Rare earth / alkaline earth metal composite ordered porous carbon material as well as preparation method and application thereof

By preparing rare earth/alkaline earth metal composite ordered porous carbon materials, the problem of removing hexavalent chromium and oxygen-containing inorganic salts from water bodies was solved, achieving efficient and stable adsorption and reduction effects, which are suitable for industrial water body remediation.

CN119034672AInactive Publication Date: 2024-11-29BEIJING NORMAL UNIV AT ZHUHAI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411460092.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing technologies are not effective at simultaneously removing hexavalent chromium and oxygen-containing inorganic salts from water. Furthermore, the removal efficiency of traditional adsorbents for hexavalent chromium is inhibited in the presence of oxygen-containing inorganic salts. Rare earth metals tend to agglomerate, and calcium peroxide has poor dispersibility in water, which limits its industrial application.

Method used

By loading nano-sized rare earth hydroxides and calcium peroxide onto ordered porous carbon materials, rare earth/alkaline earth metal composite ordered porous carbon materials are prepared. Utilizing their high stability, good adsorption and reduction properties, they can simultaneously process hexavalent chromium and oxygen-containing inorganic salts.

Benefits of technology

It improves the adsorption performance of hexavalent chromium and oxygen-containing inorganic salts, reduces separation and production costs, enhances the stability and environmental tolerance of the material, has a wide range of applications, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034672A_ABST
    Figure CN119034672A_ABST
Patent Text Reader

Abstract

The invention discloses a rare earth / alkaline earth metal composite ordered porous carbon material and a preparation method and application thereof, and belongs to the technical field of composite materials, the preparation method of the rare earth / alkaline earth metal composite ordered porous carbon material comprises the following steps: (1) dispersing an ordered porous carbon material in a soluble calcium salt solution, and uniformly stirring to obtain a suspension; (2) dropwise adding an alkaline hydrogen peroxide solution into the turbid liquid, uniformly stirring, carrying out reduced-pressure suction filtration, and washing a solid obtained by the reduced-pressure suction filtration; and (3) putting the washed solid into a rare earth metal salt solution, adding alkali liquor, uniformly stirring, carrying out reduced pressure suction filtration, washing the solid obtained by the reduced pressure suction filtration, and drying to obtain the rare earth / alkaline earth metal composite ordered porous carbon material. The preparation method disclosed by the invention is simple and has very strong operability and reproducibility, and the composite material has the characteristics of stable performance, excellent effect, wide use conditions, environmental friendliness, good regeneration performance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of composite materials, and in particular relates to a rare earth / alkaline earth metal composite ordered porous carbon material and a preparation method and application thereof. Background Art

[0002] Water pollution is considered to be one of the most critical issues in environmental pollution. Therefore, promoting water pollution control in the environmental field is of great significance to environmental protection.

[0003] Solutions containing hexavalent chromium ions are widely used in mining, electroplating, leather making, textile and other industries. Excessive chromium will cause serious water quality problems and have adverse effects on human health. Cr(VI) usually exists in the form of highly soluble and highly toxic chromates (HCrO4 - or Cr2O7 2- ), which is extremely toxic even at low levels. Chemical reduction is a common method for treating Cr(VI)-contaminated wastewater. On the one hand, the toxicity of Cr(VI) is 500-1000 times that of Cr(III); on the other hand, the fluidity of Cr(III) is worse than that of Cr(VI), and it is easier to generate insoluble precipitates, which can be more easily removed. Therefore, pre-reduction of Cr(VI) to Cr(III) is crucial for treating chromium-containing wastewater.

[0004] The main source of chromium-contaminated wastewater is industrial wastewater, especially wastewater discharged from leather factories. Tanneries that use vegetable tanning often use oxygen-containing inorganic salts as surfactants, neutralizers or chelating agents, which makes chromium-contaminated wastewater rich in oxygen-containing inorganic salts, which may cause eutrophication of water bodies, seriously damage the ecosystem, and reduce species diversity. Therefore, it is of vital importance to use economical and efficient technical means to purify and repair water bodies.

[0005] In order to simultaneously reduce the content of oxygen-containing inorganic salts and Cr(VI) in polluted water, traditional treatment technologies include chemical precipitation, chemical reduction, ion exchange, adsorption, etc. However, these technologies often encounter problems such as high cost and low treatment efficiency in practical applications. Adsorption is a mature and commonly used wastewater treatment process with a series of advantages such as flexibility, simplicity, economy and high efficiency. At present, many studies have focused on developing new adsorbents or improving traditional adsorbents. However, experiments have shown that in the presence of Cr(VI), the actual adsorption efficiency of these new adsorbents for oxygen-containing inorganic salts is low. In addition, in the presence of oxygen-containing inorganic salts, the removal of Cr(VI) is always inhibited to a certain extent, further reducing its industrial application value. Therefore, in order to simultaneously remove Cr(VI) and oxygen-containing inorganic salts from polluted water, it is necessary to develop a new material that can achieve chemical reduction and adsorption at the same time.

