Organic silicon emulsion defoaming agent and preparation method thereof
By adding piperazine block modified silicone oil and glucolactone modified polysiloxane to the silicone defoamer, the problem of poor compatibility of defoamer in laundry detergent is solved, and better defoaming effect is achieved and efficient production.
Patent Information
- Application Number
- CN202411460747.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2024-11-29
AI Technical Summary
The existing laundry detergent defoaming agent has poor compatibility with laundry detergent, which leads to difficulty in controlling foam during the washing process, affecting the washing effect and water resource utilization efficiency.
Add piperazine block modified silicone oil and glucolactone modified polysiloxane as a co-emulsifier to the traditional silicone defoamer formulation to optimize their mass ratio to improve dispersion and surfactivity properties to form organic Silicone emulsion defoaming agent.
It significantly improves the compatibility and defoaming properties of defoamers in laundry detergent, simplifies the preparation process, reduces production costs, and is suitable for large-scale production.
Smart Images

Figure SMS_1 
Figure SMS_5 
Figure SMS_12
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fine chemicals, and specifically relates to an emulsion-type defoaming agent containing organic silicon and modified organic silicon and a preparation method thereof. Background Art
[0002] Defoamers are widely used in various fields and are closely related to people's food, clothing, housing and transportation. Defoamers are used in papermaking, textile, coating, ink, daily chemical, food and other industries. The application scenarios of defoamers in each industry are different, and the requirements for defoamers are also different. For example, the pulping of the papermaking industry requires the alkali resistance of the defoamer; the printing and dyeing process of the textile industry requires the defoamer not only to be alkali-resistant, but also to be resistant to high temperatures; the defoamer in the coating and ink industry must have good compatibility while eliminating and suppressing foam; the defoamer in the daily chemical industry's washing powder has the requirements for foam control in the rinsing stage and the need to eliminate foam in the drainage stage; the food industry has requirements for the defoamer preparation environment, and so on.
[0003] Many industries have requirements for the foam suppression performance of defoamers. For example, in the process of hand washing and machine washing in the daily chemical industry, people generally believe that foam can provide a better hand feel during hand washing. During machine washing, foam can provide better cleaning ability. Of course, there are literatures pointing out that the cleaning ability is not closely related to the amount of foam.
[0004] The literature "Preparation of polyether polysiloxane defoamer and its application in liquid detergent" points out that the use of polyether modified siloxane as a defoamer active substance has a good effect in defoaming. Patent CN 102698475 A points out the use of alkyl modified siloxane in the laundry powder industry. Patent CN 102307978 A points out the introduction of aromatic groups into organosilicon active substances to prepare defoamers and use them in detergents. The paper "Research on the formulation and process of a soap-based concentrated laundry detergent" points out that polyether modified organosiloxane has a certain effect in defoaming, and hydrogenated coconut oil potassium soap has a better effect. Some literature points out that soaps have an impact on cleaning ability.
[0005] Laundry detergent defoaming agent is a special type of chemical additive used to control and eliminate the foam generated by laundry detergent during the washing process. The generation of foam not only affects the washing effect, but may also cause the washing machine to overflow, increase the number of rinses and waste water resources. The use of silicone emulsion defoaming agent can improve washing efficiency, reduce rinsing time and save water resources.
[0006] In non-structured detergents, existing laundry detergent defoamers have poor compatibility with laundry detergent. If a slightly larger amount is added, the transparency of the laundry detergent will be affected. However, if the amount of defoamer added is insufficient, the defoaming effect of the laundry detergent cannot be guaranteed.
[0007] Therefore, it is necessary to develop a new silicone laundry detergent defoamer to solve the above problems. Summary of the invention
[0008] In view of this, the purpose of the present application is to provide a silicone emulsion defoamer and a preparation method thereof. The silicone emulsion defoamer is a traditional silicone defoamer formula, in which modified silicone siloxanes such as gluconolactone-modified polysiloxane B2 and piperazine block-modified silicone oil B1 are added as co-emulsifiers, which can significantly improve its dispersibility in laundry detergent, thereby improving its compatibility and ensuring excellent defoaming performance.
