Pd-O-Ce-rich interface catalyst and application of Pd-O-Ce-rich interface catalyst in catalysis of ethane-carbon dioxide oxidative dehydrogenation
By preparing a Pd/Fe bimetallic catalyst rich in Pd-O-Ce interfaces on a cerium dioxide nanoisland support, the problem of insufficient active interfaces was solved, the product yield of the ethane-carbon dioxide reaction and the H2/CO ratio of the syngas were improved, and the catalytic activity was enhanced.
Patent Information
- Application Number
- CN202411208656.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-29
AI Technical Summary
The existing bimetallic catalysts have an insufficient number of active interfaces, resulting in low yields of ethane-carbon dioxide reaction products, especially a low H2/CO ratio in the syngas, making them unsuitable as ideal feedstocks for ethylene hydroformylation.
A Pd-Fe bimetallic catalyst rich in Pd-O-Ce interfaces was prepared by loading it onto a cerium dioxide nanoisland support and adjusting the ratio and dispersion of Pd and Fe to form a Pd-CeO2 solid solution, thereby increasing the number of Pd-O-Fe interfaces.
It improved the product yield of the ethane-carbon dioxide oxidative dehydrogenation reaction, especially the H2/CO ratio of the syngas, enhanced the catalytic activity, and increased the yield of ethylene and the amount of syngas generated.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention relates to a Pd-O-Ce-rich interface catalyst and application thereof in catalyzing ethane-carbon dioxide oxidative dehydrogenation, belonging to the technical field of industrial catalysis. Background Art
[0002] With the progress of social technology and the development of economic society, the relationship between human beings, environment and energy has received more and more attention. At present, the world's energy is still dominated by fossil energy. Although the optimization of energy structure is still proceeding in an orderly manner, the contradiction and conflict between social development and energy environment is intensifying. Therefore, the efficient and clean use of fossil energy and the development of renewable clean energy have become important issues for China and even the world to solve carbon emissions and promote sustainable development. In recent decades, the increasing carbon dioxide emissions and huge shale gas reserves have attracted people's attention to the use of these low-value resources to produce high-value-added chemicals.
[0003] Low-carbon alkanes are mainly contained in natural gas, and as the cleanest fossil fuel, natural gas or shale gas has become the first choice in the development of new processes to replace petroleum routes. These limitations and defects can be avoided or reduced by using catalytic conversion technology. In addition to methane, ethane also accounts for 3%-12% of shale gas. It is of great significance to convert low-value ethane into ethylene, an important raw material for industrial production, and consuming carbon dioxide to participate in ethane dehydrogenation can also alleviate the greenhouse effect and achieve carbon dioxide emission control and reuse. Therefore, carbon dioxide-assisted ethane dehydrogenation (C2H6+CO2=C2H4+CO+H2O) is a meaningful and industrially valuable route. In addition, ethane dry reforming reaction (C2H6+2CO2=4CO+3H2) will occur simultaneously. Both pathways provide opportunities to convert greenhouse gas carbon dioxide and underutilized ethane into value-added chemicals, namely synthesis gas or ethylene, which is the most important industrial chemical raw material. In addition, the formed olefins can be further converted into aromatics (i.e., benzene, toluene, and xylenes) via a tandem aromatization reaction or can be upgraded to oxygenates via downstream Fischer-Tropsch synthesis and hydroformylation processes together with the co-produced syngas.