[0006] Some rare earth elements (such as lanthanum, cerium, yttrium, etc.) and alkaline earth metal elements (such as calcium and magnesium) are abundant in the earth's crust, so the cost is relatively low. However, in practical applications, rare earth and alkaline earth metal particles will co-aggregate to form large particles, which limits the exposure of active sites, and CaO2 has poor dispersibility in water and is easy to decompose quickly, which greatly limits its industrial application. How to prepare environmental remediation adsorption materials with high stability, cost-effectiveness and excellent environmental tolerance is a problem that people need to solve. There have been many related studies at home and abroad. Song et al. (Song, et al. Bulletin of the Korean Chemical Society. 35 (6) (2014) 1817-1824.) reported a calcined Mg-Al-CO3 layered material for treating chromium- and phosphorus-containing contaminated water bodies. The material showed high adsorption capacity for both single Cr (VI) and phosphorus, but a high content of phosphorus would significantly inhibit the adsorption of Cr (VI) by the material, inhibiting the industrial application of the material. Summary of the invention

[0007] In order to solve the above technical problems, the present invention proposes a rare earth / alkaline earth metal composite ordered porous carbon material and its preparation method and application. The present invention loads nano-scale rare earth hydroxide and calcium peroxide onto an ordered porous carbon material, and prepares a new type of efficient water body repair material - rare earth / alkaline earth metal composite ordered porous carbon material through a liquid phase synthesis method. The problem that the existing rare earth metals are easy to agglomerate, have low contact efficiency, are difficult to separate and recover, and the calcium peroxide particles are unevenly dispersed and quickly decomposed in water can be solved. The water body repair material prepared by the present invention can simultaneously give play to the good adsorption properties of rare earth hydroxides,

[0008] The reducing property of CaO2 on Cr(VI) and the high electron abundance, high mechanical strength, and good chemical thermal stability of ordered porous carbon (OPC) greatly improve the removal effect of inorganic salts in water.

[0009] To achieve the above object, the present invention provides the following technical solutions:

[0010] One of the technical solutions of the present invention:

[0011] A method for preparing a rare earth / alkaline earth metal composite ordered porous carbon material comprises the following steps:

[0012] (1) dispersing the ordered porous carbon material in a soluble calcium salt solution, stirring evenly (so that the ordered porous carbon material is fully dispersed in the soluble calcium salt solution), to obtain a suspension;

[0013] (2) adding alkaline hydrogen peroxide solution to the suspension, stirring evenly (to form calcium peroxide particles on the surface of the ordered porous carbon material), filtering under reduced pressure, and washing the solid obtained by filtering under reduced pressure (to wash away unreacted salt);

[0014] (3) placing the washed solid in a rare earth metal salt solution, adding alkaline solution, stirring evenly (to form rare earth hydroxide on the surface of the ordered porous carbon loaded with calcium peroxide particles), vacuum filtering, washing the solid obtained by vacuum filtering (washing away unreacted salt), and drying to obtain the rare earth / alkaline earth metal composite ordered porous carbon material.

[0015] Preferably, in step (1), the soluble calcium salt solution is a calcium chloride solution; and the ordered porous carbon material is graphene oxide, carbon nanotubes, fullerenes or activated carbon fibers.

[0016] Preferably, in step (1), the pH of the calcium chloride solution is 7, and the concentration of the calcium chloride solution is 0.40-0.60 mol / L.

[0017] Preferably, in step (1), the reaction temperature is 20-30°C; the stirring speed is 400-600 rpm, and the stirring time is 20-40 min.

[0018] More preferably, the step of obtaining the suspension in step (1) is as follows: dispersing 0.4-0.6 g of the ordered porous carbon material in 100 mL of a calcium chloride solution having a pH of 7 and a concentration of 0.40-0.60 mol / L, stirring evenly at 20-30° C., at a stirring speed of 400-600 rpm, and for 20-40 min to obtain a suspension.

[0019] Preferably, in step (2), the concentration of sodium hydroxide in the alkaline hydrogen peroxide solution is 0.5-1.5 mol / L, and the concentration of hydrogen peroxide is 0.25-0.75 mol / L.

[0020] Preferably, in step (2), the reaction temperature is 20-30°C; the stirring speed is 400-600 rpm, and the stirring time is 20-40 min.

[0021] Preferably, in step (3), the concentration of the rare earth metal salt solution is 0.25-1.0 mol / L.

[0022] Preferably, in step (3), the rare earth metal salt solution is a lanthanum nitrate solution, an yttrium nitrate solution or a cerium nitrate solution.

[0023] Preferably, in step (3), the alkali solution is a sodium hydroxide solution with a concentration of 0.5-1.5 mol / L.

[0024] Preferably, in step (3), the reaction temperature is 20-30°C; the stirring speed is 400-600 rpm, and the stirring time is 40-80 min.

[0025] Preferably, in step (3), the drying temperature is 100-110° C. and the drying time is 5-7 h.

