative to the total mass of the (A) polyhydroxyamide compound. The lower the chlorine atom concentration (or chlorine ion concentration) contained in the molecular structure of the negative photosensitive resin composition, the easier it is to make the cured product have excellent insulation reliability.

[0072] 1-2. (B) Oxime sulfonate compounds

[0073] The (B) oxime sulfonate compound is used as an acid generator because the sulfonate bond is cut when irradiated (exposed) with radiation to generate sulfonic acid. The (B) oxime sulfonate compound can be used alone or in combination of two or more in any ratio.

[0074] (B) The oxime sulfonate compound is not particularly limited, but preferably contains a structure represented by the following formula (2) from the viewpoint of further improving the resolution and insulation reliability of the negative photosensitive resin composition.

[0075]

[0076] (In formula (2), X is a hydrocarbon group or a halogen atom, m is an integer from 0 to 3, and R 3 is a hydrogen atom, a hydrocarbon group, an organic group containing a keto group, or a halogen atom. )

[0077] X in formula (2) is not particularly limited, and may be, for example, a hydrocarbon group (eg, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, etc.) or a halogen atom.

[0078] The hydrocarbon group may have a substituent, and may have a linear, branched, or cyclic structure. The hydrocarbon group is preferably a linear or branched one having 1 to 4 carbon atoms.

[0079] As the halogen atom, a chlorine atom or a fluorine atom is preferably used.

[0080] In the formula (2), m represents an integer of 0 to 3, and is preferably 0 or 1. When m is 2 or 3, a plurality of Xs may be the same or different.

[0081] R in formula (2) 3 There are no particular limitations, and for example, it may be a hydrogen atom, a hydrocarbon group, an organic group including a keto group, or a halogen atom. The hydrocarbon group (eg, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, etc.) may be unsubstituted or substituted with a halogen atom.

[0082] The hydrocarbon group is preferably a linear, branched, or cyclic hydrocarbon group having 1 to 20 carbon atoms, and more preferably a linear, branched, or cyclic hydrocarbon group having 1 to 10 carbon atoms.

[0083] As the halogen atom, a chlorine atom or a fluorine atom is preferably used.

[0084] Examples of commercially available products of the oxime sulfonate compound include Irgacure PAG103, Irgacure PAG108, Irgacure PAG121, and Irgacure PAG203 manufactured by BASF Corporation.

[0085] 1-3. (C) Cross-linking agent

[0086] (C) The crosslinking agent contains a plurality of methoxymethyl groups and / or hydroxymethyl groups. These functional groups use the acid generated by the (B) oxime sulfonate compound as an active substance, and produce a crosslinking reaction with the phenolic hydroxyl group and carboxyl group contained in the (A) polyhydroxyamide compound, etc. by heating, so that negative photolithography (pattern formation) is achieved by exposure, PEB and development treatment. In addition, after the pattern is formed, it is further heated, so that the curing reaction of the negative photosensitive resin composition proceeds, and the excellent properties as a cured product are reflected.

[0087] In addition, from the aspect of improving the resolution of the negative photosensitive resin composition and the insulation reliability after curing, it is expected that the crosslinking agent (C) contains a heterocycle. The heterocycle is not particularly limited, and contains a saturated or unsaturated ring containing one or more heteroatoms such as boron, nitrogen, oxygen, phosphorus, sulfur, antimony, arsenic, bismuth, selenium, silicon, tellurium, and tin, a 3-membered ring, a 4-membered ring, a 5-membered ring, a 6-membered ring, a 7-membered ring, or an 8-membered ring. From the viewpoint of the resolution of the negative photosensitive resin composition and the insulation reliability of the cured product, the heterocycle preferably contains a nitrogen heterocycle, and more preferably contains a plurality of nitrogen heterocycles. Specifically, more preferably, compounds with a triazine structure such as hexamethylol melamine and hexamethoxymethyl melamine, compounds with a guanamine structure such as tetramethylol benzoguanamine and tetramethoxymethyl benzoguanamine, compounds with a glycoluril structure such as tetramethylol glycoluril, and compounds with an imidazolidinone structure such as 1,3-bis (methoxymethyl) -2-imidazolidinone. Among these, compounds having a triazine structure including a triazine ring and compounds having a guanamine structure can be particularly preferably used from the viewpoint of providing a negative photosensitive resin composition capable of forming a finer L / S pattern with a high aspect ratio.

[0088] 1-4. (D) Compounds containing phenolic hydroxyl groups

[0089] The negative photosensitive resin composition of the present disclosure may contain (D) a compound containing a phenolic hydroxyl group. When the negative photosensitive resin composition contains (D) a compound containing a phenolic hydroxyl group, the resolution change of the negative photosensitive resin composition is excellent. It is speculated that this is because the increase in the phenolic hydroxyl group in the negative photosensitive resin composition promotes the crosslinking reaction of the exposed part with the crosslinking agent (C) and the developability of the unexposed part, but since the resolution is significantly improved to more than expected, the detailed mechanism is unclear.

[0090] In addition, (D) the compound containing a phenolic hydroxyl group is a compound different from (A) the polyhydroxyamide compound, (B) the oxime sulfonate compound, and (C) the cross-linking agent.

