Copper-based catalyst as well as preparation method and application thereof
The preparation of copper-zinc-aluminum nanofiber catalysts through electrospinning methods solved the problems of complex processes and low activity of existing copper-based catalysts, and achieved efficient carbon dioxide hydrogenation and methanol reaction, which significantly improved the catalytic performance.
Patent Information
- Application Number
- CN202411403381.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-29
AI Technical Summary
The existing copper-based catalyst preparation process has a long process and a large amount of wastewater, and the resulting catalyst has poor controllability, low specific surface area and low activity.
The copper-zinc-aluminum nanofiber catalyst was prepared by electrospinning. By mixing the copper source, zinc source and aluminum source with polymer and solvent, and post-calcining treatment was performed to prepare high specific surface area and excellent reactivity. copper-based catalyst.
The preparation process is simplified and the wastewater generation is reduced. The obtained catalyst has good copper dispersion, uniform nanometer size, and large specific surface area, which significantly improves the single-pass conversion rate of carbon dioxide hydrogenation and the selectivity of methanol reaction.
Smart Images

Figure CN119034750A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of catalysts, and in particular to a copper-based catalyst and a preparation method and application thereof. Background Art
[0002] Industrial methanol has a wide range of uses. In addition to being a good solvent for many organic substances, it is mainly used in the industrial production of synthetic fibers, formaldehyde, plastics, medicines, pesticides, dyes, synthetic proteins, etc. It is a basic organic chemical raw material. Almost all industrial methanol synthesis adopts the method of pressurized catalytic hydrogenation of carbon monoxide. The process includes gasification, synthesis purification, methanol synthesis and crude methanol distillation. The purification process of crude methanol includes distillation and chemical treatment. Chemical treatment mainly uses alkali to destroy impurities that are difficult to separate during the distillation process and adjust the pH value; distillation mainly removes volatile components such as dimethyl ether, as well as non-volatile components such as ethanol, high-carbon alcohols and water. The purity after crude distillation can generally reach more than 98%.
[0003] The preparation of nanofiber materials through electrospinning technology has been one of the most important academic and technical activities in the field of materials science and technology in the world in the past decade. Electrospinning has become one of the effective ways to prepare nanomaterials due to its simple manufacturing equipment, low spinning cost, a wide variety of spinnable materials, and controllable process.
[0004] The copper-based catalyst prepared by the traditional coprecipitation method in Chinese patent CN102716749A has a complicated preparation process, produces a large amount of wastewater, and has a low yield; the prepared catalyst has poor controllability of structure, low specific surface area, and is easily deactivated. Therefore, there is an urgent need for a new method for preparing a copper-based catalyst in the art, which can obtain a highly active copper-based catalyst while simplifying the preparation process. Summary of the invention
[0005] In view of this, the present invention is committed to providing a copper-based catalyst and a preparation method and application thereof, so as to solve the problems in the prior art that the copper-based catalyst preparation process is long, the amount of wastewater is large, and the prepared copper-based catalyst has poor structural controllability, low specific surface area and low activity.
[0006] In order to solve the above technical problems, this application is implemented as follows:
[0007] The first aspect of the present invention provides a copper-based catalyst, the copper-based catalyst comprises copper-zinc-aluminum nanofibers; the copper-zinc-aluminum nanofibers contain copper oxide, zinc oxide and aluminum oxide;
[0008] The specific surface area of the copper-based catalyst is 90 to 130 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers is 0.5-2.0 μm.
[0009] Optionally, the specific surface area of the copper-based catalyst is 90 to 120 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers is 0.8-1.8 μm.
[0010] Optionally, based on the total mass of the copper-based catalyst, the copper content in the copper-based catalyst is 50-70wt%, the zinc content is 15-35wt%, and the aluminum content is 5-30wt%, calculated as oxides.
[0011] A second aspect of the present invention provides a method for preparing a copper-based catalyst, the preparation method comprising the following steps:
[0012] S1, mixing a copper source, a zinc source and an aluminum source with a high molecular polymer and a solvent to obtain a spinning solution;
[0013] S2, electrospinning the spinning solution to obtain a copper-zinc-aluminum precursor;
[0014] S3, calcining the copper-zinc-aluminum precursor.
