Equipment and technological process for rapidly removing aluminum in die cavity in extrusion die

Through the combination of low-melting point metal replacement rod and induction heating furnace, the aluminum alloy in the extrusion mold is quickly removed, solving the problems of alkaline washing and high-temperature annealing, and achieving an efficient and lossless mold maintenance process.

CN119035296AActive Publication Date: 2024-11-29CITIC BOHAI ALUMINUM IND HLDG COMPANY +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411418363.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-29
Estimated Expiration
2044-10-11

AI Technical Summary

Technical Problem

When removing the residue of aluminum alloy inside the extrusion mold, the alkali washing method takes a long time and is difficult to handle waste liquid. High carbon steel is easily annealed and softened at high temperatures, which affects the life of the mold.

Method used

The low-melting point metal replacement rod is used to melt the replacement rod through an extrusion system and an induction heating furnace. The melted metal is used to remove the aluminum alloy in the mold, and the replacement rod is recovered through the crystallization container mechanism to achieve fast and lossless mold maintenance.

Benefits of technology

The time for removing aluminum alloy is greatly shortened, only about half an hour, and it is not damaged to the mold, the process is clean and pollution-free, and the replacement rod can be reused, avoiding the annealing and softening problem of steel molds by high temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035296A_ABST
    Figure CN119035296A_ABST
Patent Text Reader

Abstract

The invention discloses equipment and a technological process for rapidly removing aluminum in a die cavity in an extrusion die, the equipment comprises a replacement rod, an extrusion system, an induction heating furnace and a crystallization container mechanism, and the extrusion system comprises a die seat used for fixing the extrusion die through a die sleeve, a residual pressure shear, an extrusion cylinder and an extrusion rod. The process flow comprises the following steps: feeding the replacement rod into the extrusion cylinder, wherein the extrusion cylinder drives the replacement rod to abut against the die seat; the extrusion rod drives the extrusion pad mounted at the front end to extrude the replacement rod to enter the extrusion die from the extrusion cylinder and partially extrude the replacement rod from the extrusion die, so that aluminum in the extrusion die is replaced by the replacement rod; cutting off the residual replacement rod with the preset length as a pressure residue; the extrusion die filled with the replaced rod material extruded from the middle of the extrusion die is placed on a collecting funnel of an induction heating furnace, and the molten replaced rod material flows into a crystallizer of a crystallization container mechanism below from the collecting funnel through electric heating. Therefore, the die is not damaged, the replacement rod can be repeatedly used, and the process is clean and pollution-free.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of extrusion, and in particular to equipment and a process flow for quickly removing aluminum from a die cavity inside an extrusion die. Background Art

[0002] At present, almost all the extrusion dies used for aluminum alloy extrusion use Naoh alkaline washing to remove the aluminum alloy in the steel mold. The advantage is that Naoh does not react chemically with steel and can remove the residue in the mold without damage. However, there are also problems such as long alkaline washing time and difficult treatment of waste liquid. It should also be emphasized that the melting point of high carbon steel is generally between 1400℃ and 1450℃, and the melting point of aluminum alloy is between 607~650℃. If it is directly heated to about 700℃, the aluminum water will melt, and the high carbon steel will not melt. The aluminum alloy can also be separated from the mold. However, at this high temperature of about 700℃, high carbon steel is easily annealed and softened, and it cannot continue to be used or seriously affects its life, so it is not used in industry. Summary of the invention

[0003] In order to solve the above problems, the purpose of the present invention is to provide a device and process flow for quickly removing aluminum from the mold cavity of an extrusion die.

[0004] According to one aspect of the present invention, there is provided an apparatus for rapidly removing aluminum from the internal cavity of an extrusion die, comprising: a displacement rod having a material melting point lower than that of the extrusion die, an extrusion system, an induction heating furnace and a crystallization container mechanism, wherein the extrusion system comprises: a die seat for fixing the extrusion die via a die sleeve, a residual shear for cutting residual pressure, an extrusion barrel, and an extrusion rod, the extrusion barrel comprising a cavity for the displacement rod to pass therethrough when being extruded, an extrusion pad having a diameter smaller than that of the inner wall of the extrusion barrel being installed at the front end of the extrusion rod, the extrusion pad being used to extrude the displacement rod so as to enter the cavity of the extrusion die to displace the aluminum in the extrusion die; the induction heating furnace comprises: a collecting funnel for collecting the molten liquid of the displacement rod material; the crystallization container mechanism comprises: a crystallizer for accommodating the molten liquid from the collecting funnel.