[0026] In order to overcome the problems existing in the adsorption materials in the prior art, it is necessary to find a suitable carrier to reduce the particle size of rare earth metal and CaO2 particles and improve their performance. Ordered porous carbon materials (OPC) have the characteristics of high surface area, high mechanical strength, good chemical thermal stability, good electrical conductivity and thermal conductivity, etc., which can effectively avoid the co-aggregation of rare earth metals and CaO2 and improve the adsorption performance; the strong interaction between OPC and the loaded metal can effectively prevent the leakage of rare earth metals, reduce the dispersion of CaO2, and improve the stability of CaO2, thereby avoiding the waste of materials. Therefore, the new water body repair agent (i.e., rare earth / alkaline earth metal composite ordered porous carbon material) prepared by loading rare earth metals and CaO2 on OPC in the present invention has a good adsorption capacity for oxygen-containing inorganic salts and Cr (VI). Rare earth-based and calcium-based materials have strong binding ability to ligands such as oxygen-containing inorganic salts and Cr(VI), showing high adsorption performance, and can reduce metal leaching during the adsorption process to prevent secondary pollution of the environment and waste of resources; alkaline earth metal peroxides (such as CaO2) can slowly release hydrogen peroxide (H2O2) and Ca(VI) in water. 2+ , H2O2 can effectively reduce Cr(VI), Ca 2+ It can form a complex with oxygen-containing inorganic salts, so CaO2 has the potential to simultaneously reduce Cr(VI) and adsorb oxygen-containing inorganic salts. Based on the above considerations, the present invention selects a combination of rare earth and alkaline earth metals as a water body repair agent. The present invention adopts a liquid phase synthesis method to prepare a rare earth / alkaline earth metal composite ordered porous carbon material, which has high stability, high mechanical strength and excellent corrosion resistance, and can achieve a more ideal adsorption treatment effect on polluted water bodies rich in oxygen-containing inorganic salts and Cr(VI). This material simultaneously plays the advantages of the three basic materials and solves the problems of easy co-aggregation of alkaline earth metals and CaO2 and easy decomposition of CaO2. In summary, the rare earth / alkaline earth metal composite ordered porous carbon material prepared by the present invention is a water body repair material with excellent effect and good practicality for use in the field of environmental remediation, which can effectively adsorb and catalytically reduce oxygen-containing inorganic salts and Cr(VI) in coupled water bodies.

[0027] The second technical solution of the present invention:

[0028] The present invention also provides a rare earth / alkaline earth metal composite ordered porous carbon material prepared according to the above method.

[0029] The present invention proposes a novel water body repair material-a preparation process of a rare earth / alkaline earth metal composite ordered porous carbon material, wherein a liquid phase synthesis method is used to load nano-scale rare earth hydroxide and calcium peroxide onto an ordered porous carbon material, wherein the preparation method is simple, the operation safety is high, and the material cost is low, and the rare earth hydroxide and calcium peroxide are loaded onto an ordered porous carbon substrate material having sufficient active sites and good environmental tolerance, and the prepared product has stable quality and excellent environmental tolerance. The present invention simultaneously exerts the advantages of good adsorption performance of rare earth hydroxide, reducibility of calcium peroxide to hexavalent chromium, and rich electrons of ordered porous carbon, good stability, high mechanical strength, and excellent corrosion resistance, and solves the shortcomings of easy agglomeration of current rare earth hydroxides, low contact efficiency, poor dispersibility of calcium peroxide in water, and easy and rapid decomposition, so that the material can simultaneously treat phosphorus-polluted and chromium (VI)-polluted water bodies, which is beneficial to improve adsorption efficiency. The present invention has the capabilities of regeneration and raw material recovery. Rare earth hydroxide and calcium peroxide are loaded on ordered porous carbon which is easy to separate, can be used for continuous operation and has good mechanical properties, thereby reducing the difficulty of separation after use. The regeneration process is simple and operable, while the excellent adsorption performance of the ordered porous carbon itself is not changed. After regeneration, the adsorbed oxygen-containing inorganic salts can be released and recovered, thereby greatly reducing separation and production costs, creating wastewater reuse value, improving green economic benefits, and being conducive to application in production and life.

[0030] The third technical solution of the present invention:

[0031] The present invention also provides the use of the rare earth / alkaline earth metal composite ordered porous carbon material in the simultaneous treatment of water bodies polluted by oxygen-containing inorganic salts and chromium (VI).

[0032] Preferably, the oxygen-containing inorganic salt is phosphate, arsenate, selenate or dichromate.

[0033] Compared with the prior art, the present invention has the following advantages and technical effects:

[0034] (1) The product preparation method is simple, the performance is stable, and the effect is excellent. Compared with traditional water body restoration agents, the pH value of the product has a wide application range and is safe and harmless to the environment. It has a wide range of applicable conditions. At the same time, the raw material price is cheap and the preparation cost is low, which is conducive to industrial production and practical application.

[0035] (2) The material of the present invention combines rare earth hydroxide and calcium peroxide on ordered porous carbon at the same time, thereby preventing the rare earth hydroxide from agglomerating easily, resulting in structural damage and reduced active adsorption points, and effectively solving the problem of poor dispersibility and rapid dissolution of calcium peroxide in water. The potential ability of CaO2 to reduce Cr(VI) and simultaneously adsorb Cr(VI) and oxygen-containing inorganic salts is fully utilized. The loaded water body remediation agent can simultaneously treat water bodies polluted by oxygen-containing inorganic salts and chromium (VI) polluted, thereby improving the adsorption performance and catalytic reduction coupling performance of the material.

[0036] (3) The material of the present invention improves the dispersion degree of rare earth hydroxides, utilizes the strong interaction between ordered porous carbon and loaded metal to prevent leakage of rare earth metals, is easy to separate and recycle, reduces metal loss, avoids material waste, and has good regeneration performance. After regeneration, the adsorbed phosphorus can be recovered, thereby improving the utilization value of wastewater and reducing production costs and the risk of secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0038] Figure 1 A nitrogen adsorption-desorption curve diagram of the rare earth / alkaline earth metal composite ordered porous carbon material prepared in Example 2 of the present invention;

[0039] Figure 2 This is a micropore size distribution diagram of the rare earth / alkaline earth metal composite ordered porous carbon material prepared in Example 2 of the present invention;

[0040] Figure 3 This is a mesopore size distribution diagram of the rare earth / alkaline earth metal composite ordered porous carbon material prepared in Example 2 of the present invention;

[0041] Figure 4 This is a scanning electron microscope image of the rare earth / alkaline earth metal composite ordered porous carbon material prepared in Example 3 of the present invention;

[0042] Figure 5 This is the mapping element energy spectrum of the rare earth / alkaline earth metal composite ordered porous carbon material prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0043] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0044] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0045] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0046] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0047] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0048] Unless otherwise specified, the room temperature in the present invention is 25±2°C.