[0004] In the past few years, researchers have developed a series of ceria-supported bimetallic catalysts for the CO2-lower alkane reaction, which show better catalytic performance than traditional catalysts. In particular, by adjusting the molar ratio of the metals in the bimetallic catalyst, selective cleavage of CH or CC bonds can be easily achieved. The atomic ratio of the metals in the bimetallic catalyst can greatly affect the selectivity of ethane dry reforming and oxidative dehydrogenation. After the Pd-O-Fe interface selectively oxidizes ethane to ethylene, the Pd-O-Ce interface activates CO2 and provides active O* species to re-oxidize the Pd 0 -Fe0 interface, while FeO x -CeO x The interface will inhibit the production of excessive active oxygen species and thus weaken the DRE selectivity. Previous studies have focused on the effect of regulating the ratio of bimetallic catalysts on the reaction selectivity, but there is little research on the regulation of the support angle. At the same time, although there have been studies that directly react the products in series to prepare C3 products such as propanol and propionaldehyde through ethylene hydroformylation, due to the existence of the RWGS reaction, the H2 / CO ratio of the syngas in the product is relatively low and cannot be used as an ideal raw material for ethylene hydroformylation. Therefore, how to increase the number of active interfaces in these bimetallic catalysts to further improve the corresponding product yield has not actually been solved. Summary of the invention
[0005] The purpose of the present invention is to provide a Pd, Fe bimetallic catalyst loaded on a ceria nano-island carrier and rich in Pd-O-Ce interface, which can be used for efficient catalytic carbon dioxide-ethane oxidative dehydrogenation.
[0006] The method for preparing a Pd, Fe bimetallic catalyst loaded on a ceria nano-island carrier and rich in Pd-O-Ce interface provided by the present invention comprises the following steps: S1, preparing a silica carrier loaded with ceria nano-islands; S2. Adsorbing Pd metal salt and Fe metal salt onto the silica carrier supported by the ceria nano-islands by an impregnation method, and performing calcination in an air atmosphere and high-temperature reduction in a hydrogen-argon atmosphere, respectively, until the temperature is cooled to room temperature.
[0007] In step S1, the ceria nano-islands-loaded silica carrier is prepared by the following steps: The Ce metal salt is adsorbed on the silica aerogel by an electrostatic adsorption method, and then the solvent is removed by vacuum extraction, and the aerogel is dried and air-baked to obtain the aerogel.
[0008] Preferably, the specific surface area of the silica aerogel is not less than 400 m 2 / g; The Ce content in the silica carrier supported by the cerium dioxide nano-islands is 3-35%; The Ce metal salt is cerium nitrate; Ammonia water was used to adjust the pH value of the system to 7.87~8.43.
[0009] In step S2, the Pd metal salt is palladium nitrate; The mass ratio of the silica carrier supported by the cerium dioxide nano-islands to the Pd in the Pd metal salt is 1:0.02-1:0.01; The Pd metal salt solution is prepared using water.
[0010] In step S2, the Fe metal salt is ferric nitrate; The mass ratio of the silica carrier supported by the ceria nano-islands to Fe in the Fe metal salt is 1:0.032-1:0.016; The Fe metal salt solution is prepared with water.
[0011] In step S2, the conditions for calcining in air atmosphere are: in a static air atmosphere, the temperature is 350-450°C, the heating rate is 1-5°C / min, and the time is 1-3 h.
[0012] The conditions for the high-temperature reduction in a hydrogen-argon atmosphere are: in a hydrogen-argon atmosphere, the temperature is 500-600° C., the heating rate is 5-10° C. / min, and the time is 1-2 h.
[0013] In the Pd and Fe bimetallic catalyst loaded on the ceria nano-island carrier and rich in Pd-O-Ce interface prepared by the present invention, the loading amount of Pd is 1-2%, and the loading amount of Fe is 1.6-3.2%.
[0014] The Pd and Fe bimetallic catalyst provided by the present invention and rich in Pd-O-Ce interface and supported on a ceria nano-island carrier can be used to catalyze efficient carbon dioxide-ethane oxidative dehydrogenation, with argon as the balance gas, and the catalytic mechanism is as follows: Under the appropriate ceria loading and dispersion, part of the loaded Pd and Fe bimetallic will form PdFen alloy. Sufficient ceria loading improves the dispersion of PdFen alloy, prevents the appearance of large alloy particles, and increases the proportion of Pd-O-Fe interface. More importantly, part of Pd will interact with ceria to form a solid solution. When the ceria loading is moderate, the proportion of Pd-CeO2 solid solution on the surface is the highest, and the proportion of Pd-O-Ce interface responsible for the production of synthesis gas is also the highest, so the production of synthesis gas can be greatly increased.
[0015] Under the catalysis of Pd and Fe bimetallic catalysts, carbon dioxide and ethane undergo oxidative dehydrogenation reaction in a fixed bed reactor to produce ethylene and synthesis gas.