[0091] (D) The compound containing a phenolic hydroxyl group is not particularly limited as long as it contains one or more phenolic hydroxyl groups. For example, as a monomer, phenol, o-cresol, m-cresol, p-cresol, o-hydroxystyrene, m-hydroxystyrene, p-hydroxystyrene, hydroquinone, catechol, resorcinol, hydroxyhydroquinone, phloroglucinol, pyrogallol, hexahydroxybenzene, p-tert-butylphenol, p-ethylphenol, 2,3-xylenol, 2,5-xylenol, m-ethylphenol, 3,5-xylenol, m-methoxyphenol, bisphenol A, bisphenol F,

[0092] Examples of the polymer include phenolic resins such as resol-type phenolic resins and novolac-type phenolic resins; polyphenol polymers such as polyhydroxystyrene polymers polymerized with hydroxystyrene (either ortho-, meta- or para-); and polyphenol copolymers such as polyhydroxystyrene copolymers copolymerized with hydroxystyrene (either ortho-, meta- or para-) and other polymerizable compounds such as styrene.

[0093] These can be used alone or in combination of multiple types at any ratio. Among these, polyhydroxystyrene polymers obtained by polymerizing hydroxystyrene (ortho, meta, or para) or polyhydroxystyrene copolymers obtained by copolymerizing hydroxystyrene (ortho, meta, or para) with other polymerizable compounds are preferred, and polyhydroxystyrene copolymers obtained by copolymerizing hydroxystyrene (ortho, meta, or para) with styrene are more preferred.

[0094] The weight average molecular weight (Mw) of the polyhydroxystyrene polymer or the polyhydroxystyrene copolymer is preferably 2,000 to 10,000, more preferably 3,000 to 8,000, further preferably 4,000 to 6,000.

[0095] The number average molecular weight (Mn) of the polyhydroxystyrene polymer or the polyhydroxystyrene copolymer is preferably 1,000 to 5,000, more preferably 1,500 to 4,000, and even more preferably 2,000 to 3,000.

[0096] The molecular weight dispersion index (PDI) of the polyhydroxystyrene polymer or the polyhydroxystyrene copolymer is preferably 1.5 to 4.0, more preferably 1.5 to 3.0.

[0097] When the weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight dispersion (PDI) of the polyhydroxystyrene polymer or the polyhydroxystyrene copolymer are within the above ranges, the resolution of the negative photosensitive resin composition can be further improved.

[0098] (D) The hydroxyl group equivalent of the compound containing a phenolic hydroxyl group is not particularly limited, but is, for example, preferably 100 to 300 g / eq, and more preferably 100 to 200 g / eq.

[0099] The concentration of chlorine atoms (or chlorine ions) contained in the molecular structure of the compound (D) containing a phenolic hydroxyl group is not particularly limited, but is preferably 5 ppm by mass or less relative to the total mass of the compound (D) containing a phenolic hydroxyl group. The lower the concentration of chlorine atoms (or chlorine ions) contained in the molecular structure of the negative photosensitive resin composition, the easier it is to make the insulation reliability of the cured product better.

[0100] 1-5. (E) Basic compounds

[0101] The negative photosensitive resin composition of the present disclosure preferably contains (E) a basic compound from the viewpoint of improving dissolution contrast, resolution, and stability of the coating film at the delayed development time after exposure from coating the photosensitive resin composition to exposure. In particular, when the negative photosensitive resin composition of the present disclosure contains a basic compound, it is possible to suppress the diffusion of the acid generated by the oxime sulfonate compound during exposure to the unexposed portion, thereby preventing the generation of development residues in the unexposed portion after development.

[0102] (E) The basic compound is not particularly limited, and examples thereof include amine compounds such as trimethylamine, diethylamine, triethylamine, di-n-propylamine, tri-n-propylamine, tri-n-amylamine, tribenzylamine, diethanolamine, triethanolamine, n-hexylamine, n-heptylamine, n-octylamine, n-nonylamine, ethylenediamine, N,N,N',N'-tetramethylethylenediamine, tetramethylenediamine, hexamethylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 4,4'-diaminobenzophenone, and 4,4'-diaminodiphenylamine; and formamide, N-methylformamide, N,N-dimethylformamide, acetamide, N-methylacetamide, Amide compounds such as N,N-dimethylacetamide, propionamide, and benzamide; lactams such as pyrrolidone and N-methylpyrrolidone; urea compounds such as methylurea, 1,1-dimethylurea, 1,3-dimethylurea, 1,1,3,3-tetramethylurea, and 1,3-diphenylurea; nitrogen-containing heterocyclic compounds such as imidazole, benzimidazole, 4-methylimidazole, 8-hydroxyquinoline, acridine, purine, pyrrolidine, piperidine, 2,4,6-tris(2-pyridyl)-s-triazine, piperazine, 1,4-dimethylpiperazine, 1,4-diazabicyclo[2.2.2]octane, and pyridine; morpholine compounds such as morpholine and 4-methylmorpholine, etc. These can be used alone or in combination of a plurality of them at any ratio.

[0103] 1-6. (F) Inorganic fillers

[0104] The negative photosensitive resin composition disclosed herein may contain an inorganic filler. As the inorganic filler, there is no particular limitation, and conventionally known inorganic fillers can be used, for example, silica, aluminum hydroxide, aluminum oxide, aluminum nitride, boron nitride, glass powder, magnesium carbonate, barium sulfate, barium titanate, hydrotalcite, etc. They can be used alone or in combination of multiple types in any ratio. From the viewpoint of excellent insulation reliability and reducing the thermal expansion coefficient of the negative photosensitive resin composition, silica is preferably used, and spherical silica is particularly preferably used.

[0105] The volume average particle size (D50) of the inorganic filler can be 1.0 μm or less, preferably 500 nm or less, and particularly preferably 100 nm or less. The volume average particle size of the inorganic filler can be measured by a laser diffraction method.