[0015] Optionally, based on the total mass of the spinning solution, the copper content in the spinning solution is 5-7wt%, the zinc content in the spinning solution is 1.5-3.5wt%, and the aluminum content in the spinning solution is 0.5-3wt%; based on the total mass of the spinning solution, the content of the high molecular polymer is 5-15wt%.
[0016] Optionally, the copper source includes at least one of copper nitrate, copper sulfate and copper chloride; and / or, the zinc source includes at least one of zinc nitrate, zinc sulfate and zinc chloride; and / or, the aluminum source includes at least one of aluminum nitrate, aluminum sulfate and aluminum chloride; and / or, the high molecular polymer is selected from at least one of polyvinyl alcohol, polyethylene glycol and polyvinyl pyrrolidone; and / or, the solvent is water.
[0017] Optionally, in step S2, the conditions for the electrospinning include: relative humidity of 20-80%, temperature of 15-70°C, positive voltage of 10-50kV, negative voltage of 10-50kV, and electrospinning distance of 5-15cm; in step S3, the calcination treatment is carried out in an oxygen-containing atmosphere; the conditions for the calcination treatment include: temperature of 300-500°C and time of 2-10h.
[0018] The third aspect of the present invention provides a method for preparing methanol by hydrogenating carbon dioxide, the method comprising: introducing a first gas into a reactor filled with a catalyst for reduction reaction, and then introducing a reaction gas to carry out a reaction of hydrogenating carbon dioxide to prepare methanol; wherein the catalyst is the above-mentioned catalyst and / or a catalyst prepared according to the above-mentioned preparation method.
[0019] Optionally, the first gas includes a reducing gas and an inert gas; optionally, the reducing gas is H2; based on the total volume of the first gas, the content of the reducing gas is 5 to 10%; the reaction gas includes H2 and CO2; the volume ratio of H2 to CO2 in the reaction gas is 2 to 4:1.
[0020] Optionally, the reduction reaction conditions include: temperature of 180-250°C, time of 2-10h, gas space velocity of 1000-5000h -1 The conditions for the carbon dioxide hydrogenation reaction to produce methanol include: pressure 3.0-9.0 MPa; temperature 220-280°C; gas space velocity 2000-20000h -1 .
[0021] Through the above technical solution, the beneficial technical effects of the present invention are:
[0022] (1) The present invention adopts an electrospinning method to prepare a copper-based catalyst, which can reduce the process flow and reduce the generation of wastewater; the copper-based catalyst prepared by electrospinning has good copper dispersion, uniform nanometer size, large specific surface area, and excellent reaction activity.
[0023] (2) When the copper-based catalyst of the present invention is used in the reaction of hydrogenating carbon dioxide to produce methanol, it can significantly improve the single-pass conversion rate of carbon dioxide and the selectivity of methanol.
[0024] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but do not constitute a limitation of the present invention.
[0026] Figure 1 Shown is a process flow chart of the preparation method of the copper-based catalyst in the present invention.
[0027] Figure 2 Shown is an electron microscope scanning image of the copper-based catalyst prepared in Example 2. DETAILED DESCRIPTION
[0028] The present invention discloses a copper-based catalyst and a preparation method and application thereof. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the above. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art and are considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.
[0029] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.
[0030] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range or the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0031] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0032] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0033] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0034] In order to solve the problems in the prior art that the copper-based catalyst preparation process is long, the amount of wastewater is large, and the copper-based catalyst obtained has poor structural controllability, low specific surface area, and low activity, the present invention adopts the following technical solution:
[0035] The first aspect of the present invention provides a copper-based catalyst, the copper-based catalyst comprises copper-zinc-aluminum nanofibers; the copper-zinc-aluminum nanofibers contain copper oxide, zinc oxide and aluminum oxide;
[0036] The specific surface area of the copper-based catalyst is 90 to 130 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers is 0.5-2.0 μm.
[0037] The copper-based catalyst of the present invention has a significantly improved specific surface area, and the size of the copper-zinc-aluminum nanofibers is uniform, the copper dispersion is good, and the reaction activity is excellent. The copper-based catalyst of the present invention is applied to the carbon dioxide hydrogenation to methanol reaction, which can significantly improve the single-pass conversion rate of carbon dioxide and the selectivity of methanol.