[0016] The volume ratio of the carbon dioxide to the ethane is 2:1-1:2; the reaction is carried out in an atmosphere of argon and nitrogen; The oxidative dehydrogenation reaction conditions are: temperature of 580-620°C, reaction pressure of normal pressure to 0.5 MPa, total mass space velocity of 12-120 L·(g cat h) -1 , time is 15-60h.
[0017] Compared with the prior art, the present invention has the following advantages and beneficial effects: The present invention provides for the first time a Pd, Fe bimetallic catalyst loaded on a ceria nano-island carrier and rich in Pd-O-Ce interface.
[0018] The Pd-O-Ce interface-rich Pd and Fe bimetallic catalyst loaded on the ceria nano-island carrier synthesized by the present invention has a high dispersion of Pd-CeO2 solid solution on the surface and has a higher conductivity than PdFe n The supported commercial ceria catalyst has more Pd-O-Ce interfaces, which is beneficial for catalyzing the ethane-carbon dioxide reaction to produce synthesis gas.
[0019] The Pd and Fe bimetallic catalyst loaded on a ceria nano-island carrier and rich in Pd-O-Ce interface synthesized by the present invention produces appropriate carbon deposition at some Pd-SiO2 sites and silanol sites in the ethane-carbon dioxide reaction and simultaneously produces a large amount of hydrogen, thereby adjusting the H2 / CO ratio of the product synthesis gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is an energy dispersive spectrometer (EDS) of the Pd, Fe bimetallic catalyst loaded on a ceria nano-island support and rich in Pd-O-Ce interface prepared in Example 4 of the present invention under spherical aberration corrected high-angle annular dark field scanning transmission electron microscopy (AC HAADF-STEM) mode.
[0021] Figure 2 This is the X-ray diffraction spectrum (XRD) of the Pd, Fe bimetallic catalyst loaded on the ceria nano-island support and rich in Pd-O-Ce interface prepared in Example 1-7 of the present invention.
[0022] Figure 3 The Pd-O-Ce interface-rich Pd and Fe bimetallic catalyst loaded on the ceria nano-island support prepared in Example 1-7 of the present invention before and after loading Ce 3+ Proportional difference (denoted as △Ce 3+ , represents the ratio of oxygen vacancies generated after loading and the Pd-O v -Ce interface) and Pd 2+ Plot of the fitted data for peak areas.
[0023] Figure 4 This is a performance diagram of the ethane-carbon dioxide reaction catalyzed by the Pd, Fe bimetallic catalyst supported on the ceria nano-island support and rich in Pd-O-Ce interface prepared in Examples 1-7 of the present invention, wherein the main variable is the loading amount of the ceria support. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with specific embodiments. The given examples are only for illustrating the present invention, but not for limiting the scope of the present invention.
[0025] The experimental methods in the following examples, unless otherwise specified, are conventional methods and are performed according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0026] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0027] The specific surface area of the fumed silica used in the following examples is 400 m 2 / g.
[0028] Example 1. Preparation of Pd, Fe bimetallic catalysts loaded on ceria nano-islands with rich Pd-O-Ce interface and catalysis of ethane-carbon dioxide oxidative dehydrogenation Add 360 mg of fumed silica to 100 mL of water, ultrasonicate for 10 minutes, then add 34.5 mg of cerium nitrate hexahydrate, stir until dissolved, add 2 mol / L ammonia water to adjust the pH to 8.43, stir for 3 minutes, vacuum filter and dry naturally, transfer to a muffle furnace, and heat to 600 °C at a rate of 5 °C / min in a static air atmosphere and maintain for 12 h. Grind at room temperature to obtain 3%wt CeO2 / SiO2 (denoted as 3CeO2 / SiO2).
[0029] 100 mg3CeO2 / SiO2 carrier was added to 20 mL of water, and 0.25 mL of palladium nitrate containing 1.52 mg of Pd and 0.1 mL of dilute nitric acid aqueous solution and 0.157 mL of ferric nitrate aqueous solution containing 2.40 mg of Fe were added thereto, stirred at room temperature for 2 h, and then transferred to a muffle furnace after being spun dry. In a static air atmosphere, the temperature was raised to 400 ° C at a rate of 2 ° C / min and maintained for 2 h, and then transferred to a tube furnace. In a 10% H2 / Ar atmosphere, the temperature was raised to 500 ° C at a rate of 10 ° C / min and maintained for 1 h. In the obtained Pd and Fe bimetallic catalyst, the Pd loading was 1.5%, and the Fe loading was 2.3%.
