Outdoor cooling safety helmet and preparation method thereof

By using efficient composite coating, modified ABS material and phase change buffer layer on the safety helmet, combined with the lining of the thermal gel, the problem of heat dissipation of helmets in high temperature environments is solved, and passive cooling without power is achieved High environmental adaptability improves safety performance and wear comfort.

CN119033183APending Publication Date: 2024-11-29GZ YASHANG TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411322562.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The lack of effective heat dissipation design in high-temperature environments makes it difficult for the internal heat of the helmet to dissipate, increasing the user's heat load. The common cooling helmet designs rely on power supply, and there are risks such as battery life and battery thermal runaway.

Method used

Using a power-free design, by applying a composite coating with high atmospheric window emissivity and high solar spectrum reflectivity on the surface of the helmet, the shell and inner liner use modified ABS material, the buffer layer uses phase change material, and the inner liner is combined Cotton and sponge materials, and thermal gel is provided on the lining surface to achieve passive cooling and high environmental adaptability.

Benefits of technology

It realizes the cooling effect without power supply, improves heat dissipation performance, enhances environmental adaptability and safety performance, reduces battery-related risks, and improves the wearer's comfort and freedom of movement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119033183A_ABST
    Figure CN119033183A_ABST
Patent Text Reader

Abstract

The invention discloses an outdoor cooling safety helmet and a preparation method thereof. The invention discloses an outdoor cooling safety helmet. The helmet structurally comprises a surface composite coating, a shell, a buffer layer, an inner container and a lining which are sequentially arranged from outside to inside, the surface composite coating contains coupling agent modified nanoparticles; the shell and the inner container are made of flaky aluminum oxide modified ABS (Acrylonitrile Butadiene Styrene); the buffer layer is made of a phase change material; the lining is made of cotton or sponge materials, and heat conduction gel is arranged on the inner surface of the lining. According to the outdoor cooling safety helmet, semiconductor refrigeration or fan forced ventilation and other design needing an additional power source are avoided, the endurance problem and the thermal runaway risk possibly caused by a battery, a controller and other components are reduced, the safety of the helmet is improved, the surface of the helmet is coated with the composite coating with the passive radiation refrigeration effect, and the service life of the helmet is prolonged. Most of sunlight can be reflected and mid-infrared radiation can be emitted, so that the surface of the helmet can achieve the highest cooling effect of 12 DEG C under the sunlight.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of helmet preparation, and in particular to an outdoor cooling safety helmet and a preparation method thereof. Background Art

[0002] In industries such as construction, electricity, mining and chemicals, the working environment is usually high-risk and the accident rate is high. These industries have long production cycles and complex working conditions, which pose severe challenges to the safety of practitioners. Safety helmets are an important piece of equipment to protect workers' heads from impacts, falling objects, electric shocks and corrosive liquids, and their role is indispensable. When working in high temperatures, the body's natural heat dissipation mechanism is limited, and it mainly relies on sweating to regulate body temperature. Increased solar radiation and possible windless or high-humidity environments further limit the evaporation of sweat, increase the risk of heat stroke, and cause workers to experience symptoms such as dizziness and palpitations, affecting their concentration and work efficiency, thereby increasing the probability of safety accidents.

[0003] At present, the mainstream design of safety helmets usually includes a hard shell, a buffer layer and an inner lining. The hard shell is mostly made of ABS plastic material to resist external impact. The buffer layer usually uses expanded polystyrene (EPS) or expanded polypropylene (EPP) materials, which can effectively absorb impact. The inner lining is mostly made of soft cotton or sponge materials to improve wearing comfort. Although existing safety helmets have reached certain standards in terms of impact resistance and wear resistance, the problem of thermal comfort in high temperature outdoor environments has not been effectively solved.

[0004] Traditional safety helmets lack effective heat dissipation designs, such as ventilation holes and heat dissipation materials. When working in a high-temperature environment, it is difficult for the heat inside the helmet to dissipate, which increases the user's heat load. High-temperature working environments are complex and changeable, and existing helmets often lack adaptability to different environmental factors, such as additional functions such as UV protection and rain protection. In addition, common cooling helmets are designed to cool the head based on semiconductor refrigeration or fan forced ventilation, but this design often adds additional components such as batteries and controllers, and there are additional risks such as battery life and battery thermal runaway.

