Ion exchange resin for rapidly purifying seawater as well as preparation method and application of ion exchange resin
Through the combination of modified ion exchange resin and inorganic filler, the problem of long-term metal ion interference and distillation method in seawater is solved, and rapid purified seawater and efficient tritium detection are achieved, which extends the service life of the resin.
Patent Information
- Application Number
- CN202411322275.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-29
AI Technical Summary
The prior art has metal ion interference in the detection of tritium element in seawater, resulting in a reduction in detection accuracy and a long purification time of distillation method, which cannot meet the needs of rapid purification of seawater.
Using a modified ion exchange resin, the metal ion removal capability of the resin is improved by selecting appropriate phosphonic acid monomers and amine-containing monomers, and the mechanical strength and resistance of the resin are enhanced by the addition of inorganic fillers such as alumina, silicon oxide and copper oxide. Abrasiveness, seawater purification is performed using ion exchange method instead of distillation.
It realizes rapid and efficient removal of metal ions in seawater, improves the accuracy of tritium detection, extends the service life of the resin, reduces interference with tritium detection, and maintains the resin in a high salinity and acid-base environment. stability.
Smart Images

Figure CN119034829A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of element detection in seawater, in particular to tritium element detection technology, and specifically relates to an ion exchange resin for rapidly purifying seawater and a preparation method and application thereof. Background Art
[0002] Tritium, as a radioactive isotope of hydrogen, has both natural and artificial sources. Its artificial sources mainly include tritium-containing waste liquid generated during the normal operation of nuclear power plants and nuclear contaminated water accidentally discharged from nuclear power plants. After nuclear waste water or nuclear contaminated water is discharged into the sea, tritium can enter marine organisms through drinking water, food, respiratory inhalation and skin absorption, and then enter the human body through the food chain, causing internal radiation hazards to the body. Although tritium belongs to the low radiotoxicity group, once it enters the human body, it may cause cell oxidative damage, genotoxicity, reproductive toxicity and DNA damage. Therefore, in the process of nuclear energy production, rapid and accurate monitoring of the activity concentration of tritium is crucial for environmental and public health safety.
[0003] Tritium in the environment mainly exists in the form of tritiated water (HTO). At present, liquid scintillation counting (LSC) is often used to measure the activity concentration of tritium in environmental samples, and environmental samples are generally aqueous solutions. When using LSC to test the activity concentration of tritium in environmental samples, metal ions in environmental samples may have an adverse effect on the detection process: (1) Metal ions interact with scintillation liquid to produce a quenching effect, thereby reducing the scintillation efficiency and thus reducing the intensity of the tritium signal; (2) Metal ions may react chemically with the components in the scintillation liquid, changing the performance of the scintillation liquid and affecting the overall stability and luminescence efficiency of the liquid; (3) Increase background radiation, resulting in deviations in the measurement results. Therefore, when conducting tritium activity concentration detection in environmental samples, it is necessary to purify the environmental samples to remove metal ions and improve the accuracy of tritium activity concentration detection.
[0004] Distillation is a common method for purifying environmental samples, but it takes a long time to purify samples by distillation. Current water purification methods include reverse osmosis, filtration, ion exchange and distillation. Among them, ion exchange is widely used in water softening, pure water production, wastewater purification and seawater desalination, and has the advantages of fast response, low cost and high reliability. However, to date, there have been no reports on the use of ion exchange in the treatment of seawater samples and subsequent detection of tritium. It is difficult for LSC to directly measure purified seawater samples, and tritium needs to be further concentrated by electrolytic enrichment, which also puts higher requirements on the purification of seawater. It is particularly urgent to develop a fast and efficient method for seawater purification.
[0005] The use of ion exchange to treat seawater inevitably involves the use of ion exchange resins, which can cause the following defects during use: (1) Resin particles may be damaged due to mechanical wear during long-term operation, resulting in an increase in the pressure drop of the resin bed and affecting the treatment efficiency; (2) Seawater contains a large amount of salt, which may affect the performance of the water quality, especially the removal effect of certain specific metal ions; (3) Seawater is generally weakly alkaline, and the resin is easily affected by extreme pH and temperature, resulting in resin degradation.
[0006] Therefore, it is particularly urgent to develop a fast, efficient and stable ion exchange resin for seawater purification. Summary of the invention
[0007] The purpose of the present invention is to provide an ion exchange resin for rapid purification of seawater, and a preparation method and application thereof, so as to solve the problem of the long time required for the above-mentioned seawater sample purification method. The present invention uses an ion exchange method to replace the existing distillation method to purify seawater samples, and the purification time is short. The prepared ion exchange resin not only has a good purification effect on seawater samples, but also has excellent mechanical strength and environmental resistance, and has a long service life.
[0008] To achieve the above object, the first aspect of the present invention provides an ion exchange resin for rapidly purifying seawater. The ion exchange resin comprises the following raw materials in parts by weight:
[0009] MB-20 resin 100-150 parts;
[0010] 5-10 parts of phosphonic acid monomer;
[0011] 3-5 parts of amine-containing monomer;
[0012] 30-40 parts of inorganic filler;
[0013] 15-20 parts of silane coupling agent;
[0014] The phosphonic acid monomers include aminotrimethylenephosphonic acid, hydroxyethylidene diphosphonic acid and iminobis(methylenephosphonic acid) in a mass ratio of (8-10):(4-6):1;
[0015] The amine-containing monomer includes diethylamine, triethylenediamine and acrylamide in a mass ratio of 1:(5-8):(1-3);
[0016] The inorganic filler includes aluminum oxide, silicon dioxide, calcium phosphate and copper oxide in a mass ratio of (12-15):(3-6):(1-3):(8-12);
[0017] The silane coupling agent includes N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and 3-(2-aminoethylamino)propyltrimethoxysilane in a mass ratio of (1-3):(1-3):(1-3).