[0009] In order to achieve or at least partially achieve the above objectives, the present application provides the following technical solutions:
[0010] In a first aspect, the present application provides a silicone emulsion defoamer, comprising the following components in parts by mass:
[0011] Component A: 5 to 10 parts of silicone active material;
[0012] Component B: 5 to 10 parts of modified organosiloxane;
[0013] Component C: 2 to 5 parts of emulsifier;
[0014] Component D: 0.5 to 3 parts of thickener;
[0015] Component E: 77 to 82.5 parts of deionized water.
[0016] Furthermore, the organosilicon active material includes hydrogen-containing polysiloxane A1, vinyl-terminated methylphenyl polysiloxane A2, and silicon dioxide A3.
[0017] Furthermore, the modified organic siloxane includes piperazine block modified silicone oil B1 and gluconolactone modified polysiloxane B2, and the chemical structure of the piperazine block modified silicone oil B1 is as shown in formula (1):
[0018] As shown, wherein the chemical structure of R1 is as shown in formula (2): As shown, the chemical structure of R2 is as shown in formula (3): As shown, a, b, c, d are integers of 1 to 30; the chemical structural formula of the gluconolactone-modified polysiloxane is as shown in formula (4): As shown, group R3 is a reactive group or an inert group, the inert group is selected from at least one of methyl, cyclohexyl, cyclopentyl, and phenyl, and the reactive group is selected from at least one of hydrogen, vinyl, hydroxyl, epoxy, and amino; groups R4 and R5 are divalent C1-C18 hydrocarbon groups; m and n are integers of 1-1000.
[0019] Furthermore, in the modified organic siloxane, the mass ratio of piperazine block modified silicone oil B1 to gluconolactone modified polysiloxane B2 is 3-5:9-22.
[0020] In a second aspect, the present application also provides a method for preparing the aforementioned silicone emulsion defoamer, the steps of which include:
[0021] S1. preparing organosilicon active substances and preparing modified organosiloxanes;
[0022] S2. Take the organosilicon active substance, modified organosiloxane, emulsifier, thickener and deionized water according to mass parts and set aside;
[0023] S3, mixing the organosilicon active substance, modified organosiloxane and emulsifier uniformly to obtain a first mixed solution;
[0024] S4, adding half of the deionized water to the first mixed solution in sequence, then adding a thickener, and stirring evenly to obtain a second mixed solution;
[0025] S5. Add the remaining deionized water to the second mixed solution and stir evenly to obtain the organosilicon emulsion defoamer.
[0026] The present invention provides a silicone emulsion defoamer and a preparation method thereof, which, compared with the prior art, has at least the following beneficial effects:
[0027] 1. The organosilicon emulsion defoamer provided in the present application is based on the traditional organosilicon defoamer formula, and modified siloxanes such as piperazine block modified silicone oil and gluconolactone modified polysiloxane are added as co-emulsifiers, wherein the piperazine block modified silicone oil and gluconolactone modified polysiloxane both have a large number of hydrophilic groups and hydrophobic groups. By optimizing the mass ratio of the piperazine block modified silicone oil and the gluconolactone modified polysiloxane, the hydrophilic and lipophilic HLB values of the defoamer are adjusted, thereby increasing its dispersion performance in water; at the same time, in addition to being co-emulsifiers, the piperazine block modified silicone oil and the gluconolactone modified polysiloxane themselves also have the function of a surfactant, thereby achieving a more excellent defoaming effect.
[0028] 2. The preparation method of the organosilicon emulsion defoamer provided in the present application is simple to operate, convenient to control, has high production efficiency, low production cost, and is suitable for large-scale production. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.
[0030] Those skilled in the art will appreciate that, unless otherwise stated, the "said", "the", and "the aforementioned" used in the text of the present application may also include plural forms. It should be further understood that the term "comprising" used in the specification of the present application means the presence of the features, steps, and operations, but does not exclude the presence or addition of one or more other features, integers, and steps.
[0031] In the text of this application, the terms "first", "second" and the like are used to distinguish between identical or similar items with substantially the same functions and effects. This is only for the purpose of clearly describing the technical solutions of the embodiments of this application, and shall not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features.
[0032] In the present application, the term "normal temperature" refers to room temperature or general temperature, for example, the temperature range may be 15 to 25°C.