[0005] Therefore, it is necessary to design an outdoor cooling safety helmet that does not require electricity consumption, so that the helmet has obvious passive cooling effect and high environmental adaptability effect. Summary of the invention

[0006] In view of the problem that the internal heat of existing safety helmets is difficult to dissipate when working in a high-temperature environment, the present invention provides an outdoor cooling safety helmet that does not require electricity consumption and a preparation method. The zero-electricity cooling safety helmet of the present invention is sequentially provided with a surface composite coating, an outer shell, a buffer layer, an inner liner, and an inner lining from the outside to the inside, wherein the function of the composite coating is to provide a high "atmospheric window" emissivity and a high solar spectrum reflectivity, a high ultraviolet reflection effect, and a waterproof function. The outer shell and the inner liner are made of modified ABS composite materials, which have higher thermal conductivity than ordinary ABS plastics. The buffer layer adopts a composite phase change material, and the inner lining adopts a combination of skin-friendly thermal conductive gel and cotton / sponge material.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A first aspect of the present invention provides an outdoor cooling safety helmet, the structure of the helmet comprising a surface composite coating, an outer shell, a buffer layer, an inner liner and an inner lining arranged in sequence from the outside to the inside;

[0009] The surface composite coating contains coupling agent modified nanoparticles;

[0010] The material of the shell and the liner is flaky alumina modified ABS;

[0011] The material of the buffer layer is phase change material;

[0012] The lining is made of cotton or sponge material, wherein the inner surface of the lining is provided with heat-conducting gel.

[0013] Preferably, the content of the coupling agent modified nanoparticles in the surface composite coating is 10-30wt%.

[0014] Further preferably, the raw materials for preparing the surface composite coating include 10-50wt% polymer, 30-50wt% organic solvent, 10-30wt% coupling agent modified nanoparticles, 2-10wt% interface agent, and 1-5wt% auxiliary agent.

[0015] In some specific preferred embodiments of the present invention, the polymer is at least one of polyethylene glycol, polyvinyl chloride, polyvinylidene fluoride-hexafluoropropylene, and polymethyl methacrylate; the organic solvent is at least one of acetone, cyclohexanone, dimethylformamide, dimethylacetamide, butanone, and benzene; the nanoparticles of the coupling agent-modified nanoparticles are at least one of ZnO, ZnO2, ZnS, CaF2, CaCO3, SiO2, TiO2, BaSO4, Fe2O3, CuO, PbCO3, MgCO3, MgO, BN, and Y2O3; the interfacial agent is at least one of an organic functional silane, chlorinated polypropylene, and a xylene mixed solution; the additive is at least one of a dispersant, a wetting agent, a defoamer, a leveling agent, an anti-cratering additive, and a film-forming additive. The organofunctional silanes described in the present invention include aminosilanes: γ-aminopropyltriethoxysilane (KH-550); epoxysilanes: γ-(2,3-epoxypropoxy)propyltrimethoxysilane (KH-560); methacryloxysilanes: γ-methacryloxypropyltrimethoxysilane (KH-570), etc.

[0016] Preferably, the coupling agent used in the coupling agent-modified nanoparticles is a silane coupling agent; in some specific embodiments of the present invention, the coupling agent used in the coupling agent-modified nanoparticles is a perfluorooctyltriethoxysilane coupling agent (C6). The present invention does not limit the amount of the coupling agent used in the coupling agent-modified nanoparticles.

[0017] Preferably, the content of flaky aluminum oxide in the flaky aluminum oxide modified ABS is 10-30wt%.

[0018] The flaky alumina modified ABS in the present invention is made by melt blending. For cooling helmets, it is not only necessary to have excellent thermal conductivity, but also to meet the comprehensive performance of safe use. The flaky alumina not only has excellent thermal conductivity, but also has a unique two-dimensional layer structure, which is easy to form a thermal conductive network inside the composite material, and has the advantages of low price, high strength, and good electrical insulation performance. However, due to the poor interface bonding ability between the flaky alumina and the ABS matrix, the surface is difficult to be wetted by the matrix, and it is easy to agglomerate in the matrix, which makes it difficult to disperse evenly, which not only affects the improvement of thermal conductivity, but also seriously reduces the mechanical properties. Therefore, it is necessary to surface treat the flaky alumina. The modifier for surface treatment of the flaky alumina in the present invention is at least one of stearic acid, silane coupling agent KH550, and titanate coupling agent. The present invention does not limit the specific amount of the modifier.