[0106] 1-7. Solvent

[0107] The negative photosensitive resin composition of the present disclosure may contain a solvent. The solvent is not particularly limited, and examples thereof include 2-methoxy-1-methylethyl acetate (PGMEA), 4-methyl-2-pentanone, γ-butyrolactone, N-methylpyrrolidone, N-methylcaprolactam, dimethyl sulfoxide, tetramethylurea, pyridine, dimethyl sulfone, hexamethyl sulfoxide, ethyl acetate, butyl acetate, ethyl lactate, methyl 3-methoxypropionate, methyl 2-methoxypropionate, ethyl 3-methoxypropionate, ethyl 2-methoxypropionate, ethyl 3-ethoxypropionate, and ethyl 2-ethoxypropionate. , ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, propylene glycol dimethyl ether, dipropylene glycol dimethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, propylene glycol monomethyl ether acetate, carbitol acetate, ethyl cellosolve acetate, cyclohexanone, cyclopentanone, methyl ethyl ketone, methyl isobutyl ketone, 2-heptanone, etc. They can be used alone or in any ratio. In these solvents, from the viewpoint of excellent affinity with each component in the negative photosensitive resin composition, gamma-butyrolactone or cyclopentanone is preferred. In addition, cyclopentanone is particularly preferred from the viewpoint of excellent solvent removability during drying of the negative photosensitive resin composition and suitability for an edge rinse step in semiconductor production.

[0108] 1-8. Other ingredients

[0109] The negative photosensitive resin composition of the present disclosure may contain other components as long as they do not impair the effects of the disclosed technology. As other components, known substances that can be contained in the negative photosensitive resin composition can be used, for example, adhesives, surfactants, plasticizers, thermal acid generators, sensitizers, leveling agents, colorants, fibers, microparticles, etc.

[0110] The surfactant is not particularly limited, and examples thereof include fluorine-based surfactants and silicon-based surfactants. Commercially available fluorine-based surfactants include "Megaface" series manufactured by DIC Corporation (e.g., Megaface F-281, F-477, F-553, F-554, F-555, F-556, F-557, F-558, F-559, F-560, F-561, F-563, F-569, etc.). Commercially available products of silicone-based surfactants include BYK Corporation surface conditioner series (e.g., BYK-302, BYK-307, BYK-310, BYK-322, BYK-323, BYK-326, BYK-331, BYK-332, BYK-333, BYK-348, BYK-349, BYK-377, BYK-378, BYK-3455, BYK-3760, etc.) etc. These may be used alone or in combination of two or more.

[0111] 2. Preparation of negative photosensitive resin composition

[0112] The negative photosensitive resin composition of the present disclosure can be obtained by mixing (A) a polyhydroxyamide compound, (B) an oxime sulfonate compound, and (C) a crosslinking agent with arbitrary components represented by (D) a compound containing a phenolic hydroxyl group and (E) a basic compound. The components can be mixed under heating as necessary.

[0113] When the total mass of the solid content of the negative photosensitive resin composition is 100 mass %, the amount of the polyhydroxyamide compound (A) may be 50 to 80 mass %. The solid content mass in the present specification refers to the mass of the residue obtained by completely volatilizing the volatile components.

[0114] When the total mass of the solid content of the negative photosensitive resin composition is 100 mass %, the amount of the oxime sulfonate compound (B) may be 0.5 to 10 mass %, preferably 1 to 5 mass %.

[0115] When the total mass of the solid content of the negative photosensitive resin composition is set to 100 mass %, the amount of the crosslinking agent (C) can be set to 10 to 40 mass %. In addition, for the amount of the crosslinking agent (C), the ratio of the number of methoxymethyl and / or hydroxymethyl groups contained in the crosslinking agent (C) to the number of phenolic hydroxyl groups contained in the negative photosensitive resin composition (methoxymethyl and / or hydroxymethyl: phenolic hydroxyl group) can be 120:100 to 200:100. By setting such a ratio, the resolution of the negative photosensitive resin composition and the insulation reliability after curing can be made better.

[0116] When the total mass of the solid content of the negative photosensitive resin composition is 100 mass %, the compounding amount of (D) the compound containing a phenolic hydroxyl group can be 1 to 15 mass %, preferably 5 to 12 mass %, and more preferably 6 to 11 mass %. In addition, the compounding amount of the (A) polyhydroxyamide compound: the compound containing a phenolic hydroxyl group (D) can be 80:20 to 99:1, preferably 80:20 to 95:5, and more preferably 85:15 to 90:10.

[0117] In addition, the amount of the polyhydroxyamide compound (A) and the compound containing a phenolic hydroxyl group (D) can be adjusted so that the ratio of the number of methoxymethyl and / or hydroxymethyl groups contained in the crosslinking agent (C) to the number of phenolic hydroxyl groups contained in the negative photosensitive resin composition (methoxymethyl and / or hydroxymethyl groups: phenolic hydroxyl groups) is 120: 100 to 200: 100. By setting such a ratio, the resolution of the negative photosensitive resin composition and the insulation reliability after curing can be made more excellent.

[0118] When the total mass of the solid content of the negative photosensitive resin composition is 100 mass %, the amount of the basic compound (E) added can be 0.01 to 0.50 mass %, preferably 0.08 to 0.40 mass %. By setting it to such a range, it becomes easy to suppress the generation of development residues in the unexposed part after developing the negative photosensitive resin composition.

[0119] When the total mass of the solid content of the negative photosensitive resin composition is set to 100 mass %, the amount of the inorganic filler (F) added can be set to 1 mass % to 50 mass %, preferably 10 mass % to 40 mass %. By setting it to such a range, the negative photosensitive resin composition can be maintained while maintaining the developability and making the cured product of the negative photosensitive resin composition have a low thermal expansion coefficient.