[0018] In order to test the activity concentration of tritium in a liquid sample, liquid scintillation counting (LSC) is often used. However, the metal ions contained in the liquid sample itself during the LSC test will affect the accuracy of the test result, so it is necessary to remove the metal ions in the liquid sample before the formal test. The existing distillation method has the disadvantage of a long time to purify the sample. Based on this, the present invention finds that the ion exchange method in the commonly used water treatment method has the advantages of rapid response and low cost, and there is no report on the use of the ion exchange method for purifying liquid samples during the LSC test.
[0019] Although there are many existing ion exchange resins, they have different effects when applied to different fields. The present invention selects five commercially available resins to purify seawater, including MB-20, MB-106UP, MB-450, T-42 or CH-99 resins. By testing the conductivity of seawater treated with the above resins, it is found that the conductivity of seawater treated with MB-20 resin is the lowest. In addition, after testing the tritium activity concentration of the purified seawater, it is found that the test results are basically consistent with the commonly used distillation method, indicating that the resin selected by the present invention has a good purification effect and has no adverse effect on the detection of tritium.
[0020] The present invention has found that although MB-20 resin can remove metal ions in seawater to a certain extent, the removal of aluminum ions and magnesium ions is still relatively limited. Based on this, the present invention has modified MB-20 resin. The present invention selects three phosphonic acid monomers, namely aminotrimethylenephosphonic acid, hydroxyethylidene diphosphonic acid and iminobis(methylenephosphonic acid), to improve the removal ability of ion exchange resin for aluminum ions and magnesium ions. Analysis of the reasons: Each phosphonic acid monomer contains at least one phosphonic acid group, which can form stable complexes with metal ions, especially for high-valent metal ions such as aluminum ions and magnesium ions. By adding a variety of phosphonic acid monomers, the number of active sites on the resin surface can be increased, thereby increasing the overall adsorption capacity of the resin. The present invention can also optimize the selective adsorption capacity of the resin for specific metal ions by adjusting the ratio of different phosphonic acid monomers. For example, some phosphonic acid monomers may be more inclined to adsorb aluminum ions, while others may be more inclined to adsorb magnesium ions.
[0021] The present invention has been further studied and found that although the above-mentioned resin can improve the removal efficiency of metal ions such as sodium ions, potassium ions, magnesium ions and aluminum ions in seawater, as the resin is used for a longer time, the resin particles will be mechanically worn during long-term operation, resulting in not only a decrease in the treatment efficiency of seawater, but also a significant decrease in the removal effect of metal ions in seawater. In view of this problem, the present invention adds inorganic fillers, including alumina, silica, calcium phosphate and copper oxide, to increase the mechanical strength and wear resistance of the ion exchange resin. Analysis of the reasons: Alumina nanowires have high strength and rigidity, which can significantly increase the mechanical strength of the resin and reduce wear. Silica provides additional hardness and stability, which helps to resist wear. Copper oxide nanochains enhance the structural strength of the resin, reduce the relative movement between particles, and thus reduce wear. Nano-scale alumina and silica can also fill the gaps between resin particles, reduce friction between particles, and improve the wear resistance of the resin. Copper oxide nanochains can also form a protective layer through their special structure to reduce the wear of the resin during the treatment process. The inorganic filler can also improve the flow characteristics of the resin bed as a whole, reduce the pressure drop when water passes through the resin bed, and thus reduce wear. The present invention can reduce the degradation rate of the resin and extend its service life by enhancing the mechanical properties and stability of the resin. Higher mechanical strength means that the resin is less susceptible to damage during the regeneration process, thereby reducing the regeneration frequency.
[0022] The present invention also found that seawater has high salinity and weak alkalinity. The ion exchange resin used for treating seawater for a long time will be affected by the salt and alkaline environment, resulting in poor seawater treatment capacity and treatment effect. Based on this, the present invention continues to add amine-containing monomers while adding phosphonic acid monomers to improve the salt resistance and environmental resistance of the ion exchange resin. Analysis of the reasons: The amine groups in the present invention (such as those present in diethylamine and triethylenediamine) can form stable complexes with cations in salts, thereby improving the stability of the resin in a high-salinity environment. At the same time, acrylamide has strong hydrophilicity, which helps the resin maintain its hydrophilicity under high-salinity conditions and reduces the impact of salt on the performance of the resin. The amine groups of the present invention can be protonated or deprotonated under different pH conditions, which helps the resin maintain its structural stability under acidic or alkaline conditions. At the same time, acrylamide also has good chemical stability, which helps the resin maintain its performance under acidic and alkaline environments.
[0023] Preferably, the aluminum oxide is an aluminum oxide nanowire with a diameter of 4 nm and a length of 1 μm.
[0024] Preferably, the diameter of the silicon dioxide is 65 to 85 nm.
[0025] Preferably, the copper oxide is a copper oxide nanochain with a diameter of 35 to 42 nm and a length of 1.0 to 1.6 μm.