[0019] Preferably, the phase change material is silicon dioxide-coated sodium sulfate decahydrate phase change microcapsules.

[0020] Preferably, the phase change material is prepared by a preparation method comprising the following steps:

[0021] (1) taking a saturated aqueous solution of sodium sulfate, pouring it into a mixed solution of cyclohexane and n-butanol, adding sulfuric acid solution dropwise with stirring to adjust the pH value to 2.8-3.5, and continuing to stir to obtain a white emulsion;

[0022] (2) Take an aqueous solution of sodium silicate, add the white emulsion dropwise, stir, and then put the mixed solution into a microwave hydrothermal synthesizer. After the reaction is completed, take it out and let it stand to room temperature, centrifuge, wash and dry to obtain a composite phase change buffer layer material.

[0023] Further preferably, the parameters of the microwave hydrothermal synthesizer are: temperature 80-95°C, heating time 8-15min, and maximum heating power 250-300W.

[0024] A second aspect of the present invention provides a method for preparing the outdoor cooling safety helmet, comprising the following steps:

[0025] Preparation of surface composite coating: disperse nanoparticles in water, drop coupling agent, stir to obtain coupling agent modified nanoparticles; dissolve polymer and coupling agent modified nanoparticles in organic solvent, add interface agent and auxiliary agent, stir to obtain mixed slurry, dilute with water according to actual situation and apply on the helmet shell;

[0026] Preparation of a helmet shell and liner: drying flaky aluminum oxide, modifying the flaky aluminum oxide with a surface treatment agent, placing the modified flaky aluminum oxide and ABS in an oven for drying, mixing the dried ABS with the modified flaky aluminum oxide, adding the mixture to a torque rheometer to obtain a modified ABS material, placing the modified ABS material in a mold, and molding the helmet shell and liner;

[0027] Prepare phase change material for the buffer layer; prepare the lining of the helmet; assemble the outer shell, phase change buffer layer, liner and lining to obtain an outdoor cooling safety helmet.

[0028] Preferably, the surface treatment agent used in the modification process of the flaky aluminum oxide is at least one of stearic acid, silane coupling agent KH550, and titanate coupling agent.

[0029] Preferably, the ratio of the amount of the surface treatment agent used in the flaky aluminum oxide modification process to the amount of the flaky aluminum oxide used is 1:(3.5-4.5).

[0030] The heat-conducting gel provided in the inner liner of the present invention is a commercially available product, without any special specification, for example, a commercially available aluminum nitride heat-conducting silicone sheet can be used.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] 1. Cooling effect can be achieved without consuming electricity: Compared with ordinary cooling helmets, it avoids the use of semiconductor cooling or fan forced ventilation and other designs that require additional power, reduces the endurance problems and thermal runaway risks that may be caused by components such as batteries and controllers, and improves the safety of the helmet. A composite coating with passive radiation cooling effect is applied on the surface of the helmet, which can reflect most of the sunlight and emit mid-infrared radiation, so that the helmet surface can achieve a cooling effect of up to 12°C under the sun.

[0033] 2. Enhanced heat dissipation performance: Through the application of heat dissipation materials, the helmet can dissipate internal heat more effectively in high temperature environments and reduce the user's heat load.

[0034] 3. High environmental adaptability: The composite coating on the surface of the helmet has good self-cleaning, insulation, corrosion resistance and waterproof properties, etc., which enables the helmet to provide better protection in a changeable high-temperature working environment.