[0033] In view of the problems of the prior art, the embodiments of the present application have improved the existing organic silicon defoamer composition formula to obtain a new type of organic silicon emulsion defoamer, which adds modified siloxanes such as gluconolactone modified polysiloxane B2 and piperazine block modified silicone oil B1 as auxiliary emulsifiers. Both have rich hydrophilic and hydrophobic genes. By optimizing the mass ratio of the two, the dispersibility of the defoamer in the laundry detergent can be improved and the compatibility can be improved; gluconolactone modified polysiloxane B2 and piperazine block modified silicone oil B1 can also be used as excellent surfactants to ensure that the defoamer has a better defoaming ability. At the same time, the components of the organic silicon emulsion defoamer are simpler than those of the existing defoamers. In the preparation process of the organic silicon emulsion defoamer, the purpose of high production efficiency, low production cost and large-scale production can be achieved.
[0034] Based on this, the present application embodiment provides a silicone emulsion defoamer, which includes the following components in parts by mass:
[0035] Component A: 5 to 10 parts of organosilicon active material; Component B: 5 to 10 parts of modified organosiloxane; Component C: 2 to 5 parts of emulsifier; Component D: 0.5 to 3 parts of thickener; Component E: 77 to 82.5 parts of deionized water.
[0036] In certain embodiments, the organosilicon active material includes hydrogen-containing polysiloxane A1, vinyl-terminated methylphenyl polysiloxane A2, and silicon dioxide A3.
[0037] In certain embodiments, in the organosilicon active material, the molar ratio of the hydrogen-containing polysiloxane A1 to the vinyl-terminated methylphenyl polysiloxane A2 is 1:1-1.5; and the mass proportion of the silicon dioxide A3 in the organosilicon active material is 3%-6%.
[0038] In certain preferred embodiments, the molar ratio of the hydrogen-containing polysiloxane A1 to the vinyl-terminated methylphenyl polysiloxane A2 is 1:1.2; and the mass proportion of the silicon dioxide A3 in the organic silicon active material is 5%.
[0039] In certain embodiments, the specific steps of the preparation process of the organosilicon active material are as follows: hydrogen-containing polysiloxane A1, vinyl-terminated methylphenyl polysiloxane A2, and silicon dioxide A3 are put into a reaction kettle, the dispersion disk is turned on, and they are fully stirred. After stirring evenly, the temperature is raised to between 40 and 100° C., a platinum catalyst is added, and the temperature is continued to be raised to 120 to 200° C. for insulation. After insulation for 1 hour, the temperature is naturally lowered.
[0040] In the examples of the present application, the modified organic siloxane includes piperazine block modified silicone oil B1 and gluconolactone modified polysiloxane B2.
[0041] In certain embodiments, the chemical structure of the piperazine block-modified silicone oil B1 is as shown in formula (1):
[0042] As shown, wherein the chemical structure of R1 is as shown in formula (2): As shown, the chemical structure of R2 is as shown in formula (3): As shown, a, b, c, d are integers of 1 to 30. In these embodiments, the piperazine block-modified silicone oil B1 is represented by formula (5): The polyether-terminated epoxy silicone oil shown in formula (6): The N-aminoethylpiperazine shown is produced by reaction, and the specific method is: polyether-terminated epoxy silicone oil and N-aminoethylpiperazine are placed in a reaction kettle equipped with a stirrer, a thermometer and a reflux condenser, and the reaction is kept warm for 3 to 6 hours.
[0043] In certain embodiments, the chemical structure of the gluconolactone-modified polysiloxane is as shown in Formula (4): As shown, the group R3 is a reactive group or an inert group, the inert group is selected from at least one of methyl, cyclohexyl, cyclopentyl, and phenyl, the reactive group is selected from at least one of hydrogen, vinyl, hydroxyl, epoxy, and amino, the groups R3 at both ends can be selected from the same group or different groups, and there is no specific limitation here; the groups R4 and R5 are divalent C1-C18 hydrocarbon groups; m and n are integers of 1-1000.
[0044] In certain preferred embodiments, the group R3 is selected from any one of methyl, hydroxyl and phenyl.
[0045] In certain preferred embodiments, the groups R4 and R5 are 1,2-vinylene (chemical structure as shown in Formula 7: shown).
[0046] In certain preferred embodiments, in formula (4), m and n are 2 or 3.
[0047] In some embodiments, in the modified organosiloxane, the mass ratio of piperazine block modified silicone oil B1 to gluconolactone modified polysiloxane B2 is 3-5:9-22. In some preferred embodiments, the mass ratio of piperazine block modified silicone oil B1 to gluconolactone modified polysiloxane B2 is 5:20.