[0038] As a preferred embodiment of the present invention, the specific surface area of the copper-based catalyst is 90 to 120 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers is 0.8-1.8 μm. In this embodiment, the reaction activity of the copper-based catalyst is significantly improved.
[0039] According to the present invention, based on the total mass of the copper-based catalyst, the copper content in the copper-based catalyst can be 50-70wt%, the zinc content can be 15-35wt%, and the aluminum content can be 5-30wt%, calculated as oxide.
[0040] The second aspect of the present invention provides a method for preparing a copper-based catalyst, such as Figure 1 As shown, the preparation method comprises the following steps:
[0041] S1, mixing a copper source, a zinc source and an aluminum source with a high molecular polymer and a solvent to obtain a spinning solution;
[0042] S2, electrospinning the spinning solution to obtain a copper-zinc-aluminum precursor;
[0043] S3, calcining the copper-zinc-aluminum precursor.
[0044] The method for preparing a copper-based catalyst of the present invention comprises mixing a copper source, a zinc source and an aluminum source with a high molecular polymer and a solvent to prepare a spinning solution, obtaining a copper-zinc-aluminum precursor by electrostatic spinning, and then calcining the collected copper-zinc-aluminum precursor to prepare a copper-based catalyst. Among them, electrostatic spinning can improve the copper dispersion, and obtain a catalyst with uniform nanofiber size, large specific surface area and excellent performance.
[0045] According to the present invention, based on the total mass of the spinning solution, the copper content in the spinning solution can be 5-7wt%, the zinc content in the spinning solution can be 1.5-3.5wt%, and the aluminum content in the spinning solution can be 0.5-3wt%, calculated as oxide.
[0046] According to the present invention, based on the total mass of the spinning solution, the content of the high molecular weight polymer may be 5 to 15 wt %.
[0047] Illustratively, the copper source may include at least one of copper nitrate, copper sulfate, and copper chloride.
[0048] Illustratively, the zinc source may include at least one of zinc nitrate, zinc sulfate, and zinc chloride.
[0049] Illustratively, the aluminum source may include at least one of aluminum nitrate, aluminum sulfate, and aluminum chloride.
[0050] Illustratively, the high molecular polymer may be selected from at least one of polyvinyl alcohol, polyethylene glycol and polyvinyl pyrrolidone.
[0051] Illustratively, the solvent may be water.
[0052] In one embodiment of the present invention, in step S2, the electrospinning conditions may include: relative humidity of 20-80%, temperature of 15-70°C, positive voltage of 10-50 kV, negative voltage of 10-50 kV, and the electrospinning distance of 5-15 cm.
[0053] In one embodiment of the present invention, in step S3, the calcination treatment may be performed in an oxygen-containing atmosphere; the conditions of the calcination treatment may include: a temperature of 300 to 500° C. and a time of 2 to 10 hours.
[0054] The third aspect of the present invention provides a method for preparing methanol by hydrogenating carbon dioxide, the method comprising: introducing a first gas into a reactor filled with a catalyst for a reduction reaction, and then introducing a reaction gas to carry out a reaction of hydrogenating carbon dioxide to prepare methanol; wherein the catalyst is a copper-based catalyst prepared by the above-mentioned preparation method and / or according to the above-mentioned copper-based catalyst.
[0055] The copper-based catalyst of the present invention is applied to the reaction of hydrogenating carbon dioxide to produce methanol, which can significantly improve the single-pass conversion rate of carbon dioxide and the selectivity of methanol. For example, the single-pass conversion rate of carbon dioxide can reach 35%, and the selectivity of methanol can reach 95%.
[0056] According to the present invention, the first gas may include a reducing gas and an inert gas; optionally, the reducing gas is H2; based on the total volume of the first gas, the content of the reducing gas may be 5 to 10%; the reaction gas may include H2 and CO2; the volume ratio of H2 to CO2 in the reaction gas may be 2 to 4:1.
[0057] According to the present invention, the reduction reaction conditions may include: a temperature of 180-250°C, a time of 2-10 hours, a gas space velocity of 1000-5000 h -1 The conditions for the carbon dioxide hydrogenation reaction to produce methanol may include: pressure 3.0-9.0 MPa; temperature 220-280°C; gas space velocity 2000-20000h -1 .