[0120] 3. Dry film

[0121] The dry film of the present disclosure comprises: a substrate; and a resin layer formed on the substrate using the negative photosensitive resin composition of the present disclosure. In addition, a protective film may be further laminated on the surface of the resin layer to protect the resin layer.

[0122] The substrate is not particularly limited, and examples thereof include metal foils such as copper foil; and films such as polyimide films, polyester films, and polyethylene naphthalate (PEN) films.

[0123] The protective film is not particularly limited, and polyethylene film, polytetrafluoroethylene film, polypropylene film, paper, etc. can be used. The protective film is preferably selected so that the adhesion between the protective film and the resin layer is lower than the adhesion between the substrate and the resin layer. In order to make the adhesion between the protective film and the resin layer lower than the adhesion between the substrate and the resin layer, a protective film subjected to a peeling treatment can be used.

[0124] The thickness of the resin layer is not particularly limited and can be set to 1 to 150 μm depending on the application. The resin layer can be obtained, for example, by coating a negative photosensitive resin composition on a substrate, adjusting the thickness of the resin layer using a comma coater, a blade coater, a lip coater, a rod coater, a pressure coater, a reverse coater, a transfer roll coater, a gravure coater or a spray coater, and drying.

[0125] 4. Cured product

[0126] The cured product of the present disclosure is obtained by curing the negative photosensitive resin composition or the resin layer of the dry film of the present disclosure. The cured product may be a patterned cured product. As an example of a method for producing a patterned cured product, the following method may be cited.

[0127] 4-1. Dry coating film forming step

[0128] The dry coating film forming step is a step of applying the negative photosensitive resin composition of the present disclosure on a substrate to form a coating film and then drying the coating film. The dry coating film forming step can also be performed by transferring the resin layer of the dry film onto the substrate to form a dry coating film on the substrate.

[0129] There is no particular limitation on the method of coating the negative photosensitive resin composition on the substrate, and examples thereof include: a method of coating with a spin coater, a rod coater, a blade coater, a curtain coater, a screen printer, etc.; a method of spray coating with a spray coater, an inkjet method, etc. The coating film thickness is not particularly limited, and for example, it can be set to 10 μm or less, 5 μm or less, or 3 μm or less. By reducing the film thickness, a finer L / S patterning can be achieved while maintaining the aspect ratio of the pattern.

[0130] The method for drying the coating film is not particularly limited, and examples thereof include air drying, heating drying in an oven or hot plate, vacuum drying, etc. Conditions for heating drying are, for example, a heating temperature of 70 to 140° C. and a drying time of 1 to 30 minutes.

[0131] The transfer of the resin layer of the dry film onto the substrate is preferably performed under pressure and heating using a vacuum laminator or the like. The heating temperature can be, for example, 60 to 100°C.

[0132] The substrate is not particularly limited, and may be, for example, a printed circuit board formed with a circuit, a flexible printed circuit board, or a wafer formed with a semiconductor element.

[0133] 4-2. Exposure process

[0134] The exposure step is a step of irradiating the dry coating film formed in the dry coating film forming step with radiation through a photomask capable of forming a desired pattern, thereby sensitizing the (B) oxime sulfonate compound in the exposed portion to generate an active substance. When patterning is not required, there is no need to use a photomask. Alternatively, a direct drawing device may be used to draw a pattern directly with a laser.

[0135] The wavelength of the radiation used is a wavelength that can activate the (B) oxime sulfonate compound. For patterning after micronization, the maximum wavelength is preferably 410 nm or less. The irradiation energy can be adjusted according to the thickness of the dry coating film to be formed, for example, it can be set to 10 to 1000 mJ / cm 2 As the exposure light source, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury short-arc lamp, a KRF laser, or the like can be used.

[0136] 4-3.PEB process

[0137] The PEB process is a process in which the dried coating film exposed in the exposure process is subjected to a heat treatment to impart development resistance to the exposed portion of the dried coating film (hereinafter sometimes referred to as the exposed portion). In the PEB process, in the exposed portion, the acid generated by the (B) oxime sulfonate compound is used as an active substance, and a crosslinking reaction of the (A) polyhydroxyamide compound, the (D) compound containing a phenolic hydroxyl group and the (C) crosslinking agent is performed, and the exposed portion is insoluble in the developer. The heating temperature in the PEB process can be set to 90 to 150° C., and the heating time can be set to 0.5 to 10 minutes. Heating can be performed by a known method such as a hot plate or a heating furnace.

[0138] 4-4. Development process

[0139] The development step is a step of treating the dried coating film heated in the PEB step with a developer to dissolve the unexposed portion of the dried coating film in the developer and remove it, thereby obtaining a patterned coating film. As a development method, a known method can be used, for example, a rotary spray method, a paddle method, an immersion method with ultrasonic treatment, etc.

[0140] The developer can use a known substance, for example, an aqueous solution of inorganic amines such as sodium hydroxide, sodium carbonate, sodium silicate, and ammonia, organic amines such as ethylamine, diethylamine, triethylamine, and triethanolamine, and quaternary ammonium salts such as tetramethylammonium hydroxide and tetrabutylammonium hydroxide. If necessary, a water-soluble organic solvent such as methanol, ethanol, and isopropanol, and a surfactant can be added.

[0141] After the developer treatment, the coating film can be cleaned with a rinse solution as needed to obtain a patterned coating film. The rinse solution is not particularly limited, and pure water, methanol, ethanol, isopropanol, etc. can be cited. They can be used alone or in combination in any ratio.