[0035] 4. Higher safety performance: By optimizing the materials, the helmet can reduce weight without sacrificing protective performance, thereby improving the wearer's comfort and freedom of movement. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a schematic diagram of the helmet shell;

[0037] Figure 2 This is a schematic diagram of the helmet liner;

[0038] Figure 3 This is a schematic diagram of the helmet lining;

[0039] Figure 4 This is the bottom view of the helmet;

[0040] Figure 5 This is a cross-sectional view of the helmet structure;

[0041] Figure 6 The cooling effect diagram of the helmet with and without the composite coating in Example 1 and Comparative Example 1;

[0042] In the attached figure, 1: helmet shell, 1-1: top vent, 1-2: shell reinforcement rib, 1-3: vent, 2: helmet liner, 2-1: liner reinforcement rib, 2-2 air vent, 3: helmet lining, 4: phase change buffer layer, 5: composite coating, 6: thermal conductive gel. DETAILED DESCRIPTION

[0043] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0044] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0045] Example 1

[0046] 1. Preparation of surface composite coating: The coating is composed of 30wt% polymer, 40wt% organic solvent, 20wt% additive, 5wt% interface agent, and 5wt% auxiliary agent. Polymer: polyvinylidene fluoride-hexafluoropropylene, organic solvent: a mixture of acetone and butanone, additive: modified nanoparticles (ZnO and TiO2), interface agent: organic functional silane, auxiliary agent: dispersant and film-forming auxiliary agent.

[0047] Nanoparticles (ZnO and TiO2, mass ratio 1:1) are uniformly dispersed in deionized water using ultrasonic equipment, and perfluorooctyl triethoxysilane coupling agent (C6) is slowly dripped in, the mass ratio of nanoparticles to modifier is 5-6:1, and modified by magnetic stirring for 24 hours at room temperature to obtain modified nanoparticles. Polyvinylidene fluoride-hexafluoropropylene (30%) and modified nanoparticles (20%) are dissolved in a mixed organic solvent (40%) of acetone and butanone, and organic functional silane interface agent (5%) and dispersant and film-forming aid (5%) are added, and magnetic stirring is used for 12 hours at room temperature to fully mix. When using, add 10% water for dilution and fix it on the helmet shell by spraying or brushing.

[0048] 2. Production of modified ABS helmet shell and liner: matrix: ABS (75%), filler: flaky aluminum oxide (20%), surface treatment agent: a mixture of stearic acid and titanate coupling agent CS-101 (5%).

[0049] The flaky alumina was dried in an oven at 150°C for 12 hours, and the flaky alumina was modified using stearic acid and titanate coupling agent CS-101. The modified flaky alumina and ABS were placed in an oven at 60°C and dried for 12 hours. The dried ABS and modified flaky alumina were mixed evenly using a high-speed multifunctional pulverizer, added to a torque rheometer, and kneaded for 10 minutes at a temperature of 220°C and a speed of 35r / min to obtain a modified ABS material. The modified ABS material was placed in a helmet mold, and the mold was placed in a vulcanizer. The molding temperature was 220°C and the pressure was 12Mpa, and the helmet shell and liner were molded.

[0050] 3. Preparation of composite phase change buffer layer materials: main phase change material: sodium sulfate decahydrate, precursor: sodium silicate.

[0051] Silica-coated sodium sulfate decahydrate phase change microcapsules were prepared by chemical precipitation method. The specific production process is as follows: put an appropriate amount of anhydrous sodium sulfate into a beaker, dissolve it with deionized water, and ultrasonically disperse it in an ultrasonic cleaner for 30 minutes to obtain a saturated sodium sulfate solution. In another beaker, add cyclohexane and n-butanol in a ratio of 5:1, stir it with a mechanical stirrer at a speed of 2200r / min, add an appropriate amount of saturated sodium sulfate solution, stir it at high speed for 1 hour, add sulfuric acid solution to the mixed solution, adjust the pH value of the mixed solution to 2.8-3.5, continue stirring for 3 hours, and obtain a white emulsion. Put an appropriate amount of sodium silicate in a beaker, dissolve it with deionized water, and continue stirring for 1 hour to obtain a watery transparent liquid. Use a peristaltic pump to adjust the drop speed to 2, slowly drop the sodium silicate solution into the white emulsion, and use a magnetic stirrer to stir during the drop addition process. Finally, the mixed solution was placed in a microwave hydrothermal synthesizer, the temperature was set to 80°C-95°C, the heating time was 8-15 minutes, and the maximum heating power was set to between 250W-300W. After the reaction was completed, it was taken out and allowed to stand at room temperature, centrifuged, washed with anhydrous ethanol and deionized water for 3 times, and dried to obtain a composite phase change buffer layer material.