[0049] All raw materials used in the examples of the present invention are commercially available.

[0050] Existing calcium-based materials can remove phosphorus or Cr (VI) by forming a complex using an adsorption method. However, in the presence of hexavalent chromium, the efficiency of adsorption phosphorus removal is not ideal, and in the presence of phosphate, the removal of chromate is also limited because at the same pH value, chemical chromate reduction and phosphate adsorption show opposite trends. Therefore, the present invention adopts a different removal mechanism to improve the Ca-based material, prepare calcium peroxide (CaO2), react with water to slowly release H2O2, and reduce Cr (VI) to low-toxic and easily removable Cr (III) through a reduction reaction, while achieving chemical reduction and adsorption, thereby removing the highly toxic Cr (VI) ions together with oxygen-containing inorganic salts (such as phosphates). However, due to the interference of chromium ions, the effect of calcium-based materials in removing phosphates is not ideal. In order to further improve the phosphorus removal capacity, rare earth elements are combined with alkaline earth metals, and rare earth elements (such as lanthanum) are added to the Ca-based material, which can strongly bind to phosphates even at low concentrations, and has a wide working pH range and excellent stability. After phosphate is adsorbed, the phosphate on the material can shorten the electron transfer channel, improve the material's ability to reduce Cr(VI), and use the bimetallic synergistic effect to improve the removal ability of phosphate and Cr(VI). In addition, metal materials tend to agglomerate to form large particles, which limits the exposure of active sites. Therefore, a suitable carrier is needed to reduce the particle size of CaO2 and La and improve their performance. Ordered porous carbons (OPCs) have the characteristics of large specific surface area, stable structure, and easy modification. Their large π conjugated system and electron sponge effect can form a strong coupling effect with metals, which helps to reduce particle aggregation and accelerate electron transfer, thereby improving the reduction and removal ability of Cr(VI).

[0051] The technical solution of the present invention is further illustrated by the following embodiments.

[0052] Example 1

[0053] A method for preparing a rare earth / alkaline earth metal composite ordered porous carbon material comprises the following steps:

[0054] (1) Preparation of calcium chloride solution with pH=7:

[0055] Weigh 5.549 g of calcium chloride granules, dissolve in 100 mL of deionized water, stir with a glass rod until the solid is completely dissolved, and adjust the pH to 7 to obtain a pH of 7, 0.5 mol / L calcium chloride solution;

[0056] (2) Preparation of alkaline hydrogen peroxide solution:

[0057] Weigh 2.00 g of sodium hydroxide granules, measure 2.833 g of 30% hydrogen peroxide solution, dissolve them in 50 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain an alkaline hydrogen peroxide solution, wherein the concentration of sodium hydroxide is 1.0 mol / L, and the concentration of hydrogen peroxide solution is 0.5 mol / L;

[0058] (3) Preparation of cerium nitrate solution:

[0059] Weigh 32.5500 g of cerium nitrate hexahydrate solid, dissolve it in 150 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain a cerium nitrate solution with a concentration of 0.5 mol / L;

[0060] (4) Preparation of sodium hydroxide solution:

[0061] Weigh 1.00 g of sodium hydroxide pellets, dissolve in 50 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain a sodium hydroxide solution with a concentration of 0.5 mol / L;

[0062] (5) Preparation of Ce-Ca-OPC:

[0063] (5-1) Weighing 0.500 g of graphene oxide was placed in 100 mL of a pH 7, 0.5 mol / L calcium chloride solution, adding a magnet, and stirring on a magnetic stirrer at 25° C. and 500 rpm for 30 min to fully disperse the graphene oxide in the solution to obtain a uniformly dispersed suspension;

[0064] (5-2) slowly adding 50 mL of the alkaline hydrogen peroxide solution in step (2) to the dispersed suspension, stirring on a magnetic stirrer at 25° C. and 500 rpm for 30 min to form calcium peroxide particles on the surface of the graphene oxide;

[0065] (5-3) Filter the suspension under reduced pressure, place the obtained solid in deionized water, and stir on a magnetic stirrer at 25° C. and 500 rpm for 10 min. Repeat this process three times to wash away unreacted salt.

[0066] (5-4) placing the washed solid by filtration in 100 mL of a 0.5 mol / L cerium nitrate solution, adding 50 mL of a 1.0 mol / L sodium hydroxide solution, and stirring on a magnetic stirrer at 25° C. and 500 rpm for 60 min to form cerium hydroxide on the surface of the graphene oxide loaded with calcium peroxide particles;

[0067] (5-5) Filter the suspension under reduced pressure, place the obtained solid in deionized water, and stir on a magnetic stirrer at 25° C. and 500 rpm for 10 min. Repeat this process three times to wash away unreacted salt.

[0068] (5-6) The solid obtained by filtration after washing was placed in an oven and dried at 105 °C for 6 h to obtain a rare earth / alkaline earth metal composite ordered porous carbon material, which was recorded as Ce-Ca-OPC.