[0142] 4-5. Post-development heating process

[0143] The post-development heating step is a step of heating the pattern coating film formed in the development step to terminate the curing of the pattern coating film and obtain a cured pattern coating film (cured product). The heating temperature can be set to 150 to 200° C., and the heating time can be set to 1 to 120 minutes. The heating can be performed by a known method such as a hot plate or an inert oven, and it is desirable to heat under a nitrogen atmosphere.

[0144] 5. Use of negative photosensitive resin composition

[0145] The negative photosensitive resin composition disclosed in the present invention can be used as a forming material for display devices, semiconductor elements, electronic components, optical components, building materials, etc. The forming material of the semiconductor element is, for example, an anti-corrosion material, a buffer coating, and an insulating film for a rewiring layer of a wafer-level package (WLP). The negative photosensitive resin composition disclosed in the present invention can form an extremely fine wiring with an L / S of less than 2μm / 2μm and an aspect ratio of more than 2.0, and has excellent insulation reliability. Therefore, it can be particularly preferably used in a rewiring layer formation process using a mosaic method. In addition, as a forming material for electronic components, for example, a printed circuit board, an interlayer insulating film, a wiring film, etc. can be cited.

[0146] Example

[0147] The present disclosure technology will be described in more detail using examples, but the present disclosure technology is not limited to the examples.

[0148] The components used in Examples and Comparative Examples are as follows.

[0149] <(A) Polyhydroxyamide compound>

[0150] (Synthesis Example 1: Synthesis Example of the Polyhydroxyamide Compound (A-1) of the Example)

[0151] In a 500 mL flask equipped with a stirrer and a thermometer, 21.62 g (59.03 mmol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP) was stirred and dissolved in 140 g of N-methylpyrrolidone (NMP). After that, the flask was immersed in an ice bath, and while the temperature in the flask was maintained at 0 to 5°C, 12.09 g (40.97 mmol) of 4,4'-oxybis(benzoyl chloride) (DEDC) was added directly as a solid over 10 minutes, and stirred in the ice bath for 30 minutes. After stirring at room temperature for 18 hours, 5.93 g (36.13 mmol) of 5-norbornene-2,3-dicarboxylic anhydride was added at room temperature, and stirring was continued for further 3 hours. The stirred solution was put into a large amount of ion exchange water, and the precipitate was recovered. The obtained solid was dissolved in 160 g of ethyl acetate. 20 g of anion exchange resin (Organo Amberlist B-20) was added thereto and stirred rapidly for 1 hour. The stirred solution was concentrated and then added to a large amount of ion exchange water to recover the precipitate. The precipitated solid was recovered and dried under reduced pressure to obtain a carboxyl-terminated polyhydroxyamide compound (A-1).

[0152] The obtained polyhydroxyamide compound (A-1) is as follows: weight average molecular weight (Mw) is 8613, number average molecular weight (Mn) is 4557, molecular weight dispersion (PDI) is 1.9, chloride ion is 3.3 ppm, phenolic hydroxyl equivalent is 294 g / eq, and carboxyl equivalent is 2279 g / eq.

[0153] (A-1) Polyhydroxyamide compound

[0154]

[0155] (Synthesis Example 2: Synthesis Example of the Polyhydroxyamide Compound (A-2) of the Example)

[0156] In a 500 mL flask equipped with a stirrer and a thermometer, 14.93 g (44.39 mmol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP) and 4.90 g (44.84 mmol) of 3-aminophenol were stirred and dissolved in 79 g of N-methylpyrrolidone (NMP). After that, the flask was immersed in an ice bath, and while the temperature in the flask was maintained at 0 to 5°C, 16.41 g (55.61 mmol) of 4,4'-oxybis(benzoyl chloride) (DEDC) was added directly as a solid over 10 minutes, and stirred in the ice bath for 30 minutes. After stirring at room temperature for 18 hours, the solution was added to a large amount of ion exchange water, and the precipitate was recovered. The obtained solid was dissolved in 135 g of ethyl acetate. 18 g of anion exchange resin (Amberlist B-20 from Organo) was added thereto, and stirred rapidly for 1 hour. The stirred solution was concentrated and then poured into a large amount of ion exchange water to recover the precipitate. The precipitated solid was recovered and then dried under reduced pressure to obtain a hydroxyl-terminated polyhydroxyamide compound (A-2).

[0157] The obtained polyhydroxyamide compound (A-2) had a weight average molecular weight (Mw) of 4580, a number average molecular weight (Mn) of 1696, a molecular weight dispersion (PDI) of 2.7, a chloride ion of 2.3 ppm, and a phenolic hydroxyl equivalent of 218 g / eq.

[0158] (A-2) Polyhydroxyamide compound

[0159]

[0160] (Synthesis Example 3: Synthesis Example of the Polyhydroxyamide Compound (A-3) of the Example)

[0161] In a 500 mL flask equipped with a stirrer and a thermometer, 14.93 g (44.39 mmol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP) and 2.45 g (22.42 mmol) of 3-aminophenol were stirred and dissolved in 79 g of N-methylpyrrolidone (NMP). After that, the flask was immersed in an ice bath, and while the temperature in the flask was maintained at 0 to 5°C, 16.41 g (55.61 mmol) of 4,4'-oxybis(benzoyl chloride) (DEDC) was added directly as a solid over 10 minutes, and stirred in the ice bath for 30 minutes. After stirring at room temperature for 18 hours, the solution was added to a large amount of ion exchange water, and the precipitate was recovered. The obtained solid was dissolved in 79 g of ethyl acetate. 17 g of anion exchange resin (Amberlist B-20 from Organo) was added thereto, and stirred rapidly for 1 hour. The stirred solution was concentrated and then poured into a large amount of ion exchange water to recover the precipitate. The precipitated solid was recovered and then dried under reduced pressure to obtain a hydroxyl-terminated polyhydroxyamide compound (A-3).