[0030] In a quartz tube with an outer diameter of 8 mm, an inner diameter of 6 mm, and a length of 50 cm, add 270 mg of quartz sand and 30 mg of catalyst that are evenly mixed, and heat to 600 ° C at a heating rate of 10 ° C / min under argon atmosphere, switch to the reaction raw gas with a total flow rate of 12 mL / min (ethane 2.4 mL / min, carbon dioxide 2.4 mL / min, nitrogen 1.2 mL / min, argon 6 mL / min), pressure 0.1 MPa, and perform component detection by gas chromatography at regular intervals.
[0031] Figure 1 The energy spectrum (EDS) of the Pd and Fe bimetallic catalyst loaded on the ceria nano-island support and rich in Pd-O-Ce interface prepared in Example 1 under the spherical aberration corrected high-angle annular dark field scanning transmission electron microscope (AC HAADF-STEM) mode; it can be seen that in the EDS mode, the red Ce signal, the yellow Fe signal, and the pink Pd signal are uniformly mixed without obvious agglomeration, showing that the Pd-CeO2 solid solution, Pd-FeO x , Fe-CeO2 interaction and Pd-CeO2 solid solution, Pd-FeO x High dispersion.
[0032] Example 2 Preparation of Pd, Fe bimetallic catalysts loaded on ceria nano-islands with rich Pd-O-Ce interface and catalytic ethane-carbon dioxide oxidative dehydrogenation Add 360 mg of fumed silica to 100 mL of water, ultrasonicate for 10 minutes, then add 71.2 mg of cerium nitrate hexahydrate, stir until dissolved, add 2 mol / L ammonia water to adjust the pH to 8.32, stir for 3 minutes, vacuum filter and dry naturally, transfer to a muffle furnace, and heat to 600 °C at a rate of 5 °C / min in a static air atmosphere and maintain for 12 h. Grind at room temperature to obtain 6%wt CeO2 / SiO2 (referred to as 6CeO2 / SiO2).
[0033] 100 mg of 6CeO2 / SiO2 carrier was added to 20 mL of water, and 0.25 mL of palladium nitrate containing 1.52 mg of Pd and 0.1 mL of dilute nitric acid aqueous solution and 0.157 mL of ferric nitrate aqueous solution containing 2.40 mg of Fe were added thereto, stirred at room temperature for 2 h, and then transferred to a muffle furnace after being spun dry. In a static air atmosphere, the temperature was raised to 400 ° C at a rate of 2 ° C / min and maintained for 2 h, and then transferred to a tube furnace. In a 10% H2 / Ar atmosphere, the temperature was raised to 500 ° C at a rate of 10 ° C / min and maintained for 1 h. In the obtained Pd and Fe bimetallic catalyst, the Pd loading was 1.5%, and the Fe loading was 2.3%.
[0034] In a quartz tube with an outer diameter of 8 mm, an inner diameter of 6 mm, and a length of 50 cm, add 270 mg of quartz sand and 30 mg of catalyst that are evenly mixed, and heat to 600 ° C at a heating rate of 10 ° C / min under argon atmosphere, switch to the reaction raw gas with a total flow rate of 12 mL / min (ethane 2.4 mL / min, carbon dioxide 2.4 mL / min, nitrogen 1.2 mL / min, argon 6 mL / min), pressure 0.1 MPa, and perform component detection by gas chromatography at regular intervals.
[0035] Example 3 Preparation of Pd, Fe bimetallic catalysts loaded on ceria nano-islands with rich Pd-O-Ce interface and catalytic ethane-carbon dioxide oxidative dehydrogenation Add 360 mg of fumed silica to 100 mL of water, ultrasonicate for 10 minutes, then add 173.7 mg of cerium nitrate hexahydrate, stir until dissolved, add 2 mol / L ammonia water to adjust the pH to 8.20, stir for 3 minutes, vacuum filter and dry naturally, transfer to a muffle furnace, and heat to 600 °C at a rate of 5 °C / min in a static air atmosphere and maintain for 12 h. Grind at room temperature to obtain 12%wt CeO2 / SiO2 (denoted as 12CeO2 / SiO2).