[0069] The rare earth / alkaline earth metal composite ordered porous carbon material prepared in this embodiment was placed in a mixed solution of 50 mL of 100 mg / L arsenate and 10 mg / L chromium (VI) at a mass concentration of 0.2 g / L to carry out an experiment on water arsenic and chromium (VI) pollution treatment. Oscillating on a shaker at 25 ° C and 200 rpm for 4 hours. The results show that in the substrate concentrations of 100 mg / L (As) and 10 mg / L (Cr) solutions, the rare earth / alkaline earth metal composite ordered porous carbon material with a cerium-calcium molar ratio of 1.0 has an adsorption capacity of about 159 mg / g for arsenate and a removal rate of about 98% for chromium (VI). At the same time, after the reaction, it was characterized by electron scanning microscopy, and it was known that the material maintained its original structure, proving that the material has high mechanical strength, and during the reaction, no metal ion leaching (<0.2 mg / L) was detected, proving that the material has high stability and excellent corrosion resistance.

[0070] In addition, in order to demonstrate its wide pH applicability, the rare earth / alkaline earth metal composite ordered porous carbon material prepared in this embodiment was applied to sewage with pH = 4-9 (pH = 4, pH = 5, pH = 6, pH = 7, pH = 8 or pH = 9), and the results showed that its arsenate adsorption capacity was maintained at more than 80% of the initial capacity, and the chromium (VI) removal rate was maintained at more than 90%, proving that the material of the present invention can be used in a larger pH range.

[0071] Example 2

[0072] A method for preparing a rare earth / alkaline earth metal composite ordered porous carbon material comprises the following steps:

[0073] (1) Preparation of calcium chloride solution with pH=7:

[0074] Weigh 5.549 g of calcium chloride granules, dissolve in 100 mL of deionized water, stir with a glass rod until the solid is completely dissolved, and adjust the pH to 7 to obtain a pH of 7, 0.5 mol / L calcium chloride solution;

[0075] (2) Preparation of alkaline hydrogen peroxide solution:

[0076] Weigh 3.00 g of sodium hydroxide granules, measure 4.250 g of 30% hydrogen peroxide solution, dissolve them in 50 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain an alkaline hydrogen peroxide solution, wherein the concentration of sodium hydroxide is 1.5 mol / L, and the concentration of hydrogen peroxide solution is 0.75 mol / L;

[0077] (3) Preparation of yttrium nitrate solution:

[0078] Weigh 41.1941 g of yttrium nitrate trihydrate solid, dissolve it in 150 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain an yttrium nitrate solution with a concentration of 0.75 mol / L;

[0079] (4) Preparation of sodium hydroxide solution:

[0080] Weigh 3.0 g of sodium hydroxide pellets, dissolve in 50 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain a sodium hydroxide solution with a concentration of 1.5 mol / L;

[0081] (5) Preparation of Y-Ca-OPC:

[0082] (5-1) 0.600 g of fullerene was placed in 100 mL of a pH 7, 0.5 mol / L calcium chloride solution, a magnet was added, and the mixture was stirred on a magnetic stirrer at 30° C. and 600 rpm for 40 min to fully disperse the fullerene in the solution, thereby obtaining a suspension containing the fullerene;

[0083] (5-2) slowly adding 50 mL of the alkaline hydrogen peroxide solution prepared in step (2) to the above suspension, stirring the mixture on a magnetic stirrer at 30° C. and 600 rpm for 40 min to form calcium peroxide particles on the surface of the fullerene;

[0084] (5-3) Filter the suspension under reduced pressure, place the obtained solid in deionized water, and stir on a magnetic stirrer at 30° C. and 600 rpm for 15 min, repeating the process three times to wash away unreacted salt;

[0085] (5-4) The solid obtained by filtration after washing was placed in 100 mL of a 1.00 mol / L yttrium nitrate solution, and 50 mL of a 1.5 mol / L sodium hydroxide solution was added, and the mixture was stirred on a magnetic stirrer at 30° C. and 600 rpm for 80 min to form yttrium hydroxide on the surface of the fullerene loaded with calcium peroxide particles;

[0086] (5-5) Filter the suspension under reduced pressure, place the obtained solid in deionized water, and stir on a magnetic stirrer at 30° C. and 600 rpm for 15 min, repeating the process three times to wash away unreacted salt;

[0087] (5-6) The solid obtained by filtration after washing was placed in an oven and dried at 110 °C for 7 h to obtain a rare earth / alkaline earth metal composite ordered porous carbon material, which was recorded as Y-Ca-OPC.

[0088] The nitrogen adsorption-desorption curve of the rare earth / alkaline earth metal composite ordered porous carbon material prepared in this example is shown in Figure 1It can be seen that it is a V-type isotherm, accompanied by a hysteresis loop, which makes the isotherm biased towards type IV, proving that the material has both microporous and mesoporous structures, which can effectively improve the contact efficiency with pollutants in the reaction, thereby improving performance.

[0089] The micropore size distribution diagram of the rare earth / alkaline earth metal composite ordered porous carbon material prepared in this embodiment is shown in Figure 2 , the mesopore size distribution diagram is shown in Figure 3 , proving the existence of micropores and mesoporous structures in the material.