[0026] The present invention also defines the morphology of alumina, the diameter of silica, and the morphology of copper oxide, which not only improves the mechanical strength of the ion exchange resin, but also improves its environmental resistance and salt resistance. Analysis of the reasons: First, the inorganic fillers alumina and copper oxide themselves have good chemical stability, and can remain stable even in acidic and alkaline environments, which helps the resin maintain its structural integrity and basic functions. In addition, the nanoscale fillers have good dispersibility in the resin, which helps to improve the overall environmental resistance of the resin. The characteristics of different fillers in the present invention can complement and work synergistically. For example, alumina provides mechanical strength, silica provides buffering, calcium phosphate provides additional chemical stability, and copper oxide provides special structural strength, which plays an important role in improving the comprehensive performance of ion exchange resins. Therefore, there may be interactions between alumina, silica, calcium phosphate and copper oxide in the present invention, which work together on the microstructure of the resin to improve its overall performance.
[0027] Preferably, the acrylamide is one of N-methyl acrylamide and N-hydroxymethyl acrylamide.
[0028] A second aspect of the present invention provides a method for preparing an ion exchange resin for rapidly purifying seawater, comprising the following steps:
[0029] a) adding MB-20 resin into sodium hydroxide solution for activation, stirring at room temperature for 0.5 to 1.5 hours, filtering, washing and drying to obtain activated resin;
[0030] b) adding the activated resin to ethanol, stirring evenly, then sequentially adding the phosphonic acid monomer and the amine-containing monomer, stirring continuously, reacting at 40-50° C. for 3-5 hours, and after the reaction is completed, filtering, washing and drying to obtain a modified resin;
[0031] c) mixing aluminum oxide, silicon dioxide, calcium phosphate and copper oxide to obtain a mixture;
[0032] d) mixing N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-(2-aminoethylamino)propyltrimethoxysilane to obtain a mixed solution;
[0033] e) Add the mixed solution into ethanol and stir evenly, then add the mixed material, continue stirring for 5 to 8 hours, then add the modified resin, heat and stir to react, after the reaction is completed, filter, wash and dry to obtain the ion exchange resin.
[0034] Preferably, the mass concentration of the sodium hydroxide solution in step a) is 5-10%, and the mass volume ratio of MB-20 resin to the sodium hydroxide solution is 100g:400-500mL.
[0035] Preferably, in step b), the mass volume ratio of the activated resin to ethanol is 100 g: 200-400 mL.
[0036] Preferably, in step e), the volume ratio of the mixed solution to ethanol is 1:(10-20), the heating temperature is 55-65° C., and the heating time is 2-4 hours.
[0037] A third aspect of the present invention provides an application of an ion exchange resin for rapidly purifying seawater in the purification of tritium-containing seawater samples.
[0038] The ion exchange resin prepared by the present invention is used to purify seawater samples, and the obtained solution is then used to measure the activity concentration of tritium in the sample using liquid scintillation counting (LSC). It is found that the test result is not much different from the result of purifying the marine sample by distillation.
[0039] Therefore, the present invention adopts the above-mentioned ion exchange resin for rapid purification of seawater and its preparation method and application, which has the following beneficial effects:
[0040] 1. The ion exchange resin prepared by the present invention can efficiently remove metal ions. Phosphonic acid monomers (such as aminotrimethylenephosphonic acid, etc.) and amine-containing monomers (such as diethylamine, etc.) can provide a large number of active sites to effectively adsorb and remove common metal ions in seawater, such as sodium ions, potassium ions, aluminum ions and magnesium ions.
[0041] 2. The present invention can significantly improve the wear resistance of the resin by adding a specific proportion of aluminum oxide, silicon dioxide, calcium phosphate and copper oxide as inorganic fillers in the ion exchange resin. These fillers not only enhance the mechanical strength and stability of the resin, but also improve its wear resistance and service life, which is very important for ensuring the effectiveness and economy of the resin in the seawater treatment process.
[0042] 3. The present invention reduces interference in the tritium LSC determination process by efficiently removing common metal ions in seawater, thereby improving the accuracy of the determination of tritium activity concentration in seawater samples. The high selectivity and hydrophilicity of the ion exchange resin of the present invention help to improve the recovery rate of tritium, ensure that the concentration of tritium in the final sample is closer to the original concentration, and reduce analytical errors.
[0043] 4. The present invention can significantly improve the salt resistance and acid and alkali resistance of the resin by adding diethylamine, triethylenediamine and acrylamide as amine-containing monomers in the ion exchange resin. These monomers not only enhance the stability and performance of the resin in a high-salinity environment, but also improve the tolerance of the resin under acid-base change conditions. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 The influence of different types and dosage values on the conductivity of seawater;
[0045] Figure 2 Figure 1 is the SEM image and EDS image of MB-20 resin before and after seawater treatment, in which a is the SEM image of MB-20 resin before seawater treatment, b and c are the EDS spectra of MB-20 resin before seawater treatment; d is the SEM image of MB-20 resin after seawater treatment, e and f are the EDS spectra of MB-20 resin after seawater treatment;
[0046] Figure 3 Figure 1 is the SEM image and EDS image of MB-106UP resin before and after seawater treatment, in which a is the SEM image of MB-106UP resin before seawater treatment, b and c are the EDS spectra of MB-106UP resin before seawater treatment; d is the SEM image of MB-106UP resin after seawater treatment, e and f are the EDS spectra of MB-106UP resin after seawater treatment;
[0047] Figure 4 Figure 1 is the SEM image and EDS image of MB-450 resin before and after seawater treatment, in which a is the SEM image of MB-450 resin before seawater treatment, b and c are the EDS spectra of MB-450 resin before seawater treatment; d is the SEM image of MB-450 resin after seawater treatment, e and f are the EDS spectra of MB-450 resin after seawater treatment;
[0048] Figure 5 The effect of MB-20 resin addition on conductivity;
[0049] Figure 6 This is the relationship between the amount of MB-20 resin added, stirring time and conductivity. DETAILED DESCRIPTION
[0050] The present invention will be further described below. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and a specific operation process, but the present invention is not limited to this embodiment.