[0058] The present invention is further described in detail by way of examples. The raw materials used in the examples can be obtained through commercial sources.
[0059] Example 1
[0060] (1) Copper nitrate, zinc nitrate and aluminum nitrate are mixed to prepare a copper-zinc-aluminum salt solution (the total mass is 10 g, and the mass proportions are 50%, 35% and 15% respectively based on CuO, ZnO and Al2O3). The copper-zinc-aluminum salt solution is fully stirred with 85 g of deionized water and 5 g of polyvinyl alcohol until they are completely dissolved to obtain a spinning solution.
[0061] (2) Under the conditions of relative humidity of 20% and temperature of 15° C., the spinning solution was electrospun, the positive voltage of the electrospinning was 10 kV, the negative voltage of the electrospinning was 10 kV, and the distance of the electrospinning was 5 cm, to obtain a copper-zinc-aluminum precursor.
[0062] (3) The copper-zinc-aluminum precursor was calcined at 300° C. for 10 h to obtain a copper-based catalyst. The specific surface area of the copper-based catalyst prepared in this example was 90 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers in the copper-based catalyst is 0.5 μm.
[0063] (4) 0.5 g of copper-based catalyst was loaded into the reactor and heated for 1000 h. -1 The reducing gas (the reducing gas is a mixture of H2 and Ar, wherein the volume fraction of H2 is 8%) was introduced, and the reduction reaction was carried out at 250°C for 2h. After cooling to room temperature, the temperature was kept at 20000h. -1 The reaction gas (volume ratio of H2 to CO2 is 3) was introduced at a space velocity of 9.0 MPa, a pressure of 9.0 MPa, and a reaction temperature of 250°C to carry out the hydrogenation of carbon dioxide to methanol. The reaction activity of the catalyst is shown in Table 1.
[0064] Example 2
[0065] (1) Copper nitrate, zinc nitrate and aluminum nitrate are mixed to prepare a copper-zinc-aluminum salt solution (the total mass of CuO, ZnO and Al2O3 is 10 g, and the mass proportions are 70%, 25% and 5%, respectively). The copper-zinc-aluminum salt solution is mixed with 75 g of deionized water and 15 g of polyvinyl pyrrolidone, and stirred until completely dissolved to obtain a spinning solution.
[0066] (2) Under the conditions of relative humidity of 80% and temperature of 70° C., the spinning solution was electrospun, the positive voltage of the electrospinning was 50 kV, the negative voltage of the electrospinning was 50 kV, and the distance of the electrospinning was 15 cm to obtain a copper-zinc-aluminum precursor.
[0067] (3) The copper-zinc-aluminum precursor was calcined at 500°C for 2 h to obtain a copper-based fibrous catalyst. The electron microscope scanning image is shown in FIG. Figure 2 As shown. The specific surface area of the copper-based catalyst prepared in this example was 120 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers in the copper-based catalyst was 1.5 μm.
[0068] (4) 2 g of copper-based catalyst was loaded into the reactor and heated for 5000 h. -1 The reducing gas (the reducing gas is a mixture of H2 and Ar, wherein the volume fraction of H2 is 8%) was introduced, and the reduction reaction was carried out at 250°C for 2h. After cooling to room temperature, the temperature was kept at 2000h. -1 The reaction gas (volume ratio of H2 to CO2 is 3) was introduced at a space velocity of 9.0 MPa, a pressure of 9.0 MPa, and a reaction temperature of 250°C to carry out the hydrogenation of carbon dioxide to methanol. The reaction activity of the catalyst is shown in Table 1.
[0069] Example 3
[0070] (1) Copper nitrate, zinc nitrate and aluminum nitrate are mixed to prepare a copper-zinc-aluminum salt solution (the total mass of CuO, ZnO and Al2O3 is 10 g, and the mass proportions are 50%, 20% and 30%, respectively). The copper-zinc-aluminum salt solution is mixed with 80 g of deionized water and 10 g of polyethylene glycol, and stirred until completely dissolved to obtain a spinning solution.