[0090] The rare earth / alkaline earth metal composite ordered porous carbon material prepared in this embodiment was placed in a mixed solution of 50 mL of 100 mg / L selenate and 10 mg / L chromium (VI) at a mass concentration of 0.2 g / L to carry out a water body selenium and chromium (VI) pollution treatment experiment. Oscillate on a shaker at 25 ° C and 200 rpm for 4 hours. The results show that in the substrate concentrations of 100 mg / L (Se) and 10 mg / L (Cr) solutions, the rare earth / alkaline earth metal composite ordered porous carbon material with a yttrium-calcium molar ratio of 1.5 has an adsorption capacity of about 82 mg / g for selenate and a removal rate of about 90% for chromium (VI). At the same time, after the reaction, it was characterized by electron scanning microscopy, and it was known that the material maintained the initial structure, proving that the material has high mechanical strength, and during the reaction, no metal ion leaching (<0.2 mg / L) was detected, proving that the material has high stability and excellent corrosion resistance.

[0091] In addition, in order to demonstrate its wide pH applicability, the rare earth / alkaline earth metal composite ordered porous carbon material prepared in this embodiment was applied to sewage with pH = 4-9 (pH = 4, pH = 5, pH = 6, pH = 7, pH = 8 or pH = 9), and the results showed that the selenate adsorption capacity was maintained at more than 80% of the initial capacity, and the chromium (VI) removal rate was maintained at more than 85%, proving that the material of the present invention can be used in a larger pH range.

[0092] Example 3

[0093] A method for preparing a rare earth / alkaline earth metal composite ordered porous carbon material comprises the following steps:

[0094] (1) Preparation of calcium chloride solution with pH=7:

[0095] Weigh 5.549 g of calcium chloride granules, dissolve in 100 mL of deionized water, stir with a glass rod until the solid is completely dissolved, and adjust the pH to 7 to obtain a pH of 7, 0.5 mol / L calcium chloride solution;

[0096] (2) Preparation of alkaline hydrogen peroxide solution:

[0097] Weigh 1.00 g of sodium hydroxide particles, measure 1.417 g of 30% (mass percentage, the same below) hydrogen peroxide solution, dissolve them in 50 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain an alkaline hydrogen peroxide solution, wherein the concentration of sodium hydroxide is 0.5 mol / L, and the concentration of hydrogen peroxide solution is 0.25 mol / L;

[0098] (3) Preparation of lanthanum nitrate solution

[0099] Weigh 16.2375 g of lanthanum nitrate hexahydrate solid, dissolve it in 150 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain a lanthanum nitrate solution with a concentration of 0.25 mol / L;

[0100] (4) Preparation of sodium hydroxide solution:

[0101] Weigh 1.0 g of sodium hydroxide pellets, dissolve in 50 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain a sodium hydroxide solution with a concentration of 0.5 mol / L;

[0102] (5) Preparation of La-Ca-OPC:

[0103] (5-1) 0.400 g of carbon nanotubes were weighed and placed in 100 mL of a pH 7, 0.5 mol / L calcium chloride solution, a magnetic bar was added, and the mixture was stirred on a magnetic stirrer at 20° C. and 400 rpm for 20 min to fully disperse the carbon nanotubes in the solution, thereby obtaining a suspension containing dispersed carbon nanotubes;

[0104] (5-2) slowly adding 50 mL of the alkaline hydrogen peroxide solution prepared in step (2) to the suspension containing the dispersed carbon nanotubes, and stirring the mixture on a magnetic stirrer at 20° C. and 400 rpm for 20 min to form calcium peroxide particles on the surface of the carbon nanotubes;

[0105] (5-3) Filter the suspension under reduced pressure, place the obtained solid in deionized water, and stir on a magnetic stirrer at 20° C. and 400 rpm for 5 min, repeating the process three times to wash away unreacted salt;

[0106] (5-4) placing the washed solid by filtration in 100 mL of a 0.25 mol / L lanthanum nitrate solution, adding 50 mL of a 0.5 mol / L sodium hydroxide solution, and stirring on a magnetic stirrer at 20° C. and 400 rpm for 40 min to form lanthanum hydroxide on the surface of the carbon nanotubes loaded with calcium peroxide particles;

[0107] (5-5) Filter the suspension under reduced pressure, place the obtained solid in deionized water, and stir on a magnetic stirrer at 20° C. and 400 rpm for 5 min, repeating the process three times to wash away unreacted salt;

[0108] (5-6) The solid obtained by filtration after washing was placed in an oven and dried at 100 °C for 5 h to obtain a rare earth / alkaline earth metal composite carbon nanotube material, which was recorded as La-Ca-OPC.

[0109] The scanning electron microscope image of the rare earth / alkaline earth metal composite carbon nanotube material prepared in this example is shown in FIG. Figure 4 , see the energy spectrum of mapping elements Figure 5 It can be seen that the color points representing La and Ca elements are evenly distributed on the surface of the carbon nanotube material, which proves that using carbon nanotubes as carriers can solve the problem of easy agglomeration of metal materials, make them dispersed evenly, and improve the contact efficiency between active metals and reactants.