[0051] Example 1
[0052] This example provides a resin type screening process, which is as follows:
[0053] The selected ion exchange resin should have appropriate selectivity, fast exchange rate, high exchange capacity and resistance to physical rupture, be easy to regenerate and cheap and readily available. This example selected 5 commercially available resins to purify seawater. The change in conductivity before and after sample purification was used to evaluate the removal efficiency of impurities in seawater. 5, 10, 11, 12, 13, 14, 15 and 20 g of MB-20, MB-106UP, MB-450, T-42 or CH-99 resins were added to 20 mL of seawater. The brands of MB-106UP, T-42 and CH-99 are MB-20 and MB-450 are branded as AmberLite TM , after stirring in a beaker for 5 minutes, it was filtered using a 0.22 μm hydrophilic filter, its conductivity was measured, and the resin that could significantly reduce the conductivity of seawater was selected for subsequent experiments.
[0054] Figure 1 The effects of different types and dosages of resin on the conductivity of seawater are shown in Figure 2. MB-106UP, MB-20 and MB-450 resins reduce the conductivity of seawater when treating seawater. Strong acid cation and strong base anion mixed bed exchange resins have better effects on removing ions from seawater. Under the condition of constant seawater and conductivity, MB-20 resin has the least amount of resin, followed by MB-450.
[0055] In order to compare the changes in the types and contents of metal ions in seawater before and after purification, the metal ion contents in seawater diluted 100 times, MB-20, MB-106UP, MB-450 resins and seawater treated with atmospheric distillation were measured using inductively coupled plasma optical emission spectrometry (ICP-OES).
[0056] Table 1 Changes in metal ion content in treated seawater
[0057]
[0058]
[0059] The results are shown in Table 1. The main metal ions detected in seawater are sodium ions, potassium ions, magnesium ions and aluminum ions, and their contents are sodium>magnesium>potassium>aluminum. The three resins and atmospheric distillation can remove aluminum, magnesium, sodium and potassium ions from seawater, and the removal rate of resin is significantly higher than that of atmospheric distillation. In summary, MB-20, MB-106UP and MB-450 resins can effectively remove metal ions from seawater and show good effects in reducing the conductivity of seawater.
[0060] In order to further study the effect of ion exchange resin treatment on ions in seawater, the surface morphology of the resin before and after seawater treatment was characterized by scanning electron microscopy (SEM), and the changes in element content in the resin before and after seawater treatment were analyzed by energy dispersive spectrometer (EDS). Take 15g of MB-20, MB-106UP and MB-450 resins and 20mL of seawater in a beaker, place them on a magnetic stirrer and stir continuously for 10min, filter, and dry in an oven at 60℃ for 5h. Take 5g of unused MB-20, MB-106UP and MB-450 resins and the dried resins and grind them into powder. SEM and EDS analysis were performed on each group of samples.
[0061] The results are as follows Figures 2 to 4 As shown, in order to prevent errors, the results of two locations were observed during the EDS test. The SEM scanning results and EDS test results show that there is no obvious change in the surface of the three resins before and after seawater treatment, and the surface is smooth and uniform. This indicates that the resin can be reused after elution treatment. Figure 2 and Figure 3 It can be seen that the sulfur, chlorine and carbon ion contents in MB-20 and MB-106UP resins after seawater treatment remain relatively stable without significant changes. However, the atomic percentages of sodium, potassium and magnesium increased in both resins to a certain extent, increasing by 1.84%, 0.07% and 0.25% in MB-20 resin and by 0.08%, 0.02% and 0.13% in MB-106 resin, respectively. Figure 4 It can be seen that the ion contents of sulfur, chlorine and sodium in MB-450 resin after seawater treatment increased by 2.4%, 0.32% and 0.03% respectively, and there was no significant change in other ions.
[0062] In summary, when the sample volume is constant, the required amount of MB-20 resin is the least, and the conductivity can be reduced to below 5μS / cm; ICP-OES and EDS results show that the adsorption capacity of MB-20 resin for sodium ions, potassium ions and magnesium ions in seawater is significantly higher than that of the other two resins. Therefore, this experiment selected MB-20 resin for subsequent experiments.
[0063] Example 2
[0064] This example provides an optimal reaction condition for purifying a seawater sample using MB-20 resin.
[0065] (1) Resin dosage
[0066] 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, and 15 g of MB-20 resin and 20 mL of seawater were magnetically stirred for 5 min, and the conductivity was measured and recorded. The experiment was repeated 3 times.