[0048] In certain embodiments, the emulsifier is a carbon chain emulsifier, and the carbon chain emulsifier is at least two of sorbitan monostearate (S-60), sorbitan monooleate (S-80), sorbitan tristearate (S-65), sorbitan monooleate polyoxyethylene ether ester (T-80), sorbitan tristearate polyoxyethylene ether ester (T-65), fatty alcohol polyoxyethylene ether (AEO-2, AEO-3, AEO-5, AEO-7, AEO-9), castor oil polyoxyethylene ether, alkylphenol polyoxyethylene ether, and glyceryl monostearate.
[0049] In certain embodiments, the thickener is an acrylic acid alkali swelling thickener, and main components thereof include acrylic acid and sodium acrylate.
[0050] Based on this, the embodiment of the present application also provides a method for preparing a silicone emulsion defoamer, the steps of which include: S1, preparing silicone actives and preparing modified silicone siloxanes; S2, taking silicone actives, modified silicone siloxanes, emulsifiers, thickeners, and deionized water in parts by mass for later use; S3, mixing the silicone actives, modified silicone siloxanes, and emulsifiers to obtain a first mixed solution; S4, adding half of the deionized water to the first mixed solution in sequence, and then adding the thickener, stirring evenly to obtain a second mixed solution; S5, adding the remaining deionized water to the second mixed solution, stirring evenly to obtain the silicone emulsion defoamer.
[0051] In certain embodiments, the modified organosiloxane in S1 includes piperazine block modified silicone oil B1 and gluconolactone modified polysiloxane B2, wherein the chemical structure of the piperazine block modified silicone oil B1 is as shown in formula (1):
[0052] As shown, wherein the chemical structure of R1 is as shown in formula (2): As shown, the chemical structure of R2 is as shown in formula (3): As shown, a, b, c, and d are integers ranging from 1 to 30.
[0053] In certain preferred embodiments, the chemical structure of the gluconolactone-modified polysiloxane B2 is as shown in Formula (8): As shown, the group R3 is a reactive group or an inert group, the inert group is selected from at least one of methyl, cyclohexyl, cyclopentyl, and phenyl, the reactive group is selected from at least one of hydrogen, vinyl, hydroxyl, epoxy, and amino, the groups R3 at both ends can be selected from the same group or different groups, and there is no specific limitation here; the groups R4 and R5 are divalent C1-C18 hydrocarbon groups.
[0054] In a more preferred embodiment, the chemical structure of the gluconolactone-modified polysiloxane B2 is as shown in Formula (9): As shown, wherein the groups R4 and R5 are 1,2-vinylene, and the chemical structure is as shown in formula (7): shown.
[0055] In certain embodiments, in S3, the mixing temperature is 5-40°C.
[0056] The technical scheme of the present application and the technical effects achieved are described in detail below through more specific examples. The raw material compounds involved in the examples of the present application can be purchased from a regular commodity market or obtained by chemical synthesis in a laboratory.
[0057] Example 1
[0058] This embodiment provides a method for preparing a silicone emulsion defoamer, and the specific steps are:
[0059] (1) preparing an organosilicon active material according to the aforementioned method, wherein the molar ratio of the hydrogen-containing polysiloxane A1 to the vinyl-terminated methylphenyl polysiloxane A2 is 1:1.2; and the mass proportion of the silicon dioxide A3 in the organosilicon active material is 5%;
[0060] (2) Prepare modified organosiloxane according to the above method. First, prepare piperazine block modified silicone oil B1: weigh 0.2 mol of polyether-terminated epoxy silicone oil, whose chemical structure is as follows: As shown, the chemical structure of R1 is The chemical structure of R2 is Weigh 0.2 mol of N-aminoethylpiperazine (chemical formula: ), polyether-terminated epoxy silicone oil and N-aminoethyl piperazine were placed in a reactor equipped with a stirrer, a thermometer and a reflux condenser, and the reaction was kept warm for 6 hours to obtain piperazine block-modified silicone oil B1; gluconolactone-modified polysiloxane B2 was prepared, and its chemical structure is Wherein, the groups R4 and R5 are 1,2-vinylene (chemical structure: ); take 5g piperazine block modified silicone oil B1, 20g gluconolactone modified polysiloxane B2 mixed to prepare a modified organosiloxane, set aside;
[0061] (3) Weigh 8 g of organosilicon active material, 8 g of modified organosiloxane, 1.5 g of sorbitan monostearate (S-60), and 1.5 g of sorbitan tristearate polyoxyethylene ether ester (T-65), mix them evenly, and keep the temperature at 5 to 40° C. to obtain a first mixed solution;
[0062] (4) adding 40 g of deionized water and 1 g of an acrylic acid alkali-swellable thickener to the first mixed solution, mixing and stirring to form a fluid liquid, thereby obtaining a second mixed solution;
[0063] (5) Add 40 g of deionized water to the second mixed solution and mix well to obtain the organosilicon emulsion defoamer L1.