[0110] Performance test of rare earth / alkaline earth metal composite ordered porous carbon materials:

[0111] The rare earth / alkaline earth metal composite ordered porous carbon material prepared in this embodiment was placed in a 50 mL mixed solution with a phosphate concentration of 100 mg / L and a chromium (VI) concentration of 10 mg / L at a mass concentration of 0.2 g / L to conduct a water body phosphorus and chromium (VI) pollution treatment experiment. Oscillate on a shaker at 25°C and 200 rpm for 4 hours. The results show that in solutions with substrate concentrations of 100 mg / L (P) and 10 mg / L (Cr), the rare earth / alkaline earth metal composite ordered porous carbon material with a lanthanum-calcium molar ratio of 0.5 has an adsorption capacity of about 128 mg / g for phosphate and a removal rate of about 94% for chromium (VI). At the same time, after the reaction, the electron scanning microscopy showed that the morphology of the carbon nanotube material did not change significantly and still maintained the tubular structure, proving that the material has high mechanical strength. During the reaction, no leaching of metal ions was detected (<0.2 mg / L), proving that the material has high stability and excellent corrosion resistance.

[0112] In addition, in order to demonstrate its wide pH applicability, the rare earth / alkaline earth metal composite ordered porous carbon material prepared in this embodiment was applied to sewage with pH = 4-9 (pH = 4, pH = 5, pH = 6, pH = 7, pH = 8 or pH = 9), and the results showed that its phosphate adsorption capacity was maintained at more than 85% of the initial capacity, and the chromium (VI) removal rate was maintained at more than 90%, proving that the material of the present invention can be used in a larger pH range.

[0113] Comparative Example 1

[0114] A method for preparing a rare earth / metal composite molecular sieve material comprises the following steps:

[0115] (1) Preparation of lanthanum nitrate solution

[0116] Weigh 16.2375 g of lanthanum nitrate hexahydrate solid, dissolve it in 150 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain a lanthanum nitrate solution with a concentration of 0.25 mol / L;

[0117] (2) Preparation of sodium hydroxide solution:

[0118] Weigh 1.0 g of sodium hydroxide pellets, dissolve in 50 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain a sodium hydroxide solution with a concentration of 0.5 mol / L;

[0119] (3) Weigh 0.400 g of MCM-41 molecular sieve and place it in 100 mL of 0.25 mol / L lanthanum nitrate solution, add 50 mL of 0.5 mol / L sodium hydroxide solution, stir on a magnetic stirrer at 20° C. and 400 rpm for 40 min, filter under reduced pressure, place the resulting solid in deionized water, stir on a magnetic stirrer at 20° C. and 400 rpm for 5 min, repeat three times to wash away unreacted salt;

[0120] (4) The solid obtained by filtration after washing is placed in an oven and dried in the oven at 100° C. for 5 h to obtain a rare earth / metal composite molecular sieve material.

[0121] The rare earth / metal composite molecular sieve material prepared in this comparative example was placed in a mixed solution of 100 mg / L phosphate and 10 mg / L chromium (VI) at a mass concentration of 0.2 g / L to conduct a water body phosphorus and chromium (VI) pollution treatment experiment. The mixture was shaken on a shaker at 25°C and 200 rpm for 4 hours. The results showed that in solutions with substrate concentrations of 100 mg / L (P) and 10 mg / L (Cr), the material had an adsorption capacity of about 38 mg / g for phosphate and a removal rate of about 10% for chromium (VI).

[0122] It can be seen from this comparative example that after the composite ordered porous carbon material is replaced with a molecular sieve, the prepared composite material cannot simultaneously and efficiently treat phosphate and chromium (VI) in water.

[0123] Comparative Example 2

[0124] A method for preparing an alkaline earth metal composite carbon nanotube material comprises the following steps:

[0125] (1) Preparation of calcium chloride solution with pH=7:

[0126] Weigh 5.549 g of calcium chloride granules, dissolve in 100 mL of deionized water, stir with a glass rod until the solid is completely dissolved, and adjust the pH to 7 to obtain a pH of 7, 0.5 mol / L calcium chloride solution;

[0127] (2) Preparation of alkaline hydrogen peroxide solution:

[0128] Weigh 1.00 g of sodium hydroxide particles, measure 1.417 g of 30% (mass percentage, the same below) hydrogen peroxide solution, dissolve them in 50 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain an alkaline hydrogen peroxide solution, wherein the concentration of sodium hydroxide is 0.5 mol / L, and the concentration of hydrogen peroxide solution is 0.25 mol / L;

[0129] (3) Weighing 0.400 g of carbon nanotubes and placing them in 100 mL of a pH = 7, 0.5 mol / L calcium chloride solution, adding a magnet, and stirring on a magnetic stirrer at 20° C. and 400 rpm for 20 min to fully disperse the carbon nanotubes in the solution, thereby obtaining a suspension in which the carbon nanotubes are dispersed; slowly dropwise adding 50 mL of the alkaline hydrogen peroxide solution in step (2) into the suspension in which the carbon nanotubes are dispersed, and stirring on a magnetic stirrer at 20° C. and 400 rpm for 20 min to form calcium peroxide particles on the surface of the carbon nanotubes;

[0130] (4) Filter the suspension under reduced pressure, place the obtained solid in deionized water, stir on a magnetic stirrer at 20° C. and 400 rpm for 5 min, and repeat three times to wash away unreacted salt; place the washed and filtered solid in an oven, and dry it in an oven at 100° C. for 5 h to obtain an alkaline earth metal composite carbon nanotube material.

[0131] The alkaline earth metal composite carbon nanotube material prepared in this comparative example was placed in a 50mL mixed solution with a phosphate concentration of 100mg / L and a chromium (VI) concentration of 10mg / L at a mass concentration of 0.2g / L to conduct a water body phosphorus and chromium (VI) pollution treatment experiment. It was shaken on a shaker at 25°C and 200rpm for 4h. The results showed that in solutions with substrate concentrations of 100mg / L (P) and 10mg / L (Cr), the material had an adsorption capacity of about 68mg / g for phosphate and a removal rate of about 80% for chromium (VI).