[0036] 100 mg of 12CeO2 / SiO2 carrier was added to 20 mL of water, and 0.25 mL of palladium nitrate containing 6 mg of Pd and 0.1 mL of dilute nitric acid aqueous solution and 0.157 mL of ferric nitrate aqueous solution containing 2.40 mg of Fe were added thereto, stirred at room temperature for 2 h, and then transferred to a muffle furnace after being spun dry. In a static air atmosphere, the temperature was raised to 400 ° C at a rate of 2 ° C / min and maintained for 2 h, and then transferred to a tube furnace, and in a 10% H2 / Ar atmosphere, the temperature was raised to 500 ° C at a rate of 10 ° C / min and maintained for 1 h. In the obtained Pd and Fe bimetallic catalyst, the Pd loading was 1.5%, and the Fe loading was 2.3%.
[0037] In a quartz tube with an outer diameter of 8 mm, an inner diameter of 6 mm, and a length of 50 cm, add 270 mg of quartz sand and 30 mg of catalyst that are evenly mixed, and heat to 600 ° C at a heating rate of 10 ° C / min under argon atmosphere, switch to the reaction raw gas with a total flow rate of 12 mL / min (ethane 2.4 mL / min, carbon dioxide 2.4 mL / min, nitrogen 1.2 mL / min, argon 6 mL / min), pressure 0.1 MPa, and perform component detection by gas chromatography at regular intervals.
[0038] Example 4. Preparation of Pd, Fe bimetallic catalysts loaded on ceria nano-islands with rich Pd-O-Ce interface and catalysis of ethane-carbon dioxide oxidative dehydrogenation 360 mg of fumed silica was added to 100 mL of water. After ultrasonic treatment for 10 minutes, 396.3 mg of cerium nitrate hexahydrate was added (the Ce mass fraction was greater than 12%, which would result in adsorption saturation and about 40% of Ce would be lost). After stirring until dissolved, 2 mol / L of ammonia water was added dropwise to adjust the pH to 8.08. The mixture was stirred for 3 minutes, vacuum filtered and dried naturally, and then transferred to a muffle furnace. In a static air atmosphere, the temperature was raised to 600 °C at a rate of 5 °C / min and maintained for 12 h. After grinding at room temperature, 15%wt CeO2 / SiO2 (referred to as 15CeO2 / SiO2, ).
[0039] 100 mg of 15CeO2 / SiO2 carrier was added to 20 mL of water, and 0.25 mL of palladium nitrate containing 1.52 mg of Pd and 0.1 mL of dilute nitric acid aqueous solution and 0.157 mL of ferric nitrate aqueous solution containing 2.40 mg of Fe were added thereto, stirred at room temperature for 2 h, and then transferred to a muffle furnace after being spun dry. In a static air atmosphere, the temperature was raised to 400 ° C at a rate of 2 ° C / min and maintained for 2 h, and then transferred to a tube furnace, and in a 10% H2 / Ar atmosphere, the temperature was raised to 500 ° C at a rate of 10 ° C / min and maintained for 1 h. In the obtained Pd and Fe bimetallic catalyst, the Pd loading was 1.5%, and the Fe loading was 2.3%.
[0040] In a quartz tube with an outer diameter of 8 mm, an inner diameter of 6 mm, and a length of 50 cm, add 270 mg of quartz sand and 30 mg of catalyst that are evenly mixed, and heat to 600 ° C at a heating rate of 10 ° C / min under argon atmosphere, switch to the reaction raw gas with a total flow rate of 12 mL / min (ethane 2.4 mL / min, carbon dioxide 2.4 mL / min, nitrogen 1.2 mL / min, argon 6 mL / min), pressure 0.1 MPa, and perform component detection by gas chromatography at regular intervals.