[0064] Example 2
[0065] This embodiment provides a method for preparing a silicone emulsion defoamer, and the specific steps are:
[0066] (1) preparing an organosilicon active material according to the aforementioned method, wherein the molar ratio of the hydrogen-containing polysiloxane A1 to the vinyl-terminated methylphenyl polysiloxane A2 is 1:1.2; and the mass proportion of the silicon dioxide A3 in the organosilicon active material is 5%;
[0067] (2) Prepare modified organosiloxane according to the above method. First, prepare piperazine block modified silicone oil B1: weigh 0.2 mol of polyether-terminated epoxy silicone oil, whose chemical structure is as follows: As shown, the chemical structure of R1 is The chemical structure of R2 is Weigh 0.2 mol of N-aminoethylpiperazine (chemical formula: ), polyether-terminated epoxy silicone oil and N-aminoethyl piperazine were placed in a reactor equipped with a stirrer, a thermometer and a reflux condenser, and the reaction was kept warm for 6 hours to obtain piperazine block-modified silicone oil B1; gluconolactone-modified polysiloxane B2 was prepared, and its chemical structure is Wherein, the groups R4 and R5 are 1,2-vinylene (chemical structure: ); take 3g piperazine block modified silicone oil B1, 22g gluconolactone modified polysiloxane B2 mixed to prepare modified organosiloxane B2, set aside;
[0068] (3) Weigh 5 g of organosilicon active material, 10 g of modified organosiloxane, 1 g of sorbitan monostearate (S-60), and 1 g of AEO-9 and mix them evenly, maintaining the temperature at 5 to 40° C. to obtain a first mixed solution;
[0069] (4) adding 40 g of deionized water and 0.5 g of an acrylic acid alkali-swellable thickener to the first mixed solution, and then stirring the mixture to form a fluid liquid to obtain a second mixed solution;
[0070] (5) Add 40 g of deionized water to the second mixed solution and mix well to obtain the organosilicon emulsion defoamer L2.
[0071] Example 3
[0072] This embodiment provides a method for preparing a silicone emulsion defoamer, and the specific steps are:
[0073] (1) preparing an organosilicon active material according to the aforementioned method, wherein the molar ratio of the hydrogen-containing polysiloxane A1 to the vinyl-terminated methylphenyl polysiloxane A2 is 1:1.2; and the mass proportion of the silicon dioxide A3 in the organosilicon active material is 5%;
[0074] (2) Prepare modified organosiloxane according to the above method. First, prepare piperazine block modified silicone oil B1: weigh 0.2 mol of polyether-terminated epoxy silicone oil, whose chemical structure is as follows: As shown, the chemical structure of R1 is The chemical structure of R2 is Weigh 0.2 mol of N-aminoethylpiperazine (chemical formula: ), polyether-terminated epoxy silicone oil and N-aminoethyl piperazine were placed in a reactor equipped with a stirrer, a thermometer and a reflux condenser, and the reaction was kept warm for 6 hours to obtain piperazine block-modified silicone oil B1; gluconolactone-modified polysiloxane B2 was prepared, and its chemical structure is Wherein, the groups R4 and R5 are 1,2-vinylene (chemical structure: ); Take 4g piperazine block modified silicone oil B1, 9g gluconolactone modified polysiloxane B2 mixed to prepare a modified organosiloxane, set aside;
[0075] (3) Weigh 10 g of organosilicon active material, 5 g of modified organosiloxane, 1 g of sorbitan monostearate (S-60), and 1 g of AEO-7, mix them evenly, and keep the temperature at 5 to 40° C. to obtain a first mixed solution;
[0076] (4) adding 40 g of deionized water and 1.5 g of an acrylic acid alkali-swellable thickener to the first mixed solution, mixing and stirring to form a fluid liquid, thereby obtaining a second mixed solution;
[0077] (5) Add 40 g of deionized water to the second mixed solution and mix well to obtain the organosilicon emulsion defoamer L3.