[0005] Preferably, the equipment for quickly removing aluminum from the internal mold cavity of the extrusion mold also includes multiple mold sleeves, each mold sleeve has an inner circle consistent with the outer circle diameter of different extrusion molds, and has an outer circle diameter consistent with each other, so as to match extrusion molds of various diameter specifications.

[0006] Preferably, the extrusion system also includes: a moving beam connected to the extrusion rod, a main thrust rod and a main cylinder for pushing the moving beam, a front beam for setting a mold seat, a rear beam for setting a main cylinder, and a pull rod connected between the front beam and the rear beam.

[0007] Preferably, the mold base is in a U-shaped structure with an upper opening, and the mold base is provided with a protrusion for restricting the movement of the mold sleeve.

[0008] Preferably, the induction heating furnace further comprises: a ceramic lining, an induction coil, a heat-insulating outer shell and a heat-insulating cover.

[0009] Preferably, the crystallization container mechanism comprises a multi-stage crystallizer, and adjacent stages of the crystallizer are arranged as a whole in a stepped shape with a high middle and gradually lower levels for step-by-step overflow filling, and the interior of each stage of the crystallizer is a crystallizer inner cavity for accommodating the melt melted from the induction heating furnace.

[0010] Preferably, an outermost liquid baffle plate is provided at the outermost crystallizer to prevent the melt from overflowing, and / or a plurality of groups of multi-stage crystallization containers are arranged in a cross-shaped overall shape.

[0011] Preferably, the displacer rod material is lead and / or tin.

[0012] According to another aspect of the present invention, a process flow for quickly removing aluminum from the mold cavity inside an extrusion die is provided. Based on the above-mentioned equipment, the process flow includes the following steps: installing the extrusion die into the corresponding mold sleeve, and the mold sleeve is installed into the mold seat; sending a displacement rod into the extrusion barrel, and the extrusion barrel with the displacement rod is abutted against the mold seat; the extrusion rod moves toward the mold seat with the extrusion pad, and the extrusion displacement rod continues to move from the extrusion barrel into the extrusion die and is partially extruded from the extrusion die, thereby replacing the aluminum in the extrusion die with the displacement rod; when the displacement rod that has not entered the extrusion die has a remaining predetermined length, the extrusion rod stops moving and retreats with the extrusion pad, and the extrusion barrel is retreated, and the displacement rod of the remaining predetermined length is used as a residual and is sheared off; the aluminum profile extruded from the middle of the extrusion die and the displacement rod combination profile, the residual and at least the extrusion die of the extrusion die filled with the displacement rod material are placed on a collecting funnel, and the induction heating furnace is powered on and heated to a certain temperature and kept warm, so that the melted displacement rod material melt flows from the collecting funnel into the crystallizer below.

[0013] Preferably, after the replacement rod material solidifies in the crystallizer, the bottom baffle below the crystallizer is opened and knocked from above to demould the replacement rod.

[0014] The beneficial effects of the present invention are as follows: by extruding replacement rods, the residual aluminum in the extrusion die is replaced with low-melting-point metals. When the molds, profiles, and replacement rod combination profiles filled with replacement rods and the residual pressure of pure replacement rod components are heated to a certain degree, the replacement rods will melt, while the steel mold and aluminum alloy profiles are still solid. The melted metal enters the crystallizer mechanism and turns into replacement rods again. The mold is maintained, and the aluminum alloy profiles are returned to the furnace for recasting. Compared with the alkali washing method that takes several hours for small molds and even dozens of hours for large molds, this method greatly shortens the time and only takes about half an hour. There is no damage to the mold, and the replacement rods can be reused repeatedly, and the process is clean and pollution-free.