[0041] Example 5. Preparation of Pd, Fe bimetallic catalysts loaded on ceria nano-islands with rich Pd-O-Ce interface and catalytic ethane-carbon dioxide oxidative dehydrogenation Add 360 mg of fumed silica to 100 mL of water, ultrasonicate for 10 minutes, then add 627.6 mg of cerium nitrate hexahydrate (Ce mass fraction greater than 12% will be adsorbed saturated, and about 40% of Ce will be lost), stir until dissolved, add 2 mol / L ammonia water to adjust the pH to 8.00, stir for 3 minutes, vacuum filter and dry naturally, transfer to a muffle furnace, and heat to 600°C at a rate of 5°C / min in a static air atmosphere and maintain for 12 h. Grind at room temperature to obtain 20%wt CeO2 / SiO2 (denoted as 20CeO2 / SiO2).
[0042] 100 mg of 20CeO2 / SiO2 carrier was added to 20 mL of water, and 0.25 mL of palladium nitrate containing 1.52 mg of Pd and 0.1 mL of dilute nitric acid aqueous solution and 0.157 mL of ferric nitrate aqueous solution containing 2.40 mg of Fe were added thereto, stirred at room temperature for 2 h, and then transferred to a muffle furnace after being spun dry. In a static air atmosphere, the temperature was raised to 400 ° C at a rate of 2 ° C / min and maintained for 2 h, and then transferred to a tube furnace, and in a 10% H2 / Ar atmosphere, the temperature was raised to 500 ° C at a rate of 10 ° C / min and maintained for 1 h. In the obtained Pd and Fe bimetallic catalyst, the Pd loading was 1.5%, and the Fe loading was 2.3%.
[0043] In a quartz tube with an outer diameter of 8 mm, an inner diameter of 6 mm, and a length of 50 cm, add 270 mg of quartz sand and 30 mg of catalyst that are evenly mixed, and heat to 600 ° C at a heating rate of 10 ° C / min under argon atmosphere, switch to the reaction raw gas with a total flow rate of 12 mL / min (ethane 2.4 mL / min, carbon dioxide 2.4 mL / min, nitrogen 1.2 mL / min, argon 6 mL / min), pressure 0.1 MPa, and perform component detection by gas chromatography at regular intervals.
[0044] Example 6 Preparation of Pd, Fe bimetallic catalysts loaded on ceria nano-islands with rich Pd-O-Ce interface and catalytic ethane-carbon dioxide oxidative dehydrogenation Add 360 mg of fumed silica to 100 mL of water, and after ultrasonication for 10 minutes, add 1029.8 mg of cerium nitrate hexahydrate (Ce mass fraction greater than 12% will be adsorbed saturated, and about 40% of Ce will be lost), stir until dissolved, add 2 mol / L ammonia water to adjust the pH to 7.94, stir for 3 minutes, vacuum filter and dry naturally, transfer to a muffle furnace, and in a static air atmosphere, heat to 600°C at a rate of 5°C / min and maintain for 12 h. Grind at room temperature to obtain 27%wt CeO2 / SiO2 (denoted as 27CeO2 / SiO2).
[0045] 100 mg of 27CeO2 / SiO2 carrier was added to 20 mL of water, and 0.25 mL of palladium nitrate containing 1.52 mg of Pd and 0.1 mL of dilute nitric acid aqueous solution and 0.157 mL of ferric nitrate aqueous solution containing 2.40 mg of Fe were added thereto, stirred at room temperature for 2 h, and then transferred to a muffle furnace after being spun dry. In a static air atmosphere, the temperature was raised to 400 ° C at a rate of 2 ° C / min and maintained for 2 h, and then transferred to a tube furnace, and in a 10% H2 / Ar atmosphere, the temperature was raised to 500 ° C at a rate of 10 ° C / min and maintained for 1 h. In the obtained Pd and Fe bimetallic catalyst, the Pd loading was 1.5%, and the Fe loading was 2.3%.
[0046] In a quartz tube with an outer diameter of 8 mm, an inner diameter of 6 mm, and a length of 50 cm, add 270 mg of quartz sand and 30 mg of catalyst that are evenly mixed, and heat to 600 ° C at a heating rate of 10 ° C / min under argon atmosphere, switch to the reaction raw gas with a total flow rate of 12 mL / min (ethane 2.4 mL / min, carbon dioxide 2.4 mL / min, nitrogen 1.2 mL / min, argon 6 mL / min), pressure 0.1 MPa, and perform component detection by gas chromatography at regular intervals.