[0078] Comparative Example 1
[0079] This comparative example provides a method for preparing a silicone defoamer, and the specific steps are as follows:
[0080] (1) preparing an organosilicon active material according to the aforementioned method, wherein the molar ratio of the hydrogen-containing polysiloxane A1 to the vinyl polysiloxane A2 is 1:1.2; and the mass proportion of the silicon dioxide A3 in the organosilicon active material is 5%;
[0081] (2) Weigh 8 g of organosilicon active material, 1.5 g of sorbitan monostearate (S-60), and 1.5 g of sorbitan tristearate polyoxyethylene ether ester (T-65), mix them evenly, and keep the temperature at 5 to 40° C. to obtain a first mixed solution;
[0082] (3) adding 40 g of deionized water and 1 g of an acrylic acid alkali-swellable thickener to the first mixed solution, mixing and stirring to form a fluid liquid, thereby obtaining a second mixed solution;
[0083] (4) Add 40 g of deionized water to the second mixed solution and mix well to obtain the organosilicon emulsion defoamer L4.
[0084] Comparative Example 2
[0085] This comparative example provides a method for preparing a silicone emulsion defoamer, and the specific steps are:
[0086] (1) preparing an organosilicon active material according to the aforementioned method, wherein the molar ratio of the hydrogen-containing polysiloxane A1 to the vinyl-terminated methylphenyl polysiloxane A2 is 1:1.2; and the mass proportion of the silicon dioxide A3 in the organosilicon active material is 5%;
[0087] (2) Preparation of piperazine block modified silicone oil B1: Weigh 0.2 mol of polyether-terminated epoxy silicone oil, whose chemical structure is as follows: As shown, the chemical structure of R1 is The chemical structure of R2 is Weigh 0.2 mol of N-aminoethylpiperazine (chemical formula: ), placing polyether-terminated epoxy silicone oil and N-aminoethyl piperazine in a reaction kettle equipped with a stirrer, a thermometer and a reflux condenser, and reacting at this temperature for 6 hours to obtain piperazine block-modified silicone oil B1; set aside;
[0088] (3) Weigh 8 g of organic silicon active material, 8 g of piperazine block modified silicone oil B1, 1.5 g of sorbitan monostearate (S-60), and 1.5 g of sorbitan tristearate polyoxyethylene ether ester (T-65), mix them evenly, and keep the temperature at 5 to 40° C. to obtain a first mixed solution;
[0089] (4) adding 40 g of deionized water and 1 g of an acrylic acid alkali-swellable thickener to the first mixed solution, mixing and stirring to form a fluid liquid, thereby obtaining a second mixed solution;
[0090] (5) Add 40 g of deionized water to the second mixed solution and mix well to obtain the organosilicon emulsion defoamer L5.
[0091] Comparative Example 3
[0092] This comparative example provides a method for preparing a silicone emulsion defoamer, and the specific steps are:
[0093] (1) preparing an organosilicon active material according to the aforementioned method, wherein the molar ratio of the hydrogen-containing polysiloxane A1 to the vinyl-terminated methylphenyl polysiloxane A2 is 1:1.2; and the mass proportion of the silicon dioxide A3 in the organosilicon active material is 5%;
[0094] (2) Take 8 g of gluconolactone-modified polysiloxane B2 (chemical formula is the same as in Example 1) and set aside;
[0095] (3) Weigh 8 g of organosilicon active material, 8 g of gluconolactone modified polysiloxane B2, 1.5 g of sorbitan monostearate (S-60), and 1.5 g of sorbitan tristearate polyoxyethylene ether ester (T-65), mix them evenly, and keep the temperature at 5 to 40° C. to obtain a first mixed solution;
[0096] (4) adding 40 g of deionized water and 1 g of an acrylic acid alkali-swellable thickener to the first mixed solution, mixing and stirring to form a fluid liquid, thereby obtaining a second mixed solution;
[0097] (5) Add 40 g of deionized water to the second mixed solution and mix well to obtain the silicone emulsion defoamer L6.