[0015] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 A schematic diagram of a displacement rod used in a device according to an embodiment of the present invention, wherein (A) shows a top view and (B) shows a front view;

[0017] Figure 2 A schematic diagram of the extrusion system used in the device;

[0018] Figure 3 It is a schematic diagram of the matching between extrusion dies and die sets of different specifications;

[0019] Figure 4 It is a front cross-sectional schematic diagram of the induction heating furnace and crystallization container mechanism used in the equipment;

[0020] Figure 5 A top view of the crystallization container mechanism used in the device. DETAILED DESCRIPTION

[0021] The exemplary embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. The exemplary embodiments described below and shown in the accompanying drawings are intended to teach the principles of the present invention so that those skilled in the art can implement and use the present invention in several different environments and for several different applications. Therefore, the scope of protection of the present invention is defined by the appended claims, and the exemplary embodiments are not intended to be, and should not be considered to be, a limiting description of the scope of protection of the present invention. Moreover, for the convenience of description, the sizes of the various parts shown in the accompanying drawings are not necessarily drawn according to the actual proportional relationship, and the orientation description, such as the longitudinal direction corresponding to the longitudinal length of the main body, and the orientation or position relationship indicated by the upper, lower, left, right, top, bottom, etc., are all based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention. Unless otherwise specifically stated, the order of the components and assembly steps described in the embodiments and the numerical values ​​do not limit the scope of the present invention. Moreover, any numerical range stated herein is intended to include all sub-ranges contained therein, and the numerical range represented by "value A to value B" refers to a range including the endpoint values ​​A and B. Those skilled in the art will understand that the terms "first", "second", "step" and the like in the present invention are only used to distinguish different steps, devices or modules, etc., and do not represent any specific technical meanings, nor do they represent the necessary logical order between them. For example, the second and third steps can be swapped or performed in parallel.

[0022] like Figures 1 to 5As shown, a device for quickly removing aluminum from a mold cavity inside an extrusion die according to an embodiment of the present invention includes a replacement rod 100, an extrusion system 200, an induction heating furnace 300, and a crystallization container mechanism 400.

[0023] The replacement rod 100 includes: a cylindrical rod made of, for example, pure lead.

[0024] Among them, the extrusion system 200 includes: a mold sleeve 201, an extrusion mold 202, a mold base 203, a shear 204, a main thrust rod 205 and a main cylinder 206 for pushing a movable beam 213, a front beam 207 for setting the mold base 203, a pull rod 208 connected between the front beam 207 and the rear beam 214, an extrusion cylinder 220 including an extrusion cylinder inner wall 209 and an extrusion cylinder body 210, an extrusion pad 211, an extrusion rod 212, a movable beam 213, and a rear beam 214 for setting the main cylinder 206.

[0025] The induction heating furnace 300 includes: a ceramic lining 301 , an induction coil 302 , a heat-insulating outer shell 303 , a heat-insulating cover 304 , and a collecting funnel 307 .

[0026] The crystallization container mechanism 400 includes: a primary crystallizer 401 , a secondary crystallizer 402 , a tertiary crystallizer 403 , a quaternary crystallizer 404 , a fifth crystallizer 405 , a crystallizer inner cavity 406 , a liquid baffle 407 , a crystallizer wall 408 , and a bottom baffle 409 .

[0027] <Replacement Rod 100>

[0028] The displacement rod 100 is cylindrical in shape and is made of a low melting point metal, such as lead or tin. Here, pure lead, which has a more stable chemical property and is relatively cheap, is used as an example.

[0029] <Extrusion system 200>

[0030] The corresponding extrusion die 202 just off the machine is installed in the appropriate die sleeve 201 and hoisted into the die seat 203. Here, the die seat 203 is a U-shaped structure with an upper opening, and the die sleeve 201 (containing the extrusion die 202) is hoisted and fixed into the die seat 203 from top to bottom. The die seat 203 is provided with protrusions (not shown) at the front and rear to restrict the movement of the die sleeve 201.

[0031] The displacement rod 100 is fed into the extrusion cylinder 220, and the extrusion cylinder 220 is brought into contact with the die seat 203 with the displacement rod 100. The driving mechanism of the extrusion cylinder 220 is not shown here, and can be appropriately arranged as required.

[0032] It should be noted that, since extruders of different tonnages correspond to an extrusion die 202 of a certain specification, the present invention, for the sake of universality, can optionally correspond to extrusion dies 202 of different specifications and die sleeves 201 of different specifications, and the characteristic is that the outer diameter of the die sleeve 201 remains unchanged, and the inner diameter of the die sleeve 201 is consistent with the outer diameter of the extrusion die 202, such as Figure 3 As shown in the examples of matching under three different specifications of left, middle and right, such matching can be directly used with one extrusion system 200 to meet the needs.