[0067] Considering the loss of samples during resin purification and meeting the measurement requirements of LSC, the volume of seawater samples was set to 20 mL. The relationship between seawater conductivity and the amount of resin added when the sample volume was 20 mL was discussed, and the optimal amount of resin was determined. Figure 5 As shown in the figure, under the conditions of 20 mL of seawater sample and 5 min of reaction time, when the amount of resin is in the range of 5 to 10 g, it can be observed that the conductivity of seawater gradually decreases with the increase of the amount of resin added. When the amount of resin is 11 g, the conductivity of seawater drops below 1.5 μS / cm. With the further increase of the amount of resin, the conductivity of seawater does not change significantly.
[0068] (2) Mixing time
[0069] 9, 10, and 11 g of resin were mixed with 20 mL of seawater and magnetically stirred, and the conductivity was measured at 1, 2, 3, 4, 5, 10, 15, 20, and 30 min, respectively.
[0070] In order to study the effect of different magnetic stirring times on the conductivity of seawater, mixed samples containing 9, 10, and 11 g of resin and 20 mL of seawater were prepared. Figure 6 As shown in the figure, when 9g of resin is added, the conductivity of seawater gradually decreases with the extension of stirring time, and stabilizes at 1.6μS / cm after 20min. When 10g of resin is added, the conductivity of seawater gradually decreases within 15min of stirring, and then remains unchanged at 0.9μS / cm. When the amount of resin is 11g, the conductivity of seawater decreases within 10min, and then stabilizes at around 0.9μS / cm. In summary, the best experimental effect can be achieved when 11g of MB-20 resin is selected and the stirring time is 10min.
[0071] Example 3
[0072] This example provides the effects of using MB-20 resin to treat seawater samples and using the currently used distillation method to treat seawater samples on the detection of tritium by the LSC method.
[0073] By adding different amounts (0.25, 2.5 and 5 mL) of tritium standard solution, tritium spiked samples of 5.1, 51 and 102 Bq / L were prepared respectively. 20 mL of spiked sample and 11 g of MB-20 resin were mixed and magnetically stirred for 10 min. After filtering with a 0.22 μm filter, the tritium activity concentration in the sample was determined by LSC method. To ensure the reliability of the results, each group of spiked samples was repeated 4 times. In addition, this experiment also subjected 3 groups of spiked samples to atmospheric distillation. The specific operation is as follows: 30 mL of spiked sample, an appropriate amount of zeolite and 0.05 g of potassium permanganate were added to the distillation flask for distillation, and the intermediate distillate was collected. To ensure the reliability of the results, each group of spiked samples was repeated 4 times.
[0074] Table 2 Comparison of tritium recovery results by ion exchange resin and atmospheric distillation
[0075]
[0076] The recovery rate is calculated based on the ratio of the tritium activity concentration of the treated seawater to the activity concentration of the standard solution prepared before treatment. As shown in Table 2, the tritium recovery rate after treatment with MB-20 resin is above 85%, ranging from 85.12% to 98.45%. This indicates that the use of MB-20 resin in the present invention to treat metal ions in seawater samples does not have an adverse effect on the subsequent detection of tritium activity concentration, and MB-20 resin can replace the existing distillation method to quickly purify seawater samples.
[0077] Example 4
[0078] This example provides the process and results of using MB-20 resin to treat seawater samples.
[0079] To verify the applicability of this method, 10 seawater samples were collected near Hangzhou Bay, Zhejiang Province on August 27, 2023. In order to compare the performance, the 10 seawater samples were purified by ion exchange resin and distillation (the sample volume required for the ion exchange resin method was 600 mL, and the sample volume required for the distillation method was 750 mL) and then electrolytically concentrated.
[0080] Table 3 Tritium activity concentration in seawater
[0081]
[0082] As shown in Table 3, the activity concentrations of tritium in seawater treated with ion exchange resin and atmospheric distillation were 1.30 ± 0.35 Bq / L and 1.58 ± 0.32 Bq / L, respectively. Considering the uncertainty, the results of tritium determination by ion exchange resin method and atmospheric distillation method were in good agreement. For the purification of each seawater sample, the ion exchange resin method took 10 min, and the atmospheric distillation method took > 24 h (distillation treatment for more than two times). The MB-20 resin in the present invention can be applied to the actual seawater purification process for purifying seawater samples.
[0083] Example 5
[0084] This embodiment provides an ion exchange resin for rapidly purifying seawater. The ion exchange resin comprises the following raw materials in parts by weight:
[0085]
[0086] The phosphonic acid monomers include aminotrimethylenephosphonic acid, hydroxyethylidene diphosphonic acid and iminobis(methylenephosphonic acid) in a mass ratio of 9:5:1; aminotrimethylenephosphonic acid CAS: 6419-19-8, hydroxyethylidene diphosphonic acid CAS: 2809-21-4, iminobis(methylenephosphonic acid) CAS: 17261-34-6.
[0087] The amine-containing monomers include diethylamine, triethylenediamine and acrylamide in a mass ratio of 1:6:2; the acrylamide is N-methylacrylamide.
[0088] The inorganic filler includes aluminum oxide, silicon dioxide, calcium phosphate and copper oxide in a mass ratio of 14:5:2:10.
[0089] Alumina is aluminum oxide nanowires with a diameter of 4 nm and a length of 1 μm, purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., model number XFJ37.
[0090] The diameter of silicon dioxide is 65-85 nm and it was purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd. with the model number of XFF48.
[0091] Calcium phosphate was purchased from Lianyungang Zhonghong Chemical Co., Ltd., CAS: 7758-87-4.