[0052] 4. Assemble the prepared outer shell, phase change buffer layer, inner liner and lining to obtain an outdoor cooling safety helmet without electric refrigeration.

[0053] Example 2

[0054] 1. Preparation of surface composite coating: The coating is composed of 40wt% polymer, 35wt% organic solvent, 15wt% additive, 7wt% interface agent, and 3wt% auxiliary agent. Polymer: polymethyl methacrylate, organic solvent: a mixture of cyclohexanone and dimethylformamide, additive: modified nanoparticles (SiO2 and BaSO4), interface agent: a mixed solution of chlorinated polypropylene and xylene, auxiliary agents: a wetting agent and a thickening and leveling agent.

[0055] Nanoparticles (SiO2 and BaSO4, mass ratio 1:1) were uniformly dispersed in deionized water using ultrasonic equipment, and perfluorooctyl triethoxysilane coupling agent (C6) was slowly dripped in, and modified by magnetic stirring at room temperature for 24 hours to obtain modified nanoparticles. Polymethyl methacrylate (40%) and modified nanoparticles (15%) were dissolved in a mixed organic solvent (35%) of cyclohexanone and dimethylformamide, and a mixed solution of chlorinated polypropylene and xylene as an interface agent (7%) and a wetting agent and a thickening and leveling agent (3%) were added, and the mixture was fully mixed by magnetic stirring at room temperature for 12 hours. When using, 10% water was added for dilution, and fixed on the helmet shell by spraying or brushing.

[0056] 2. Production of modified ABS helmet shell and liner: matrix: ABS (70%), filler: flaky aluminum oxide (25%), surface treatment agent: silane coupling agent KH550 (5%).

[0057] The flaky alumina was dried in an oven at 150°C for 12 hours, and the flaky alumina was modified using a silane coupling agent KH550. The modified flaky alumina and ABS were placed in an oven at 60°C and dried for 12 hours. The dried ABS and the modified flaky alumina were mixed evenly using a high-speed multifunctional pulverizer, and then added to a torque rheometer. The modified ABS material was obtained by mixing for 10 minutes at a temperature of 220°C and a speed of 35r / min. The modified ABS material was placed in a helmet mold, and the mold was placed in a vulcanizer. The molding temperature was 220°C and the pressure was 12Mpa, and the helmet shell and liner were molded.

[0058] 3. Preparation of composite phase change buffer layer materials: main phase change material: sodium sulfate decahydrate, precursor: sodium silicate.

[0059] Silica-coated sodium sulfate decahydrate phase change microcapsules were prepared by chemical precipitation method. The specific production process is as follows: put an appropriate amount of anhydrous sodium sulfate into a beaker, dissolve it with deionized water, and ultrasonically disperse it in an ultrasonic cleaner for 30 minutes to obtain a saturated sodium sulfate solution. In another beaker, add cyclohexane and n-butanol in a ratio of 5:1, stir it with a mechanical stirrer at a speed of 2200r / min, add an appropriate amount of saturated sodium sulfate solution, stir it at high speed for 1 hour, add sulfuric acid solution to the mixed solution, adjust the pH value of the mixed solution to 2.8-3.5, continue stirring for 3 hours, and obtain a white emulsion. Put an appropriate amount of sodium silicate in a beaker, dissolve it with deionized water, and continue stirring for 1 hour to obtain a watery transparent liquid. Use a peristaltic pump to adjust the drop speed to 2, slowly drop the sodium silicate solution into the white emulsion, and stir it with a magnetic stirrer during the drop addition. Finally, put the mixed solution into a microwave hydrothermal synthesizer, set the temperature to 85℃, the heating time to 13 minutes, and the maximum heating power to between 260W. After the reaction is completed, the material is taken out and allowed to stand at room temperature, centrifuged, washed three times with anhydrous ethanol and deionized water, and dried to obtain a composite phase change buffer layer material.

[0060] 4. Assemble the prepared outer shell, phase change buffer layer, inner liner and lining to obtain an outdoor cooling safety helmet without electric refrigeration.