[0033] The main thrust rod 205 carries the moving beam 213 and the connected extrusion rod 212 , and the front end of the extrusion rod 212 is equipped with an extrusion pad 211 with a diameter smaller than the inner wall 209 of the extrusion cylinder, and the whole moves toward the mold seat 203 .

[0034] Since the die sleeve 201 and the extrusion die 202, the extrusion cylinder 220, and the extrusion pad 211 in the die seat 203 form a closed space, the displacement rod 100 in the extrusion cylinder 220 is squeezed into the extrusion die 202 by the extrusion pad 211. It is preferred that the diameter of the displacement rod 100 is consistent with the cavity diameter of the extrusion die 202, but it is not limited to this. This is because the displacement rod 100 is made of a softer material, and the displacement rod 100 on the front end side can only be extruded through the extrusion die 202. At this time, the aluminum alloy remaining in the extrusion die 202 before leaving the machine will be squeezed out of the extrusion die 202 first, so the displacement rod 100 will replace the aluminum alloy in the extrusion die 202 and continue for a period of time, effectively taking away the residual aluminum alloy in the extrusion die 202 that may be firmly adsorbed on the inner wall of the die. The profile extruded from the extrusion die 202 in the early stage is the residual aluminum alloy before, and the middle is the aluminum profile and the displacement rod combination profile 305, and the profile extruded later is pure lead.

[0035] When only a small section of the replacement rod 100 that has not entered the extrusion die 202 is left, such as a predetermined length, the main thrust rod 205 stops moving and retreats, and then the extrusion cylinder 220 also retreats. When only a small section of the replacement rod 100 is left, it is called the residual pressure, and the residual pressure is cut off by the residual pressure shear 204.

[0036] At this time, only pure lead remains in the inner space of the extrusion die 202.

[0037] <Induction Heating Furnace 300>

[0038] As mentioned above, the extrusion die 202 extrudes an aluminum profile and a displacement rod combination profile 305, and the final cut-off residue is a pure lead residue 306. The extrusion die 202 filled with the displacement rod 100 contains pure lead. Preferably, the extrusion die 202 is made of high carbon steel, and the melting point of high carbon steel is greater than that of aluminum alloy and pure lead.

[0039] Then, if Figure 4As shown, the aluminum profile and replacement rod combination profile 305, the residual pressure 306 and the extrusion die 202 filled with the replacement rod 100 are placed on the collecting funnel 307, covered with the insulation cover 304, powered on and heated to a certain temperature and kept warm. The temperature is required to be greater than the melting point of pure lead by 30 to 50°C to ensure the fluidity of pure lead metal and save energy.

[0040] The inner lining of the induction heating furnace 300 is a ceramic lining 301, which is resistant to high temperature and friction. The outer layer is a heat-insulating shell 303, which is made of heat-insulating bricks to prevent heat loss. In the middle of the two is an induction coil 302, which can heat the intermediate metal.

[0041] The function of the collecting funnel 307 in the induction heating furnace 300 is to allow the molten metal after the pure lead is melted to flow into the collecting funnel 307 below.

[0042] The insulation cover 304 is used to reduce heat loss. The insulation cover 304 is opened before heating to allow the aluminum profile and replacement rod combination profile 305, the residual pressure 306, and the extrusion die 202 filled with the replacement rod 100 to be placed. The insulation cover 304 is opened after heating to allow the aluminum profile (corresponding to the structure obtained after the aluminum profile and replacement rod combination profile 305 is heated and the lead material of the replacement rod is lost) and the extrusion die 202 to be taken out.

[0043] <Crystallization Container Mechanism 400>

[0044] like Figure 4 , 5 As shown, from the cross-sectional view of the crystallization container mechanism 400, the crystallizers at each level are arranged in a stepped shape, which is high in the middle and gradually becomes lower. For the convenience of description, they are respectively called the first-level crystallizer 401, the second-level crystallizer 402, the third-level crystallizer 403, the fourth-level crystallizer 404, and the fifth-level crystallizer 405 (collectively referred to as "crystallizers"). Except for the position, the crystallizers at each level have the same structure. In this way, even in the scene where the induction heating furnace 300 is stationary, the crystallizers at each level can be filled by overflowing step by step.