[0092] The copper oxide is a copper oxide nanochain with a diameter of 35-42 nm and a length of 1.0-1.6 μm, purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., model number XFI16.
[0093] The silane coupling agent includes N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and 3-(2-aminoethylamino)propyltrimethoxysilane in a mass ratio of 2:1:3, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane CAS: 1760-24-3, 3-aminopropyltriethoxysilane CAS: 919-30-2, 3-(2-aminoethylamino)propyltrimethoxysilane CAS: 1760-24-3.
[0094] This embodiment also provides a method for preparing an ion exchange resin for rapidly purifying seawater, comprising the following steps:
[0095] a) adding MB-20 resin to a sodium hydroxide solution for activation, wherein the mass concentration of the sodium hydroxide solution is 6%, the mass volume ratio of MB-20 resin to the sodium hydroxide solution is 100 g:450 mL, stirring at room temperature for 1 h, filtering, washing and drying to obtain an activated resin;
[0096] b) adding the activated resin to ethanol in a mass volume ratio of the activated resin to ethanol of 100 g:300 mL, stirring evenly, then sequentially adding the phosphonic acid monomer and the amine-containing monomer, stirring continuously, reacting at 40° C. for 3 h, and after the reaction is completed, filtering, washing and drying to obtain a modified resin;
[0097] c) mixing aluminum oxide, silicon dioxide, calcium phosphate and copper oxide to obtain a mixture;
[0098] d) mixing N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-(2-aminoethylamino)propyltrimethoxysilane to obtain a mixed solution;
[0099] e) Add the mixed solution into ethanol and stir evenly. The volume ratio of the mixed solution to ethanol is 1:10. Then add the mixed material and continue stirring for 5 hours. Then add the modified resin and heat and stir at 60°C for 2 hours. After the reaction is completed, filter, wash and dry to obtain the ion exchange resin.
[0100] Example 6
[0101] The difference between this embodiment and embodiment 5 is that the formula of the ion exchange resin is different.
[0102] The ion exchange resin in this embodiment includes the following raw materials in parts by weight:
[0103] MB-20 resin 100 parts;
[0104] 5 parts of phosphonic acid monomer;
[0105] 3 parts of amine-containing monomer;
[0106] 38 parts of inorganic filler;
[0107] Silane coupling agent 16 parts.
[0108] The phosphonic acid monomers include aminotrimethylenephosphonic acid, hydroxyethylidene diphosphonic acid and iminobis(methylenephosphonic acid) in a mass ratio of 10:6:1.
[0109] The amine-containing monomers include diethylamine, triethylenediamine and acrylamide in a mass ratio of 1:5:1; the acrylamide is N-methylacrylamide.
[0110] The inorganic filler includes aluminum oxide, silicon dioxide, calcium phosphate and copper oxide in a mass ratio of 12:3:3:12.
[0111] Comparative Example 1
[0112] The difference between this comparative example and Example 5 is that the alumina nanowires are replaced with alumina powder, which is purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., with a model of XFI08 and a particle size of 10 to 15 nm.
[0113] Comparative Example 2
[0114] The difference between this comparative example and Example 5 is that the particle size of silicon dioxide is replaced with 100-140 nm, and silicon dioxide is purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., model number XFF48.
[0115] Comparative Example 3
[0116] The difference between this comparative example and Example 5 is that the copper oxide nanochains are replaced by copper oxide particles, and the copper oxide particles are purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., model XFI30, with a diameter of 10 to 50 nm.
[0117] Comparative Example 4
[0118] The difference between this comparative example and Example 5 is that calcium phosphate is replaced with an equal mass of aluminum oxide nanowires.
[0119] Comparative Example 5
[0120] The difference between this comparative example and Example 5 is that the inorganic filler includes aluminum oxide, silicon dioxide, calcium phosphate and copper oxide in a mass ratio of 14:10:2:10.
[0121] Comparative Example 6
[0122] The difference between this comparative example and Example 5 is that the phosphonic acid monomers include aminotrimethylenephosphonic acid, hydroxyethylidene diphosphonic acid and iminobis(methylenephosphonic acid) in a mass ratio of 9:5:5.
[0123] Comparative Example 7
[0124] The difference between this comparative example and Example 5 is that the phosphonic acid monomer does not contain iminobis(methylenephosphonic acid), and an equal mass of aminotrimethylenephosphonic acid is used to replace iminobis(methylenephosphonic acid).
[0125] Comparative Example 8
[0126] The difference between this comparative example and Example 5 is that no amine-containing monomer is added, and an equal mass of phosphonic acid monomer is used to replace the amine-containing monomer.
[0127] Comparative Example 9
[0128] The difference between this comparative example and Example 5 is that the amine-containing monomer includes diethylamine, triethylenediamine and acrylamide in a mass ratio of 8:6:2.
[0129] Performance Testing
[0130] (1) The mechanical strength test was performed on the resins prepared in Example 1, Examples 5-6 and Comparative Examples 1-9.
[0131] The crushing strength was tested according to DL / T 771-2014 “Guidelines for the Selection of Ion Exchange Resins for Water Treatment in Power Plants”.