[0098] Comparative Example 4
[0099] This comparative example provides a defoamer L7 configured with reference to the formula of a commercially available silicone defoamer. The defoamer mainly consists of: 80g deionized water, 8g polydimethylsiloxane, 1g polyoxyethylene sorbitan monostearate (Tween 60), 1g diglycerol fatty acid ester, 0.4g silicon dioxide A3, 1g sorbitan monostearate (Span 60), and 1g sodium carboxymethyl cellulose.
[0100] The compatibility and defoaming performance of the defoamers L1 to L7 prepared in the above examples and comparative examples were tested in laundry detergent, and the specific testing methods are as follows:
[0101] (1) preparing laundry detergent, the specific steps are as follows: preparing raw materials according to the formula in Table 1 below, ensuring that the purity and quality of the raw materials meet the requirements; adding a certain amount of water to a mixing tank; gradually adding sodium alkylbenzene sulfonate and AES, and dissolving them under low-speed stirring; adding liquid caustic soda, AEO-9, acrylic acid alkali swelling type thickener, essence, and kasone, and continuing to stir until completely dissolved; adding acrylic acid alkali swelling type thickener, adjusting the stirring speed to ensure uniform mixing; adjusting the pH value: using a pH meter to measure the pH value of the solution, and using an acid or base (such as citric acid or sodium hydroxide) to adjust it to a range of 7 to 9;
[0102] Table 1
[0103]
[0104] (2) Compatibility test: Take 250g of laundry detergent, add 3g of defoamers L1 to L7 respectively, stir magnetically for 15min, and let stand for 2h to compare the presence of obvious floating matter or floccules in each defoaming system; observe the appearance under natural light to determine whether it is transparent, foggy, or turbid;
[0105] (3) Defoaming performance test: 100 g of laundry detergent was added to a sample bottle, and 1 g of defoaming agent L1 to L7 was added respectively. The bottle was capped and the sample bottle was vertically shaken up and down 20 times at a frequency of 2 times / s and an amplitude of (30 to 35) cm. The sample bottle was allowed to stand and a stopwatch was used to record the time required to eliminate the foam.
[0106] The compatibility test and defoaming performance test results are shown in Table 2 below.
[0107] Table 2
[0108] Examples and Comparative Examples Defoamer No. Compatibility Defoaming time (Sec) Example 1 L1 transparent 13 Example 2 L2 transparent 14 Example 3 L3 transparent 15 Comparative Example 1 L4 turbid 20 Comparative Example 2 L5 turbid 18 Comparative Example 3 L6 turbid 18 Comparative Example 4 L7 turbid 17
[0109] It can be seen from the results in Table 2 that the compatibility and defoaming performance of the silicone emulsion defoamers prepared in Examples 1 to 3 are better than those in Comparative Examples 1 to 4. The defoamers in Examples 1 to 4 have no floating oil or floccules in the system formed with the laundry detergent, have good transparency, and the defoaming time is much shorter than that of the defoamers prepared in the comparative examples.
[0110] This is mainly because the components of the silicone emulsion defoamer provided in the embodiments of the present application, piperazine block modified silicone oil B1 and gluconolactone modified polysiloxane B2, can increase its dispersion performance in water; by optimizing the mass ratio of piperazine block modified silicone oil B1 and gluconolactone modified polysiloxane B2, the compatibility of the defoamer with other materials in the foaming system is improved; at the same time, the piperazine block modified silicone oil B1 and gluconolactone modified polysiloxane B2 can simultaneously serve as excellent surfactants, further improving the defoaming performance of the defoamer, and taking into account the compatibility and defoaming performance of the defoamer in laundry detergent.
[0111] The present application is described in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the present application and its core ideas. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.
Claims
1. A silicone emulsion defoamer, characterized in that: By mass, it includes the following components: Component A: 5 to 10 parts of organosilicon active material; the organosilicon active material includes hydrogen-containing polysiloxane A1, vinyl-terminated methylphenyl polysiloxane A2, and silicon dioxide A3; Component B: 5 to 10 parts of modified organic siloxane; the modified organic siloxane includes piperazine block modified silicone oil B1 and gluconolactone modified polysiloxane B2, wherein the chemical structure of the piperazine block modified silicone oil B1 is as shown in formula (1): As shown, wherein the chemical structure of R1 is as shown in formula (2): As shown, the chemical structure of R2 is as shown in formula (3): As shown, a, b, c, d are integers of 1 to 30; the chemical structural formula of the gluconolactone-modified polysiloxane is as shown in formula (4): As shown, the group R3 is an inert group, and the inert group is selected from at least one of methyl, cyclohexyl, cyclopentyl, and phenyl; the groups R4 and R5 are divalent C1-C18 hydrocarbon groups; m and n are integers of 1 to 1000; Component C: 2 to 5 parts of emulsifier; Component D: 0.5 to 3 parts of thickener; Component E: 77 to 82.5 parts of deionized water.