[0045] The interior of the crystallizer is a crystallizer inner cavity 406 for containing the pure lead metal melt melted from the induction heating furnace 300 .

[0046] The outermost liquid baffle plate 407 is used to prevent the pure lead metal melt from overflowing the crystallizer mechanism 400. After the five-stage crystallizer 405 is also filled, the induction heating furnace 300 needs to be stopped immediately.

[0047] In order to facilitate the separation of pure lead from the crystallizer after solidification, a release agent such as a mixture of talcum powder and vegetable oil is evenly applied on the crystallizer wall 408 and the bottom baffle 409. After the pure lead solidifies, the bottom baffle 409 is opened, and the top is knocked with a wooden hammer to release the rod 100. At this time, a small amount of talcum powder remains on the surface, which can be rinsed with water and blown dry with a blower for use.

[0048] <Example>

[0049] Take the die for extruding 6005 alloy aluminum alloy photovoltaic frame, die specification (diameter * thickness): 250 (± 0.03) mm * 200 (± 0.03) mm, and the extrusion die 202 containing aluminum alloy after unloading as an example. The composition of 6005 alloy meets the requirements of GBT3190-2020.

[0050] The displacement rod 100 has an outer diameter of 178 (±0.5) mm and a height of 800 (±5) mm. Pure lead is used here with a melting point of 327.5°C.

[0051] The corresponding mold sleeve 201 just removed from the machine is installed in the appropriate mold sleeve 201 and hoisted into the mold seat 203. The displacement rod 100 is sent into the extrusion cylinder 220, and the extrusion cylinder 220 leans against the mold seat 203 with the displacement rod 100.

[0052] For example, after the extrusion die 202 is removed from the machine after production, it is first cooled to below 300°C, and then the extrusion die 202 is installed in the die sleeve 201 (inner circle 250 (-0, +0.03) mm, outer circle 400 mm), and then hung in the die seat 203. The displacement rod 100 is clamped into the extrusion barrel 220 by a hand-held clamp (not shown). The extrusion barrel 220 has a diameter of 185 (±1) mm and a length of 1100 (-0, +1) mm. The hydraulic system (not shown) brings the extrusion barrel 220 against the die seat 203, with a locking force of 280-300T.

[0053] The hydraulic system (not shown) drives the main thrust rod 205, drives the movable beam 213 and the connected extrusion rod 212 at a speed of 6 mm / s, and moves the extrusion pad 211 at the front end of the extrusion rod 212 toward the die seat 203. The expanded diameter of the extrusion pad 211 is 0.005-0.008 mm smaller than the diameter of the extrusion cylinder 220.

[0054] Since the mold sleeve 201 and the extrusion mold 202, the extrusion cylinder 220, and the extrusion pad 211 in the mold seat 203 form a closed space, the replacement rod 100 in the extrusion cylinder 220 can only be extruded through the extrusion mold 202 after being subjected to the extrusion force of the extrusion pad 211. At this time, the aluminum alloy before leaving the machine remains in the extrusion mold 202, and the aluminum alloy will be extruded out of the extrusion mold 202 first, and then the replacement rod 100 will replace the aluminum alloy in the extrusion mold 202, and continue to extrude for a period of time, effectively taking away the residual aluminum alloy in the extrusion mold 202 that may be firmly adsorbed on the inner wall of the mold.

[0055] When only a small section of the displacement rod 100 is left, about 30-35 mm thick, the main thrust rod 205 stops moving and retreats, and then the extrusion cylinder also retreats. The small section of the displacement rod 100 is called the pressure residue, which is cut off by the pressure residue shear 204. The retreat drive mechanism of the extrusion cylinder 220 is not shown here, and can be appropriately set according to needs.

[0056] The extrusion die 202 is hung down from the equipment, and at this time, only pure lead is left in the inner space of the extrusion die 202.

[0057] That is, what is extruded from the middle of the extrusion die 202 is the aluminum profile and the replacement rod combination profile 305, and the remaining pressure 306 cut off at last is pure lead. The extrusion die 202 filled with the replacement rod 100 is pure lead.

[0058] The extrusion die 202 is made of high carbon steel, and the melting point of high carbon steel (1400°C to 1450°C)>aluminum alloy (607~650°C)>pure lead (327.5°C).