[0132] It can be seen from this comparative example that although the alkaline earth metal composite carbon nanotube material can also adsorb phosphate and chromium (VI) at the same time, since rare earth elements are not introduced into the composite material, the removal effect of the two pollutants is not ideal.

[0133] Comparative Example 3

[0134] A method for preparing a rare earth metal composite carbon nanotube material comprises the following steps:

[0135] (1) Preparation of lanthanum nitrate solution

[0136] Weigh 16.2375 g of lanthanum nitrate hexahydrate solid, dissolve it in 150 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain a lanthanum nitrate solution with a concentration of 0.25 mol / L;

[0137] (2) Preparation of sodium hydroxide solution:

[0138] Weigh 1.0 g of sodium hydroxide pellets, dissolve in 50 mL of deionized water, and stir with a glass rod until the solid is completely dissolved to obtain a sodium hydroxide solution with a concentration of 0.5 mol / L;

[0139] (3) Weighing 0.400 g of carbon nanotubes into 100 mL of 0.25 mol / L lanthanum nitrate solution, adding 50 mL of 0.5 mol / L sodium hydroxide solution, and stirring on a magnetic stirrer at 20° C. and 400 rpm for 40 min to form lanthanum hydroxide on the surface of the carbon nanotubes loaded with calcium peroxide particles;

[0140] (4) Filter the suspension under reduced pressure, place the obtained solid in deionized water, stir on a magnetic stirrer at 20° C. and 400 rpm for 5 min, and repeat three times to wash away unreacted salt; place the washed and filtered solid in an oven, and dry it in an oven at 100° C. for 5 h to obtain a rare earth metal composite carbon nanotube material.

[0141] The rare earth metal composite carbon nanotube material prepared in this comparative example was placed in a 50mL mixed solution with a phosphate concentration of 100mg / L and a chromium (VI) concentration of 10mg / L at a mass concentration of 0.2g / L to conduct a water body phosphorus and chromium (VI) pollution treatment experiment. It was shaken on a shaker at 25°C and 200rpm for 4h. The results showed that in solutions with substrate concentrations of 100mg / L (P) and 10mg / L (Cr), the material had an adsorption capacity of about 90mg / g for phosphate and a removal rate of about 10% for chromium (VI).

[0142] It can be seen from this comparative example that although the rare earth metal composite carbon nanotube material has a certain adsorption effect on phosphate, its removal effect on chromium (VI) is very poor.

[0143] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A method for preparing a rare earth / alkaline earth metal composite ordered porous carbon material, characterized in that: The following steps are involved: (1) dispersing the ordered porous carbon material in a soluble calcium salt solution and stirring the mixture to obtain a suspension; (2) adding alkaline hydrogen peroxide solution dropwise to the suspension, stirring evenly, filtering under reduced pressure, and washing the solid obtained by filtering under reduced pressure; (3) placing the washed solid in a rare earth metal salt solution, adding alkali solution, stirring evenly, filtering under reduced pressure, washing the solid obtained by filtering under reduced pressure, and drying to obtain the rare earth / alkaline earth metal composite ordered porous carbon material.

2. The method for preparing the rare earth / alkaline earth metal composite ordered porous carbon material according to claim 1, characterized in that: In step (1), the soluble calcium salt solution is a calcium chloride solution; and the ordered porous carbon material is graphene oxide, carbon nanotubes, fullerenes or activated carbon fibers.

3. The method for preparing the rare earth / alkaline earth metal composite ordered porous carbon material according to claim 2, characterized in that: In step (1), the pH of the calcium chloride solution is 7, and the concentration of the calcium chloride solution is 0.40-0.60 mol / L.

4. The method for preparing the rare earth / alkaline earth metal composite ordered porous carbon material according to claim 1, characterized in that: In step (2), the concentration of sodium hydroxide in the alkaline hydrogen peroxide solution is 0.5-1.5 mol / L, and the concentration of hydrogen peroxide is 0.25-0.75 mol / L.

5. The method for preparing the rare earth / alkaline earth metal composite ordered porous carbon material according to claim 1, characterized in that: In step (3), the concentration of the rare earth metal salt solution is 0.25-1.0 mol / L.

6. The method for preparing the rare earth / alkaline earth metal composite ordered porous carbon material according to claim 5, characterized in that: In step (3), the rare earth metal salt solution is a lanthanum nitrate solution, an yttrium nitrate solution or a cerium nitrate solution.

7. The method for preparing the rare earth / alkaline earth metal composite ordered porous carbon material according to claim 1, characterized in that: In step (3), the alkali solution is a sodium hydroxide solution with a concentration of 0.5-1.5 mol / L.

8. A rare earth / alkaline earth metal composite ordered porous carbon material, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 7.

9. Use of the rare earth / alkaline earth metal composite ordered porous carbon material according to claim 8 in the simultaneous treatment of water bodies contaminated by oxygen-containing inorganic salts and chromium (VI).

10. The use according to claim 9, characterized in that: The oxygen-containing inorganic salt is phosphate, arsenate, selenate or dichromate.

Citation Information

Cited By

  • Carbon-based calcium peroxide material with oxygen slow-release function as well as preparation method and application of carbon-based calcium peroxide material

    CN120289243A