[0047] Example 7. Preparation of Pd, Fe bimetallic catalysts loaded on ceria nano-islands with rich Pd-O-Ce interface and catalysis of ethane-carbon dioxide oxidative dehydrogenation Add 360 mg of fumed silica to 100 mL of water, and then add 1673.6 mg of cerium nitrate hexahydrate (Ce mass fraction greater than 12% will be adsorbed saturated, and about 40% of Ce will be lost) after ultrasonic treatment for 10 minutes. Stir until dissolved, add 2 mol / L ammonia water to adjust the pH to 7.87, stir for 3 minutes, vacuum filter and dry naturally, transfer to a muffle furnace, and heat to 600 ° C at a rate of 5 ° C / min in a static air atmosphere and maintain for 12 h. Grind at room temperature to obtain 35%wt CeO2 / SiO2 (denoted as 35CeO2 / SiO2).
[0048] 100 mg of 35CeO2 / SiO2 carrier was added to 20 mL of water, and 0.25 mL of palladium nitrate containing 1.52 mg of Pd and 0.1 mL of dilute nitric acid aqueous solution and 0.157 mL of ferric nitrate aqueous solution containing 2.40 mg of Fe were added thereto, stirred at room temperature for 2 h, and then transferred to a muffle furnace after being spun dry. In a static air atmosphere, the temperature was raised to 400 ° C at a rate of 2 ° C / min and maintained for 2 h, and then transferred to a tube furnace. In a 10% H2 / Ar atmosphere, the temperature was raised to 500 ° C at a rate of 10 ° C / min and maintained for 1 h. In the obtained Pd and Fe bimetallic catalyst, the Pd loading was 1.5%, and the Fe loading was 2.3%.
[0049] In a quartz tube with an outer diameter of 8 mm, an inner diameter of 6 mm, and a length of 50 cm, add 270 mg of quartz sand and 30 mg of catalyst that are evenly mixed. Heat the tube to 600 °C at a heating rate of 10 °C / min under argon atmosphere, switch to reaction raw gas with a total flow rate of 12 mL / min (ethane 2.4 mL / min, carbon dioxide 2.4 mL / min, nitrogen 1.2 mL / min, argon 6 mL / min), and a pressure of 0.1 MPa. Perform component detection by gas chromatography at regular intervals.
[0050] Figure 1The high-angle annular dark field scanning transmission electron microscope energy spectrum (HAADF-STEM EDS) of the Pd and Fe bimetallic catalyst loaded on the ceria nano-island support and rich in Pd-O-Ce interface prepared in Example 4 of the present invention shows that when the Ce loading is moderate, the Ce signal and the Pd signal highly overlap, indicating that the surface Pd and Ce form a solid solution and are well dispersed, forming more Pd-O-Ce interfaces.
[0051] Figure 2 The X-ray diffraction spectra (XRD) of the Pd and Fe bimetallic catalysts loaded on the ceria nano-island carrier and rich in Pd-O-Ce interface prepared in Examples 1-7 of the present invention show that as the Ce loading gradually increases, the particle size of the ceria nano-islands increases and the dispersion decreases; PdFe n The particle size of alloy particles decreases and the dispersion increases.
[0052] Figure 3 The Pd-O-Ce interface-rich Pd and Fe bimetallic catalyst loaded on the ceria nano-island support prepared in Example 1-7 of the present invention before and after loading Ce 3+ Proportional difference (denoted as △Ce 3+ , represents the ratio of oxygen vacancies generated after loading and the Pd-O v -Ce interface) and Pd 2+ The fitted data of the peak area shows that as the Ce loading increases, △Ce 3+ At the same time, the Pd corresponding to the Pd-CeO2 solid solution 2+ The ratio gradually increases, indicating that the overall Pd-CeO2 solid solution ratio increases, but the cerium dioxide dispersion decreases, and the amount of Pd entering the subsurface increases, indicating that the surface Pd-CeO2 solid solution ratio decreases, that is, the Pd-O-Ce interface ratio decreases.