[0162] The obtained polyhydroxyamide compound (A-3) had a weight average molecular weight (Mw) of 9222, a number average molecular weight (Mn) of 3561, a molecular weight dispersion (PDI) of 2.6, a chloride ion of 3.1 ppm, and a phenolic hydroxyl equivalent of 252 g / eq.

[0163] (A-3) Polyhydroxyamide compound

[0164]

[0165] (Synthesis Examples 4 to 8: Synthesis Examples of Polyhydroxyamide Compounds (A-4 to A-8) of Examples)

[0166] A polyhydroxyamide compound was synthesized by the same method as in Synthesis Example 3 except that the blending amounts of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP), 3-aminophenol, and 4,4'-oxybis(benzoyl chloride) (DEDC) were set to the ratios shown in Table 1. The weight average molecular weight, number average molecular weight, and molecular weight dispersion of the obtained polyhydroxyamide compound are also shown in Table 1.

[0167] [Table 1]

[0168] 6FAP(mmol) Aminophenol(mmol) DEDC(mmol) M Mn PDI Hydroxyl equivalent A-4 44.49 22.03 55.51 9,500 3,800 2.5 255 A-5 46.34 14.63 53.66 12,800 4,400 2.9 260 A-6 47.03 11.88 52.97 14,000 5,200 2.7 264 A-7 47.50 10.00 52.50 16,500 6,100 2.7 268 A-8 48.04 7.83 51.96 18,000 6,000 3.0 268

[0169] (Synthesis Example 9: Synthesis Example of the Polyhydroxyamide Compound (A-9) of Comparative Example)

[0170] In a 500 mL flask equipped with a stirrer and a thermometer, 18.90 g (51.60 mmol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP) was stirred and dissolved in 80 g of N-methylpyrrolidone (NMP). After that, the flask was immersed in an ice bath, and while the temperature in the flask was maintained at 0 to 5°C, 14.28 g (48.40 mmol) of 4,4'-oxybis(benzoyl chloride) (DEDC) was added directly as a solid over 10 minutes, and stirred in the ice bath for 30 minutes. After stirring at room temperature for 18 hours, 1.05 g (6.40 mmol) of 5-norbornene-2,3-dicarboxylic anhydride was added at room temperature, and stirring was continued for further 3 hours. The stirred solution was put into a large amount of ion exchange water, and the precipitate was recovered. The obtained solid was dissolved in 140 g of ethyl acetate. 8 g of anion exchange resin (Organo Amberlist B-20) was added thereto and stirred rapidly for 1 hour. The stirred solution was concentrated and then added to a large amount of ion exchange water to recover the precipitate. The precipitated solid was recovered and dried under reduced pressure to obtain a carboxyl-terminated polyhydroxyamide compound.

[0171] The obtained polyhydroxyamide compound is as follows: weight average molecular weight (Mw) is 32992, number average molecular weight (Mn) is 12310, molecular weight dispersion (PDI) is 2.7, chloride ion is 2.8 ppm, phenolic hydroxyl equivalent is 294 g / eq, and carboxyl equivalent is 6155 g / eq.

[0172] Polyhydroxyamide compounds

[0173]

[0174] (Synthesis Example 10: Synthesis Example of a polyamic acid compound (A-10) of a comparative example)

[0175] In a 500mL flask equipped with a stirrer and a thermometer, 96g of 2-methoxy-1-methylethyl acetate (PGMEA) and 14.87g (46.45mmol) of 2,2'-bis(trifluoromethyl)benzidine (TFMB) were added and stirred to dissolve. After confirming that the monomer was completely dissolved, 23.79g (53.55mmol) of 6FDA was added directly as a solid over 5 minutes, and stirring was continued at room temperature for 1 hour. After that, 2.33g (14.20mmol) of 5-norbornene-2,3-dicarboxylic anhydride was added directly as a solid to the stirred solution, and stirred at room temperature for 16 hours. The stirred solution was put into a large amount of ion exchange water, and the precipitate was recovered. It was dried under reduced pressure to obtain a polyamic acid compound at the carboxyl end.

[0176] The obtained polyamic acid compound had a weight average molecular weight (Mw) of 10324, a number average molecular weight (Mn) of 4382, a molecular weight dispersion (PDI) of 2.4, a chloride ion content of 2.1 ppm, and a carboxyl equivalent of 382 g / eq.

[0177] Polyamic acid compounds

[0178]

[0179] (Synthesis Example 11: Synthesis Example of the Polyhydroxyamide-Polyamic Acid Copolymer Compound (A-11) of Comparative Example)

[0180] In a 500 mL flask equipped with a stirrer and a thermometer, 13.97 g (38.15 mmol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP) and 5.24 g (16.35 mmol) of 2,2'-bis(trifluoromethyl)benzidine (TFMB) were added to 80 g of N-methylpyrrolidone (NMP) and stirred to dissolve. After confirming that the monomers were completely dissolved, the flask was immersed in an ice bath, and while the temperature in the flask was maintained at 0 to 5°C, 8.11 g (18.26 mmol) of 6FDA and 9.40 g (31.85 mmol) of 4,4'-oxybis(benzoyl chloride) (DEDC) were added as a solid over 10 minutes, and stirred in the ice bath for 30 minutes. Thereafter, 2.95 g (18.00 mmol) of 5-norbornene-2,3-dicarboxylic anhydride was added as a solid to the stirred solution, and stirred at room temperature for 3 hours. The stirred solution was put into a large amount of ion exchange water and the precipitate was recovered. The obtained solid was dissolved in 150g of ethyl acetate. 38g of anion exchange resin (Organo Amberlist B-20) was added thereto and stirred sharply for 1 hour. After the stirred solution was concentrated, it was put into a large amount of ion exchange water and the precipitate was recovered. After the precipitated solid was recovered, it was dried under reduced pressure to obtain a carboxyl-terminated polyhydroxyamide-polyamic acid copolymer compound.