[0132] Table 4 Mechanical properties test results
[0133] Example / Comparative Example Crushing strength MPa Example 1 18.3 Example 5 32.5 Example 6 31.8 Comparative Example 1 25.4 Comparative Example 2 24.6 Comparative Example 3 25.1 Comparative Example 4 23.5 Comparative Example 5 22.9 Comparative Example 6 24.3 Comparative Example 7 22.6 Comparative Example 8 23.8 Comparative Example 9 20.5
[0134] (2) 11 g of the resin prepared in Example 1, Examples 5-6 and Comparative Examples 1-9 was added to 20 mL of seawater sample and magnetically stirred for 10 min. The metal ion content in the seawater diluted 100 times, MB-20 of Example 1, and the seawater treated with the resin prepared in Examples 5-6 and Comparative Examples 1-9 was measured using an inductively coupled plasma optical emission spectrometer (ICP-OES).
[0135] Table 5 Changes in metal ion content in seawater after treatment with resins prepared in Examples and Comparative Examples
[0136]
[0137]
[0138] (3) Method validation
[0139] A 51 Bq / L tritium spiked sample was prepared by adding 2.5 mL of tritium standard solution. 11 g of MB-20 resin of Example 1, resins prepared in Examples 5-6, and resins prepared in Comparative Examples 1-9 were added to 20 mL of the spiked sample, mixed and magnetically stirred for 10 min, filtered with a 0.22 μm filter, and the tritium activity concentration in the sample was determined by LSC method. To ensure the reliability of the results, the experiment was repeated 4 times for each group of spiked samples.
[0140] Table 6 Comparison of tritium recovery rates of resins prepared in Examples and Comparative Examples and treated by atmospheric distillation
[0141] method Recovery rate range % Atmospheric distillation 102.57~106.51 Example 1 90.87~98.45 Example 5 99.23~102.68 Example 6 98.37~103.51 Comparative Example 1 90.23~95.46 Comparative Example 2 88.19~93.22 Comparative Example 3 89.65~94.69 Comparative Example 4 85.37~88.68 Comparative Example 5 82.47~86.25 Comparative Example 6 88.52~95.36 Comparative Example 7 83.16~86.92 Comparative Example 8 80.81~92.45 Comparative Example 9 84.56~93.18
[0142] (4) The MB-20 resin of Example 1 and the resins prepared in Examples 5-6 and Comparative Examples 1-9 were placed in a mixed solution of 3 mol / L sodium hydroxide and 30% sodium chloride, respectively, and soaked at 80° C. for 15 days. The resins were then taken out, washed and dried. The obtained resins were used to purify seawater samples and the tritium activity concentration in the samples was determined by the LSC method. The test was repeated four times and the average value was taken.
[0143] The MB-20 resin of Example 1 and the resins prepared in Examples 5-6 and Comparative Examples 1-9 were placed in a mixed solution of 3 mol / L hydrochloric acid and 30% sodium chloride by mass, respectively, and soaked at 80° C. for 15 days. The resins were taken out, washed and dried. The obtained resins were used to purify seawater samples and the tritium activity concentration in the samples was determined by the LSC method. The test was repeated four times and the average value was taken.
[0144] Table 7 Environmental resistance of resins prepared in Examples and Comparative Examples
[0145] Example / Comparative Example Recovery range after alkali treatment% Recovery range after acid treatment % Example 1 73.23 72.54 Example 5 95.68 103.27 Example 6 93.21 94.85 Comparative Example 1 85.32 86.85 Comparative Example 2 83.48 82.96 Comparative Example 3 84.57 83.24 Comparative Example 4 80.21 81.73 Comparative Example 5 78.58 77.19 Comparative Example 6 82.49 83.65 Comparative Example 7 79.17 78.49 Comparative Example 8 76.35 77.11 Comparative Example 9 79.28 80.06
[0146] It can be seen from the above performance test results that the ion exchange resins of Examples 5-6 have a good seawater purification effect, which is convenient for determining tritium in seawater by the LSC method. The ion exchange resins also have good environmental resistance and excellent mechanical strength, which prolongs the service life of the ion exchange resins. In particular, the comprehensive performance of the resin prepared in Example 1 is the most outstanding. This is mainly because the present invention, on the basis of the MB-20 resin matrix, also carries out modifications of inorganic fillers, phosphonic acid monomers and amine-containing monomers, thereby improving the removal of high-valent metal ions in seawater and reducing the adverse effects of metal elements on the determination of tritium by the LSC method.