[0053] Figure 4 The performance diagram of the ethane-carbon dioxide reaction catalyzed by the Pd, Fe bimetallic catalyst loaded on the ceria nano-island carrier and rich in Pd-O-Ce interface prepared in Examples 1-7 of the present invention, the main variable is the loading of ceria carrier. It can be seen that the product yield shows a volcano-shaped relationship with ΔCe 3+ The trend of change is consistent, indicating that the Pd-O-Ce interface is closely related to the synthesis gas yield; when the cerium dioxide loading is moderate, the catalyst has the highest proportion of Pd-O-Ce interface and exhibits the best synthesis gas activity. At the same time, the Pd-O-Fe interface ratio is also the highest, which also ensures that the ethylene yield is at a high level.
Claims
1. A method for preparing a Pd, Fe bimetallic catalyst loaded on a ceria nano-island support and rich in Pd-O-Ce interface, comprising the following steps: S1, preparing a silica carrier loaded with ceria nano-islands; S2. Adsorbing Pd metal salt and Fe metal salt onto the silica carrier supported by the ceria nano-islands by an impregnation method, and performing calcination in an air atmosphere and high-temperature reduction in a hydrogen-argon atmosphere, respectively, until the temperature is cooled to room temperature.
2. The preparation method according to claim 1, characterized in that: In step S1, the ceria nano-islands-loaded silica carrier is prepared by the following steps: The Ce metal salt is adsorbed on the silica aerogel by an electrostatic adsorption method, and then the solvent is removed by vacuum pumping, and the aerogel is dried and air-baked to obtain the aerogel.
3. The preparation method according to claim 2, characterized in that: The specific surface area of the silica aerogel is not less than 400 m 2 / g; The Ce content in the silica carrier supported by the cerium dioxide nano-islands is 3-35%; The Ce metal salt is cerium nitrate; Ammonia water was used to adjust the pH value of the system to 7.87~8.
43.
4. The preparation method according to any one of claims 1 to 3, characterized in that: In step S2, the Pd metal salt is palladium nitrate; The mass ratio of the silica carrier supported by the cerium dioxide nano-islands to the Pd in the Pd metal salt is 1:0.02-1:0.01; The Pd metal salt solution is prepared using water.
5. The preparation method according to any one of claims 1 to 4, characterized in that: In step S2, the Fe metal salt is ferric nitrate; The mass ratio of the silica carrier supported by the ceria nano-islands to Fe in the Fe metal salt is 1:0.0314-1:0.0157; The Fe metal salt solution is prepared with water.
6. The preparation method according to any one of claims 1 to 5, characterized in that: In step S2, the conditions for calcining in air atmosphere are: in a static air atmosphere, the temperature is 350-450°C, the heating rate is 1-5°C / min, and the time is 1-3h.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The conditions for the high-temperature reduction in a hydrogen-argon atmosphere are: in a hydrogen-argon atmosphere, the temperature is 500-600° C., the heating rate is 5-10° C. / min, and the time is 1-2 h.
8. A Pd, Fe bimetallic catalyst rich in Pd-O-Ce interface and supported on a ceria nano-island support, prepared by the method of any one of claims 1 to 7; In the Pd and Fe bimetallic catalyst, the loading amount of Pd is 1%-2%, and the loading amount of Fe is 1.6-3.2%.
9. Use of the Pd and Fe bimetallic catalyst according to claim 8 in catalyzing the ethane-carbon dioxide oxidative dehydrogenation reaction: Under the catalysis of the Pd and Fe bimetallic catalyst, carbon dioxide and ethane undergo oxidative dehydrogenation reaction in a fixed bed reactor to obtain ethylene and synthesis gas.
10. The use according to claim 9, characterized in that: The volume ratio of the carbon dioxide to the ethane is 2:1-1:2; the reaction is carried out in an atmosphere of argon and nitrogen; The oxidative dehydrogenation reaction conditions are: temperature of 580-620°C, reaction pressure of normal pressure to 0.5 MPa, total mass space velocity of 12-120 L·(g cat h) -1 , time is 15-60h.