[0181] The obtained polyhydroxyamide-polyamic acid copolymer compound is as follows: weight average molecular weight (Mw) is 11447, number average molecular weight (Mn) is 5283, molecular weight dispersion (PDI) is 2.2, chloride ion is 4.2 ppm, phenolic hydroxyl equivalent is 458 g / eq, and carboxyl equivalent is 1069 g / eq.

[0182] <(B) Oxime sulfonate compound>

[0183] (B-1) PAG-103 (oxime sulfonate compound manufactured by BASF Co., Ltd.)

[0184]

[0185] <Photoacid generator of comparative example> SP606 (naphthalene imide compound manufactured by ADEKA Corporation)

[0186]

[0187] <(C) Cross-linking agent>

[0188] (C-1) MW-390 (Hexamethoxymethylmelamine compound manufactured by NIPPON CARBIDE INDUSTRIES CO., INC.)

[0189]

[0190] <(D) Compounds containing phenolic hydroxyl groups>

[0191] (D-1) VPS-2515 (polyhydroxystyrene-styrene copolymer manufactured by Nippon Soda Co., Ltd., weight average molecular weight (Mw): 4667, number average molecular weight (Mn): 2593, molecular weight dispersion (PDI): 1.8, chloride ion: 2.8 ppm, phenolic hydroxyl equivalent: 140 g / eq)

[0192] <(E) Basic compounds>

[0193] (E-1) Triethanolamine (TEA)

[0194] <Inorganic fillers>

[0195] Y50SV-AH2 (spherical silica manufactured by Admatechs, volume average particle size D50 = 50 nm)

[0196] <Surfactant>

[0197] BYK-310 (manufactured by BYK Corporation, silicone-based surfactant)

[0198] <Solvent>

[0199] γ-Butyrolactone (manufactured by Daishin Chemical Co., Ltd.)

[0200] Cyclopentanone (Tokyo Chemical Industry Co., Ltd.)

[0201] <Preparation of negative photosensitive resin composition>

[0202] The components were mixed in the amounts shown in Tables 2 to 4, and dissolved in a solvent and adjusted so that the concentration of the nonvolatile components in the varnish was 30%, thereby obtaining the varnish of the negative photosensitive resin composition of each embodiment and comparative example. It should be noted that the amount of each component in Tables 2 to 4, except for the amount of the solvent, represents the solid content mass. In addition, the equivalent ratio (NCH) of the functional group of the crosslinking agent to the phenolic hydroxyl group calculated from the amount of the raw materials of the negative photosensitive resin composition was 2 OCH 3 Group: OH group) are shown in Tables 2 to 4.

[0203] <Evaluation>

[0204] The following evaluations were performed using the obtained varnishes of the respective Examples and Comparative Examples. The evaluation results are shown in Tables 2 to 4.

[0205] (Resolution evaluation)

[0206] ·Measurement of line width / line spacing (L / S) and aspect ratio

[0207] The varnish of each example and comparative example was applied on a silicon wafer using a spin coater so that the film thickness after curing was 3.0 μm or 3.5 μm, and dried on a hot plate at 110° C. for 3 minutes to obtain a dry coating film of the negative photosensitive resin composition of each example and comparative example. A test pattern with L / S of 0.5 / 0.5 μm, 0.6 / 0.6 μm, 0.7 / 0.7 μm, 0.8 / 0.8 μm, 1 / 1 μm, 1.2 / 1.2 μm, 1.5 / 1.5 μm, 1.7 / 1.7 μm, 2 / 2 μm, 3 / 3 μm, 4 / 4 μm, and 5 / 5 μm was exposed to the dry coating film using a linear stepper exposure device (reduced projection exposure device: NSR-2005i9C (manufactured by Nikon Corporation; NA (numerical aperture) = 0.5, σ = 0.68, light source: high pressure mercury lamp) and the dried coating film was exposed to a test pattern with L / S of 0.5 / 0.5 μm, 0.6 / 0.6 μm, 0.7 / 0.7 μm, 0.8 / 0.8 μm, 1 / 1 μm, 1.2 / 1.2 μm, 1.5 / 1.5 μm, 1.7 / 1.7 μm, 2 / 2 μm, 3 / 3 μm, 4 / 4 μm, and 5 / 5 μm, and the dried coating film was exposed on a hot plate. Post-exposure heating (PEB) was performed at 140°C for 60 minutes. Thereafter, development was performed with a 2.38% TMAH aqueous solution for 60 seconds, rinsed with ultrapure water for 30 seconds, and spin dried for 30 seconds. A sample having a pattern of the negative photosensitive resin composition of each embodiment and comparative example was obtained. It should be noted that the exposure conditions (exposure amount and focusing) in the negative photosensitive resin composition of each embodiment and comparative example were selected to obtain the best resolution for the negative photosensitive resin composition of each embodiment and comparative example. The exposure conditions of each embodiment and comparative example are shown in Tables 2 to 4.