[0147] The comparative examples, however, were not equipped with the necessary technical solutions, which resulted in the corresponding performance tests being significantly worse than those of the embodiments. In comparative examples 1-3, the type of aluminum oxide, the particle size of silicon dioxide, and the type of copper oxide were changed respectively. From the results, it can be seen that the mechanical strength of the ion exchange resin decreased, and the treatment effect on the seawater sample also deteriorated, resulting in a large difference between the detection result of the tritium activity concentration and the distillation method, proving that the type and parameters of the inorganic filler have an important influence on the treatment effect of the seawater sample and the detection of the tritium activity concentration. In comparative example 4, no calcium phosphate was added to the inorganic filler. From the results, it can be seen that the mechanical strength and the accuracy of the detection result of the tritium activity concentration further decreased, indicating that the simultaneous addition of the four inorganic fillers has an important influence on improving the seawater treatment effect and improving the accuracy of the detection of the tritium activity concentration. Comparative example 5 changed the ratio of the four inorganic fillers. From the results, it can be seen that the treatment effect of the seawater sample of the ion exchange resin deteriorated, and the detection result of the tritium activity concentration was different from the commonly used distillation method. The test results were not accurate enough, indicating that the ratio of the four inorganic fillers played an important role in the detection of the tritium activity concentration in seawater. Comparative Example 6 changes the ratio of the three phosphonic acid monomers. From the results, it can be seen that the treatment effect of the seawater sample of the ion exchange resin is deteriorated. At the same time, the detection result of the tritium activity concentration is different from the commonly used distillation method, and the test result is not accurate enough, indicating that the ratio of the three phosphonic acid monomers has an important influence on the detection of tritium activity concentration in seawater. In Comparative Example 7, two phosphonic acid monomers are used to prepare the ion exchange resin. From the results, it can be seen that the metal ion removal effect of the seawater sample of the prepared ion exchange resin is deteriorated, and the detection result of the tritium activity concentration of seawater is also biased, indicating that the type of phosphonic acid monomer also has an impact on the use of the ion exchange resin. Comparative Example 8 does not use amine-containing monomers, and only uses phosphonic acid monomers to modify MB-20 resin. From the results, it can be seen that the metal ion removal effect of the seawater sample of the prepared ion exchange resin is further deteriorated, and the detection result of the tritium activity concentration of seawater is also more biased, indicating that the simultaneous modification of the two monomers has a very important influence on the use effect of the ion exchange resin. In Comparative Example 9, the ratio of the three amine-containing monomers was changed. From the results, it can be seen that the mechanical strength, metal ion removal effect and tritium activity concentration detection accuracy of the prepared ion exchange resin all decreased to varying degrees, indicating that the ratio of the three amine-containing monomers has an impact on the use effect of the ion exchange resin. The above experimental results further prove the importance of the technical solution defined in the present invention to its technical effect.
[0148] Therefore, the present invention adopts an ion exchange resin with the above structure for rapid purification of seawater, and its preparation method and application. The prepared ion exchange resin not only has a good purification effect on seawater samples, but also has excellent mechanical strength, wear resistance and environmental resistance, and has a long service life.
[0149] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. An ion exchange resin for rapid purification of seawater, characterized in that: The ion exchange resin comprises the following raw materials in parts by weight: MB-20 resin 100-150 parts; 5-10 parts of phosphonic acid monomer; 3-5 parts of amine-containing monomer; 30-40 parts of inorganic filler; 15-20 parts of silane coupling agent; The phosphonic acid monomers include aminotrimethylenephosphonic acid, hydroxyethylidene diphosphonic acid and iminobis(methylenephosphonic acid) in a mass ratio of (8-10):(4-6):1; The amine-containing monomer includes diethylamine, triethylenediamine and acrylamide in a mass ratio of 1:(5-8):(1-3); The inorganic filler includes aluminum oxide, silicon dioxide, calcium phosphate and copper oxide in a mass ratio of (12-15):(3-6):(1-3):(8-12); The silane coupling agent includes N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane and 3-(2-aminoethylamino)propyltrimethoxysilane in a mass ratio of (1-3):(1-3):(1-3).
2. The ion exchange resin for rapid purification of seawater according to claim 1, characterized in that: Alumina is aluminum oxide nanowires with a diameter of 4 nm and a length of 1 μm.
3. The ion exchange resin for rapid purification of seawater according to claim 1, characterized in that: The diameter of silicon dioxide is 65 to 85 nm.
4. The ion exchange resin for rapid purification of seawater according to claim 1, characterized in that: The copper oxide is a copper oxide nanochain with a diameter of 35 to 42 nm and a length of 1.0 to 1.6 μm.
5. The ion exchange resin for rapid purification of seawater according to claim 1, characterized in that: Acrylamide is one of N-methylacrylamide and N-hydroxymethylacrylamide.
6. A method for preparing an ion exchange resin for rapid purification of seawater according to any one of claims 1 to 5, characterized in that: The following steps are involved: a) adding MB-20 resin into sodium hydroxide solution for activation, stirring at room temperature for 0.5 to 1.5 hours, filtering, washing and drying to obtain activated resin; b) adding the activated resin to ethanol, stirring evenly, then sequentially adding the phosphonic acid monomer and the amine-containing monomer, stirring continuously, reacting at 40-50° C. for 3-5 hours, and after the reaction is completed, filtering, washing and drying to obtain a modified resin; c) mixing aluminum oxide, silicon dioxide, calcium phosphate and copper oxide to obtain a mixture; d) mixing N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and 3-(2-aminoethylamino)propyltrimethoxysilane to obtain a mixed solution; e) Add the mixed solution into ethanol and stir evenly, then add the mixed material, continue stirring for 5 to 8 hours, then add the modified resin, heat and stir to react, after the reaction is completed, filter, wash and dry to obtain the ion exchange resin.
7. The method for preparing the ion exchange resin for rapid purification of seawater according to claim 6, characterized in that: In step a), the mass concentration of the sodium hydroxide solution is 5-10%, and the mass volume ratio of the MB-20 resin to the sodium hydroxide solution is 100 g: 400-500 mL.
8. The method for preparing the ion exchange resin for rapid purification of seawater according to claim 6, characterized in that: In step b), the mass volume ratio of the activated resin to ethanol is 100 g: 200-400 mL.
9. The method for preparing the ion exchange resin for rapid purification of seawater according to claim 6, characterized in that: In step e), the volume ratio of the mixed solution to ethanol is 1:(10-20), the heating temperature is 55-65° C., and the heating time is 2-4 hours.
10. Use of the ion exchange resin for rapid purification of seawater according to any one of claims 1 to 5 in the purification of tritium-containing seawater samples.
Citation Information