[0071] (2) Under the conditions of relative humidity of 50% and temperature of 60° C., the spinning solution was subjected to electrospinning, the positive voltage of the electrospinning was 40 kV, the negative voltage of the electrospinning was 40 kV, and the distance of the electrospinning was 10 cm, to obtain a copper-zinc-aluminum precursor.
[0072] (3) The copper-zinc-aluminum precursor was calcined at 400° C. for 5 h to obtain a copper-based catalyst. The specific surface area of the copper-based catalyst prepared in this example was 130 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers in the copper-based catalyst was 2.0 μm.
[0073] (4) 1 g of copper-based catalyst was loaded into the reactor and heated for 2500 h. -1 The reducing gas (the reducing gas is a mixture of H2 and Ar, wherein the volume fraction of H2 is 8%) was introduced, and the reduction reaction was carried out at 250°C for 2 hours. After cooling to room temperature, the temperature was kept at 10,000 hours. -1 The reaction gas (volume ratio of H2 to CO2 is 3) was introduced at a space velocity of 5.0 MPa, a pressure of 5.0 MPa, and a reaction temperature of 250°C to carry out the hydrogenation of carbon dioxide to methanol. The reaction activity of the catalyst is shown in Table 1.
[0074] Example 4
[0075] (1) Copper nitrate, zinc nitrate and aluminum nitrate are mixed to prepare a copper-zinc-aluminum salt solution (the total mass of CuO, ZnO and Al2O3 is 10 g, and the mass proportions are 55%, 15% and 30%, respectively). The copper-zinc-aluminum salt solution is mixed with 82 g of deionized water and 8 g of polyethylene glycol, and stirred until completely dissolved to obtain a spinning solution.
[0076] (2) Under the conditions of relative humidity of 40% and temperature of 50° C., the spinning solution was electrospun, the positive voltage of the electrospinning was 30 kV, the negative voltage of the electrospinning was 30 kV, and the distance of the electrospinning was 12 cm to obtain a copper-zinc-aluminum precursor.
[0077] (3) The copper-zinc-aluminum precursor was calcined at 350° C. for 6 h to obtain a copper-based catalyst. The specific surface area of the copper-based catalyst prepared in this example was 100 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers in the copper-based catalyst was 1.8 μm.
[0078] (4) 1.5 g of copper-based catalyst was loaded into the reactor and heated for 3000 h. -1 The reducing gas (the reducing gas is a mixture of H2 and Ar, wherein the volume fraction of H2 is 8%) was introduced, and the reduction reaction was carried out at 250°C for 2 hours. After cooling to room temperature, the temperature was kept at 15000 h. -1 The reaction gas (volume ratio of H2 to CO2 is 3) was introduced at a space velocity of 7.0 MPa, a pressure of 7.0 MPa, and a reaction temperature of 250°C to carry out the hydrogenation of carbon dioxide to methanol. The reaction activity of the catalyst is shown in Table 1.
[0079] Example 5
[0080] (1) Copper nitrate, zinc nitrate and aluminum nitrate are mixed to prepare a copper-zinc-aluminum salt solution (the total mass is 10 g, and the mass proportions are 60%, 20%, and 20%, respectively, based on CuO, ZnO, and Al2O3). The copper-zinc-aluminum salt solution is fully stirred with 78 g of deionized water and 12 g of polyethylene glycol until they are completely dissolved to obtain a spinning solution.
[0081] (2) Under the conditions of relative humidity of 30% and temperature of 40° C., the spinning solution was electrospun, the positive voltage of the electrospinning was 20 kV, the negative voltage of the electrospinning was 20 kV, and the distance of the electrospinning was 8 cm, to obtain a copper-zinc-aluminum precursor.
[0082] (3) The copper-zinc-aluminum precursor was calcined at 450° C. for 3 h to obtain a copper-based catalyst. The specific surface area of the copper-based catalyst prepared in this example was 110 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers in the copper-based catalyst was 0.8 μm.
[0083] (4) 1.0 g of copper-based catalyst was loaded into the reactor and heated for 4000 h. -1 The reducing gas (the reducing gas is a mixture of H2 and Ar, wherein the volume fraction of H2 is 8%) was introduced, and the reduction reaction was carried out at 250°C for 2 hours. After cooling to room temperature, the temperature was kept at 5000 h. -1 The reaction gas (volume ratio of H2 to CO2 is 3) was introduced at a space velocity of 4.0 MPa, a pressure of 4.0 MPa, and a reaction temperature of 250°C to carry out the hydrogenation of carbon dioxide to methanol. The reaction activity of the catalyst is shown in Table 1.