[0059] Open the insulation cover 304, place the aluminum profile and replacement rod combination profile 305, the residual pressure 306 and the extrusion die 202 filled with the replacement rod 100 in the collecting funnel 307, cover the collecting funnel 307 with the insulation cover 304, turn on the power to heat to a certain temperature and keep it warm, the specific temperature is 357.5 ~ 377.5 ℃, to ensure the fluidity of pure lead metal and save energy.

[0060] The inner lining of the induction heating furnace 300 is a ceramic lining 301 made of boron carbide high temperature resistant ceramic. The outer layer is a heat-insulating shell 303 made of lightweight mullite brick. The induction coil 302 between the two has a power of 600kw and a heating rate of 60℃ / min.

[0061] The collecting funnel 307 is located at the bottom of the induction heating furnace 300 and is funnel-shaped and made of high-carbon steel. After the pure lead melts, it flows into the collecting funnel 307 below and further flows into the crystallizer below for step-by-step overflow filling.

[0062] The insulation cover 304 is also made of lightweight mullite brick.

[0063] like Figure 5 As shown, the overall shape of the multiple groups of multi-stage crystallization containers is arranged in a cross shape. The inner diameter of each crystallizer is 178 (±1) mm and the depth is 800 (±5) mm. The crystallizer wall 408 and the bottom baffle 409 are both made of boron carbide high temperature resistant ceramics.

[0064] When the first-level crystallizer 401 is full of pure lead melt, it will flow to the second-level crystallizer 402, and so on. In this way, when the pure lead melt is less, the replacement rod 100 finished product can be collected faster, which is convenient for subsequent work. The outermost liquid baffle 407 is 200 (-0, +5) mm higher than the fifth-level crystallizer 405 to prevent the pure lead metal melt from overflowing the crystallizer mechanism 400. After the fifth-level crystallizer 405 is also filled, the induction heating furnace 300 needs to be stopped immediately.

[0065] In order to facilitate the separation of pure lead from the crystallizer after solidification, a mixture of talcum powder and vegetable oil is evenly applied on the crystallizer wall 408 and the bottom baffle 409 in advance, with a thickness of about 0.02-0.05mm. After the pure lead solidifies, open the bottom baffle 409 below, knock the top with a wooden hammer, and the replacement rod 100 can be demoulded. At this time, a small amount of talcum powder remains on the surface, which can be rinsed with water and blown dry with a blower for standby use.

[0066] In this way, by extruding the replacement rod, the residual aluminum in the extrusion die is replaced with a low-melting-point metal. The extrusion die filled with the replacement rod, the aluminum profile and the replacement rod combination profile, and the pure replacement rod component are heated to a certain degree, and the replacement rod will melt, while the steel mold and the aluminum alloy profile are still solid. The melted metal enters the crystallizer mechanism and turns into a replacement rod again. The mold is maintained and the aluminum alloy profile is returned to the furnace for casting. Compared with the alkali washing method that takes several hours for small molds and even dozens of hours for large molds, this method greatly shortens the time and only takes about half an hour. There is no damage to the mold. And the replacement rod can be reused repeatedly, and the process is clean and pollution-free.

[0067] In the description of the present application, "multiple" means two or more than two, unless otherwise clearly and specifically defined. Unless otherwise clearly defined and defined, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances. Although the present invention has been described with reference to various specific embodiments, it should be understood that variations can be made within the spirit and scope of the described inventive concept. Therefore, it is intended that the present invention is not limited to the described embodiments, but will have the full scope defined by the language of the appended claims.

Claims

1. A device for quickly removing aluminum from the cavity of an extrusion die, characterized in that: include: A replacement rod (100) having a material melting point lower than that of an extrusion die, an extrusion system (200), an induction heating furnace (300) and a crystallization container mechanism (400), wherein the extrusion system (200) comprises: a die seat (203) for fixing an extrusion die (202) via a die sleeve (201), a pressure residue shear (204) for cutting off pressure residue (306), an extrusion cylinder (220), and an extrusion rod (212), wherein the extrusion cylinder (220) comprises a pressure residue shear (204) for the replacement rod (100) to pass through when being extruded. The induction heating furnace (300) comprises a collecting funnel (307) for collecting the molten material of the replacement rod (100); and the crystallization container mechanism (400) comprises a crystallizer for accommodating the molten material from the collecting funnel (307).