[0061] Example 3

[0062] 1. Preparation of surface composite coating: The coating is composed of 50wt% polymer, 25wt% organic solvent, 15wt% additive, 5wt% interface agent, and 5wt% auxiliary agent. Polymer: a mixture of polyethylene glycol and polyvinyl chloride, organic solvent: a mixture of acetone and benzene, additive: modified nanoparticles (Fe2O3 and MgCO3), interface agent: organic functional silane, auxiliary agent: defoamer and anti-shrinkage auxiliary agent.

[0063] Nanoparticles (Fe2O3 and MgCO3, mass ratio 1:1) were uniformly dispersed in deionized water using ultrasonic equipment, and perfluorooctyl triethoxysilane coupling agent (C6) was slowly dripped in, and modified by magnetic stirring for 24 hours at room temperature to obtain modified nanoparticles. Polyethylene glycol and polyvinyl chloride (50%) and modified nanoparticles (15%) were dissolved in a mixed organic solvent (25%) of acetone and benzene (volume ratio 1:1), and organic functional silane interface agent (5%) and defoamer and anti-shrinkage crater additive (5%) were added, and magnetic stirring was used for 12 hours at room temperature to fully mix. When using, 10% water was added for dilution, and fixed on the helmet shell by spraying or brushing.

[0064] 2. Production of modified ABS helmet shell and liner: matrix: ABS (80%), filler: flaky aluminum oxide (20%), surface treatment agent: stearic acid (5%).

[0065] The flaky alumina was dried in an oven at 150°C for 12 hours, and the flaky alumina was modified with stearic acid. The modified flaky alumina and ABS were placed in an oven at 60°C and dried for 12 hours. The dried ABS and modified flaky alumina were mixed evenly using a high-speed multifunctional pulverizer, and then added to a torque rheometer. The modified ABS material was obtained by mixing for 10 minutes at a temperature of 220°C and a speed of 35r / min. The modified ABS material was placed in a helmet mold, and the mold was placed in a vulcanizer. The molding temperature was 220°C and the pressure was 12Mpa, and the helmet shell and liner were molded.

[0066] 3. Preparation of composite phase change buffer layer materials: main phase change material: sodium sulfate decahydrate, precursor: sodium silicate.

[0067] Silica-coated sodium sulfate decahydrate phase change microcapsules were prepared by chemical precipitation method. The specific production process is as follows: put an appropriate amount of anhydrous sodium sulfate into a beaker, dissolve it with deionized water, and ultrasonically disperse it in an ultrasonic cleaner for 30 minutes to obtain a saturated sodium sulfate solution. In another beaker, add cyclohexane and n-butanol in a ratio of 5:1, stir it with a mechanical stirrer at a speed of 2200r / min, add an appropriate amount of saturated sodium sulfate solution, stir it at high speed for 1 hour, add sulfuric acid solution to the mixed solution, adjust the pH value of the mixed solution to 2.8-3.5, continue stirring for 3 hours, and obtain a white emulsion. Put an appropriate amount of sodium silicate in a beaker, dissolve it with deionized water, and continue stirring for 1 hour to obtain a watery transparent liquid. Use a peristaltic pump to adjust the drop speed to 2, slowly drop the sodium silicate solution into the white emulsion, and stir it with a magnetic stirrer during the drop addition process. Finally, put the mixed solution into a microwave hydrothermal synthesizer, set the temperature to 90℃, the heating time to 14 minutes, and the maximum heating power to between 270W. After the reaction is completed, the material is taken out and allowed to stand at room temperature, centrifuged, washed three times with anhydrous ethanol and deionized water, and dried to obtain a composite phase change buffer layer material.

[0068] 4. Assemble the prepared outer shell, phase change buffer layer, inner liner and lining to obtain an outdoor cooling safety helmet without electric refrigeration.

[0069] Comparative Example 1

[0070] On the basis of Example 1, a comparative example without a surface composite coating was set up to test the cooling effects of the helmets of Example 1 and Comparative Example 1. The results are shown in the attached figure. Figure 6 shown.