[0084] Example 6
[0085] (1) Copper nitrate, zinc nitrate and aluminum nitrate are mixed to prepare a copper-zinc-aluminum salt solution (the total mass of CuO, ZnO and Al2O3 is 10 g, and the mass proportions are 65%, 25% and 10%, respectively). The copper-zinc-aluminum salt solution is mixed with 84 g of deionized water and 6 g of polyethylene glycol, and stirred until completely dissolved to obtain a spinning solution.
[0086] (2) Under the conditions of relative humidity of 20% and temperature of 30° C., the spinning solution was subjected to electrospinning, the positive voltage of the electrospinning was 10 kV, the negative voltage of the electrospinning was 10 kV, and the distance of the electrospinning was 13 cm, to obtain a copper-zinc-aluminum precursor.
[0087] (3) The copper-zinc-aluminum precursor was calcined at 300° C. for 7 h to obtain a copper-based catalyst. The specific surface area of the copper-based catalyst prepared in this example was 105 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers in the copper-based catalyst was 1.5 μm.
[0088] (4) 1.0 g of copper-based catalyst was loaded into the reactor and heated for 2000 h. -1 The reducing gas (the reducing gas is a mixture of H2 and Ar, wherein the volume fraction of H2 is 8%) was introduced, and the reduction reaction was carried out at 250°C for 2h. After cooling to room temperature, the reaction was heated for 20000h. -1 The reaction gas (volume ratio of H2 to CO2 is 3) was introduced at a space velocity of 3.0 MPa, a pressure of 3.0 MPa, and a reaction temperature of 250°C to carry out the hydrogenation of carbon dioxide to methanol. The reaction activity of the catalyst is shown in Table 1.
[0089] Comparative Example 1
[0090] (1) Copper nitrate, zinc nitrate and aluminum nitrate were mixed to prepare a copper-zinc-aluminum salt solution (the total mass of CuO, ZnO and Al2O3 was 10 g, and the mass proportions were 60%, 25% and 15%, respectively). The copper-zinc-aluminum salt solution was mixed with 90 g of deionized water and the mixture was fully stirred and recorded as solution A.
[0091] (2) Dissolve 20 g of alkali (a mixture of sodium carbonate and sodium hydroxide, with a molar ratio of 1:2.5) in 80 g of deionized water to obtain solution B.
[0092] (3) Solution A and solution B are added dropwise in parallel, and the dropping speeds of solution A and solution B are controlled to be 2 mL / min and 4 mL / min, respectively, to obtain a slurry containing a precipitate; the slurry is allowed to stand and age for 12 hours, filtered, and washed. The catalyst precursor is dried at 100°C for 8 hours, and calcined at 500°C for 4 hours to obtain a copper-based catalyst prepared by the co-precipitation method. The specific surface area of the copper-based catalyst prepared in this comparative example is 50 m 2 / g.
[0093] (4) 1.0 g of copper-based catalyst was loaded into the reactor and heated for 3000 h. -1 The reducing gas (the reducing gas is a mixture of H2 and Ar, wherein the volume fraction of H2 is 8%) was introduced and reduced at 250°C for 2h. After cooling to room temperature, the mixture was heated for 10000h. -1 The reaction gas (volume ratio of H2 to CO2 is 3) was introduced at a space velocity of 5.0 MPa, a pressure of 5.0 MPa, and a reaction temperature of 250°C to carry out the hydrogenation of carbon dioxide to methanol. The reaction activity of the catalyst is shown in Table 1.
[0094] Table 1
[0095] Group Carbon dioxide conversion rate (%) Methanol selectivity (%) By-product selectivity (%) Example 1 25 95 5 Example 2 35 90 10 Example 3 25 85 15 Example 4 28 87 13 Example 5 20 80 20 Example 6 32 70 30 Comparative Example 1 18 65 35
[0096] It can be seen from Table 1 that the copper-based catalyst in the embodiment of the present invention has a reaction space velocity of 2000-20000h -1The reaction of hydrogenating carbon dioxide to produce methanol was carried out under the following conditions. The single-pass conversion rate of carbon dioxide was 20-35%, and the selectivity of methanol was 70-95%. Compared with the copper-based catalyst prepared by the traditional coprecipitation method in Comparative Example 1, the copper-based catalyst prepared by electrospinning in the embodiment of the present invention had significantly improved catalytic performance when applied to the reaction of hydrogenating carbon dioxide to produce methanol.