2. The device for rapidly removing aluminum from the cavity of an extrusion die according to claim 1, characterized in that: It also includes a plurality of die sleeves (201), each die sleeve (201) having an inner circle that is consistent with the outer circle diameter of a different extrusion die (202), and having outer circle diameters that are consistent with each other, so as to be compatible with extrusion dies (202) of various diameters.

3. The device for rapidly removing aluminum from the cavity of an extrusion die according to claim 1, characterized in that: The extrusion system (200) further includes: a movable beam (213) connected to the extrusion rod (212), a main thrust rod (205) and a main cylinder (206) for pushing the movable beam (213), a front beam (207) for setting the mold seat (203), a rear beam (214) for setting the main cylinder (206), and a pull rod (208) connected between the front beam (207) and the rear beam (214).

4. The device for rapidly removing aluminum from the cavity of an extrusion die according to claim 3, characterized in that: The mold base (203) is in the form of a U-shaped structure with an upper opening, and the mold base (203) is provided with a protrusion for restricting the movement of the mold sleeve (201).

5. The device for rapidly removing aluminum from the cavity of an extrusion die according to claim 1, characterized in that: The induction heating furnace (300) further comprises: a ceramic lining (301), an induction coil (302), a heat-insulating outer shell (303), and a heat-insulating cover (304).

6. The device for rapidly removing aluminum from the internal cavity of an extrusion die according to claim 1, characterized in that: The crystallization container mechanism (400) includes a multi-stage crystallizer, and the adjacent crystallizers at each stage are arranged as a whole in a stepped shape with a high middle and gradually lower levels for step-by-step overflow filling. The interior of each crystallizer is a crystallizer inner cavity (406) for accommodating the melt melted from the induction heating furnace (300).

7. The device for rapidly removing aluminum from the cavity of an extrusion die according to claim 6, characterized in that: An outermost liquid baffle (407) is provided at the outermost crystallizer to prevent the melt from overflowing, and / or a plurality of groups of multi-stage crystallization containers are arranged so that the overall appearance is in the shape of a cross.

8. The device for rapidly removing aluminum from the cavity of an extrusion die according to claim 1, characterized in that: The displacer rod material is lead and / or tin.

9. A process for rapidly removing aluminum from the cavity of an extrusion die, based on the device described in any one of claims 1 to 8, characterized in that: The process comprises the following steps: The extrusion die (202) is installed in the corresponding die sleeve (201), and the die sleeve (201) is installed in the die seat (203); The replacement rod (100) is fed into the extrusion cylinder (220), and the extrusion cylinder (220) with the replacement rod (100) is abutted against the mold seat (203); The extrusion rod (212) moves with the extrusion pad (211) toward the die seat (203), and the extrusion replacement rod (100) continues to move from the extrusion cylinder (220) into the extrusion die (202) and is partially extruded from the extrusion die (202), so that the aluminum in the extrusion die (202) is replaced by the replacement rod (100); When the replacement rod (100) that has not entered the extrusion die (202) has a predetermined length remaining, the extrusion rod (212) and the extrusion pad (211) stop moving and retreat, and the extrusion cylinder (220) retreats, and the replacement rod (100) of the predetermined length remaining as the extrusion residue (306) is cut off by the extrusion residue shear (204); The aluminum profile extruded from the middle of the extrusion die (202) and the replacement rod combination profile (305), the residual pressure (306) and at least the extrusion die (202) filled with the replacement rod (100) material are placed on a collecting funnel (307), and the induction heating furnace (300) is powered on and heated to a certain temperature and kept warm, so that the melted replacement rod material melt flows from the collecting funnel (307) into the crystallizer below.

10. The process flow for rapidly removing aluminum from the internal cavity of an extrusion die according to claim 9, characterized in that: After the displacement rod material solidifies in the crystallizer, the bottom baffle (409) below the crystallizer is opened and knocked from above to demould the displacement rod (100).

Citation Information

Patent Citations

  • Method for cleaning an extrusion die

    CN111295250A

  • Novel composite material manufactured die cleaning rod for aluminum extrusion and application of novel composite material manufactured die cleaning rod

    CN115921566A

  • Manufacture and device for molding

    JP1996047220A

  • Method for removing residual slag from aluminum extruding die and apparatus therefor

    JP2007196272A