[0071] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. An outdoor cooling safety helmet, It is characterized in that The structure of the helmet includes a surface composite coating, an outer shell, a buffer layer, an inner liner and an inner lining which are arranged in sequence from the outside to the inside; The surface composite coating contains coupling agent modified nanoparticles; The material of the shell and the liner is flaky alumina modified ABS; The material of the buffer layer is phase change material; The lining is made of cotton or sponge material, wherein the inner surface of the lining is provided with heat-conducting gel.

2. The outdoor cooling safety helmet according to claim 1, It is characterized in that The content of the coupling agent modified nanoparticles in the surface composite coating is 10-30wt%.

3. The outdoor cooling safety helmet according to claim 2, It is characterized in that The raw materials for preparing the surface composite coating include 10-50wt% of polymer, 30-50wt% of organic solvent, 10-30wt% of coupling agent modified nanoparticles, 2-10wt% of interface agent and 1-5wt% of auxiliary agent.

4. The outdoor cooling safety helmet according to claim 3, It is characterized in that The polymer is at least one of polyethylene glycol, polyvinyl chloride, polyvinylidene fluoride-hexafluoropropylene, and polymethyl methacrylate; the organic solvent is at least one of acetone, cyclohexanone, dimethylformamide, dimethylacetamide, butanone, and benzene; the nanoparticles of the coupling agent-modified nanoparticles are ZnO, ZnO 2 、ZnS、CaF 2 、CaCO 3 、SiO 2 、TiO 2 ,BaSO 4 , Fe 2 O 3 ,CuO,PbCO 3 MgCO 3 ,MgO,BN,Y 2 O 3 At least one of the following: the interfacial agent is at least one of an organic functional silane, a chlorinated polypropylene and a xylene mixed solution; the auxiliary agent is at least one of a dispersant, a wetting agent, a defoamer, a leveling agent, an anti-shrinkage cratering agent and a film-forming agent.

5. The outdoor cooling safety helmet according to claim 1, It is characterized in that The content of flaky aluminum oxide in the flaky aluminum oxide modified ABS is 10-30wt%.

6. The outdoor cooling safety helmet according to claim 1, It is characterized in that The phase change material is a silicon dioxide-coated sodium sulfate decahydrate phase change microcapsule.

7. The outdoor cooling safety helmet according to claim 6, It is characterized in that The phase change material is prepared by a preparation method comprising the following steps: (1) taking a saturated aqueous solution of sodium sulfate, pouring it into a mixed solution of cyclohexane and n-butanol, adding sulfuric acid solution dropwise with stirring to adjust the pH value to 2.8-3.5, and continuing to stir to obtain a white emulsion; (2) Take an aqueous solution of sodium silicate, add the white emulsion dropwise, stir, and then put the mixed solution into a microwave hydrothermal synthesizer. After the reaction is completed, take it out and let it stand to room temperature, centrifuge, wash and dry to obtain a composite phase change buffer layer material.

8. The outdoor cooling safety helmet according to claim 7, It is characterized in that The parameters of the microwave hydrothermal synthesizer are: temperature 80-95°C, heating time 8-15min, and maximum heating power 250-300W.

9. A method for preparing the outdoor cooling safety helmet according to any one of claims 1 to 8, It is characterized in that The following steps are involved: Preparation of surface composite coating: disperse nanoparticles in water, drop coupling agent, stir to obtain coupling agent modified nanoparticles; dissolve polymer and coupling agent modified nanoparticles in organic solvent, add interface agent and auxiliary agent, stir to obtain mixed slurry, dilute with water according to actual situation and apply on the helmet shell; Preparation of a helmet shell and liner: drying flaky aluminum oxide, modifying the flaky aluminum oxide with a surface treatment agent, placing the modified flaky aluminum oxide and ABS in an oven for drying, mixing the dried ABS with the modified flaky aluminum oxide, adding the mixture to a torque rheometer to obtain a modified ABS material, placing the modified ABS material in a mold, and molding the helmet shell and liner; Prepare phase change material for the buffer layer; prepare the lining of the helmet; assemble the outer shell, phase change buffer layer, liner and lining to obtain an outdoor cooling safety helmet.

10. The method for preparing the outdoor cooling safety helmet according to claim 9, It is characterized in that The surface treatment agent used in the modification process of the flaky aluminum oxide is at least one of stearic acid, silane coupling agent KH550, and titanate coupling agent.