2. The organosilicon emulsion defoamer according to claim 1, characterized in that: In the component A, the molar ratio of the hydrogen-containing polysiloxane A1 to the vinyl-terminated methylphenyl polysiloxane A2 is 1:1-1.5; the mass proportion of the silicon dioxide A3 in the organic silicon active material is 3%-6%; the specific steps of the preparation process of the organic silicon active material are as follows: hydrogen-containing polysiloxane A1, vinyl-terminated methylphenyl polysiloxane A2, and silicon dioxide A3 are added into a reaction kettle, and a dispersion plate is turned on to fully stir. After stirring evenly, the temperature is raised to between 40 and 100° C., a platinum catalyst is added, and the temperature is continued to be raised to 120 to 200° C. for heat preservation. After heat preservation for 1 hour, the temperature is naturally lowered.
3. The organosilicon emulsion defoamer according to claim 2, characterized in that: The molar ratio of the hydrogen-containing polysiloxane A1 to the vinyl-terminated methylphenyl polysiloxane A2 is 1:1.2; and the mass proportion of the silicon dioxide A3 in the organic silicon active material is 5%.
4. The organosilicon emulsion defoamer according to claim 1, characterized in that: The group R3 is selected from any one of methyl, hydroxyl and phenyl; the groups R4 and R5 are 1,2-vinylene.
5. The organosilicon emulsion defoamer according to claim 1, characterized in that: In formula (4), m and n are 2 or 3.
6. The organosilicon emulsion defoamer according to claim 1, characterized in that: In the modified organic siloxane, the mass ratio of piperazine block modified silicone oil B1 to gluconolactone modified polysiloxane B2 is 3-5:9-22.
7. The organosilicon emulsion defoamer according to claim 1, characterized in that: The mass ratio of the piperazine block modified silicone oil B1 to the gluconolactone modified polysiloxane B2 is 5:
20.
8. The organosilicon emulsion defoamer according to claim 1, characterized in that: The emulsifier is a carbon chain emulsifier, and the carbon chain emulsifier is at least one of sorbitan monostearate (S-60), sorbitan monooleate (S-80), sorbitan tristearate (S-65), sorbitan monostearate (S-60), sorbitan monooleate polyoxyethylene ether ester (T-80), sorbitan tristearate polyoxyethylene ether ester (T-65), fatty alcohol polyoxyethylene ether (AEO-2, AEO-3, AEO-7, AEO-9), castor oil polyoxyethylene ether, alkylphenol polyoxyethylene ether, and glyceryl monostearate; the thickener is an acrylic acid alkali swelling thickener.
9. The method for preparing the organosilicon emulsion defoamer according to claim 1, comprising the steps of: S1. preparing organosilicon active substances and preparing modified organosiloxanes; S2. Take the organosilicon active substance, modified organosiloxane, emulsifier, thickener and deionized water according to mass parts and set aside; S3, mixing the organosilicon active substance, modified organosiloxane and emulsifier uniformly to obtain a first mixed solution; S4, adding half of the deionized water to the first mixed solution in sequence, then adding a thickener, and stirring evenly to obtain a second mixed solution; S5. Add the remaining deionized water to the second mixed solution and stir evenly to obtain the modified organosilicon laundry detergent defoamer.
10. The preparation method according to claim 9, characterized in that: In S3, the mixing temperature is 5 to 40°C.
Citation Information
Patent Citations
Method for preparing glycosyl amide modified polysiloxane
CN101942097A
Antifoaming agent composition and preparation method thereof
CN102489048A
Glycerol group-containing organopolysiloxane, cosmetic, and method for producing glycerol group-containing organopolysiloxane
CN103044685A
Trisiloxane containing glucosamide group and preparation method of trisiloxane
CN104086578A