[0097] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A copper-based catalyst, characterized in that The copper-based catalyst comprises copper-zinc-aluminum nanofibers; the copper-zinc-aluminum nanofibers contain copper oxide, zinc oxide and aluminum oxide; The specific surface area of the copper-based catalyst is 90 to 130 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers is 0.5-2.0 μm.
2. The copper-based catalyst according to claim 1, characterized in that The specific surface area of the copper-based catalyst is 90 to 120 m 2 / g, and the average radial length of the copper-zinc-aluminum nanofibers is 0.8-1.8 μm.
3. The copper-based catalyst according to claim 1, characterized in that Based on the total mass of the copper-based catalyst, the copper content in the copper-based catalyst is 50-70wt%, the zinc content is 15-35wt%, and the aluminum content is 5-30wt%, calculated as oxide.
4. A method for preparing the copper-based catalyst according to claims 1 to 3, characterized in that: The preparation method comprises the following steps: S1, mixing a copper source, a zinc source and an aluminum source with a high molecular polymer and a solvent to obtain a spinning solution; S2, electrospinning the spinning solution to obtain a copper-zinc-aluminum precursor; S3, calcining the copper-zinc-aluminum precursor.
5. The preparation method according to claim 4, characterized in that: Based on the total mass of the spinning solution, the content of copper in the spinning solution is 5-7wt%, the content of zinc in the spinning solution is 1.5-3.5wt%, and the content of aluminum in the spinning solution is 0.5-3wt% in terms of oxides; Based on the total mass of the spinning solution, the content of the high molecular weight polymer is 5-15wt%.
6. The preparation method according to claim 4, characterized in that: The copper source includes at least one of copper nitrate, copper sulfate and copper chloride; and / or, the zinc source comprises at least one of zinc nitrate, zinc sulfate and zinc chloride; and / or, the aluminum source comprises at least one of aluminum nitrate, aluminum sulfate and aluminum chloride; And / or, the high molecular polymer is at least one selected from polyvinyl alcohol, polyethylene glycol and polyvinyl pyrrolidone; And / or, the solvent is water.
7. The preparation method according to claim 4, characterized in that: In step S2, the electrospinning conditions include: relative humidity of 20-80%, temperature of 15-70°C, positive voltage of 10-50 kV, negative voltage of 10-50 kV, and electrospinning distance of 5-15 cm; In step S3, the calcination treatment is performed in an oxygen-containing atmosphere; the conditions of the calcination treatment include: a temperature of 300 to 500° C. and a time of 2 to 10 hours.
8. A method for preparing methanol by hydrogenating carbon dioxide, characterized in that: The method comprises: introducing a first gas into a reactor filled with a catalyst to carry out a reduction reaction, and then introducing a reaction gas to carry out a carbon dioxide hydrogenation to methanol reaction; Wherein, the catalyst is the catalyst according to claims 1 to 3 and / or the catalyst prepared according to the preparation method according to claims 4 to 7.
9. The method according to claim 8, characterized in that The first gas includes a reducing gas and an inert gas; optionally, the reducing gas is H2; based on the total volume of the first gas, the content of the reducing gas is 5-10%; The reaction gas includes H2 and CO2; the volume ratio of H2 to CO2 in the reaction gas is 2-4:
1.
10. The method according to claim 8, characterized in that The reduction reaction conditions include: temperature of 180-250°C, time of 2-10 hours, gas space velocity of 1000-5000 h -1 ; The conditions for the carbon dioxide hydrogenation to methanol reaction include: pressure 3.0-9.0 MPa; temperature 220-280° C.; gas space velocity 2000-20000 h -1 .
Citation Information
Patent Citations
Auxiliary agent-modified catalyst for CO-CO2 co-hydrogenation synthesis of methanol
CN102716749A