[0208] The samples of the obtained embodiments and comparative examples were cut in such a way that a cross section perpendicular to the length direction of the pattern could be observed. The cut surface of the pattern was observed with a scanning electron microscope (observation magnification of 10,000 times) to obtain the minimum L / S of normal patterning. It should be noted that the samples in which each pattern was patterned vertically without collapse were judged to be normal patterning.

[0209] In addition, the aspect ratio (=film thickness÷line width of the minimum L / S) was determined for the minimum L / S pattern formed from the negative photosensitive resin composition of each example and comparative example.

[0210] In addition, when the cross-sectional observation is performed for the minimum L / S of the normal patterning, it is observed whether there is development residue in the unexposed part. For samples with slight development residue, it is recorded as (residue) in the column of the minimum L / S in Tables 2 to 4.

[0211] Determination of through hole opening diameter

[0212] The test patterns with opening diameters of 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0, 15.0, and 20.0 μm were exposed using a contact exposure device (light source: high pressure mercury lamp). The minimum through hole opening diameter that can be patterned was determined in the same manner as the above-mentioned L / S measurement except for the exposure step. For samples with slightly visible development residues, the column of the minimum through hole opening diameter in Tables 2 to 4 is recorded as (residue).

[0213] (Insulation reliability evaluation)

[0214] The varnish of each embodiment and comparative example was applied on a comb-shaped wiring substrate with L / S=12 / 13μm manufactured by KYOCERA Corporation using a spin coater in a film thickness of 20μm. The coating was dried at 110°C for 5 minutes using a hot plate to obtain a negative photosensitive resin composition coating film of each embodiment and comparative example formed on the comb-shaped wiring substrate. The coating film was exposed to light (1000mJ / cm2) on the entire surface using a high-pressure mercury lamp. 2 ), heat-cured at 200°C for 1 hour in an inert oven under a nitrogen atmosphere. After that, the cured material on the electrode portion of the comb-shaped wiring substrate was removed with a cutter, and the power plug was soldered to serve as an insulation reliability evaluation substrate. For this evaluation substrate, a voltage of 20V (1.7V / μm for a wiring of 12μm) was applied in an environment of 130°C and 85RH%, and the time when the resistance between the comb-shaped wirings (cured material formed by a negative photosensitive resin composition) became less than 10MΩ was measured. It should be noted that when the resistance between the comb-shaped wirings (negative photosensitive resin composition film) becomes less than 10MΩ, it is considered that the circuit has failed.

[0215] It should be noted that when the measurement result is recorded as ">300h", it means that even if it exceeds 300 hours, the resistance between the comb-shaped wirings (negative photosensitive resin composition film) does not become 10MΩ or less. In addition, when it is recorded as "<20h", it means that the resistance between the comb-shaped wirings (negative photosensitive resin composition film) becomes 10MΩ or less in less than 20 hours.

[0216] [Table 2]

[0217]

[0218] [Table 3]

[0219]

[0220] [Table 4]

[0221]

Claims

1. A negative photosensitive resin composition, characterized in that: contain: (A) a polyhydroxyamide compound comprising a structural unit represented by the following formula (1); (B) an oxime sulfonate compound; and (C) a cross-linking agent, The weight average molecular weight of the polyhydroxyamide compound (A) is 2,000 to 20,000, The (A) polyhydroxyamide compound does not contain a carboxyl group or has a carboxyl equivalent of 1500 g / eq or more, The (C) cross-linking agent comprises a plurality of methoxymethyl groups and / or hydroxymethyl groups, In formula (1), R 1 is a divalent organic group, R 2 It is a tetravalent organic group.

2. The negative photosensitive resin composition according to claim 1, characterized in that The (A) polyhydroxyamide compound has a carboxyl group or a phenolic hydroxyl group at a terminal.

3. The negative photosensitive resin composition according to claim 1 or 2, characterized in that: The (B) oxime sulfonate compound has a structure represented by the following formula (2): In formula (2), X is a hydrocarbon group or a halogen atom, m is an integer of 0 to 3, and R 3 is a hydrogen atom, a hydrocarbon group, an organic group including a keto group, or a halogen atom.

4. The negative photosensitive resin composition according to any one of claims 1 to 3, characterized in that: The (C) cross-linking agent contains a heterocyclic ring.

5. The negative photosensitive resin composition according to claim 4, characterized in that: The (C) cross-linking agent is a compound having a triazine ring.

6. The negative photosensitive resin composition according to any one of claims 1 to 5, characterized in that: (D) A compound containing a phenolic hydroxyl group is contained.

7. The negative photosensitive resin composition according to claim 6, characterized in that: The (D) compound containing a phenolic hydroxyl group contains a polyhydroxystyrene polymer or a polyhydroxystyrene copolymer.

8. The negative photosensitive resin composition according to any one of claims 1 to 7, characterized in that: Contains (E) a basic compound.

9. A dry film, characterized in that: The invention comprises a resin layer formed from the negative photosensitive resin composition according to any one of claims 1 to 8.

10. A solidified product, characterized in that: The negative photosensitive resin composition is formed of any one of claims 1 to 8 or the resin layer of the dry film is formed of claim 9 .

11. An electronic component, characterized in that: A cured product according to claim 10.

Citation Information

Patent Citations

  • Negative type photosensitive resin composition, method for producing pattern and electronic parts

    JP2001125267A

  • Negative photosensitive resin composition, method for producing patterned cured film, and electronic component

    JP2008033159A