Magnetic positioning method for ceramic core
By applying magnetic coating on the surface of the positioning core head of the ceramic core and photocuring, the precise positioning of the ceramic core is achieved on the metal wax press mold using the magnetic effect, the low accuracy and wear problems of traditional slot positioning methods are solved, and the improvement of the improvement of the improvement of the accuracy and wear of the traditional slot positioning method. Productivity and positioning accuracy are achieved.
Patent Information
- Application Number
- CN202411163481.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-29
AI Technical Summary
The positioning accuracy of the ceramic core on the wax pressing mold is low, inconvenient to operate, and the positioning slot is prone to wear, which affects the dimensional accuracy and production efficiency of the turbine blade cavity.
Magnetic coating is used to coat the surface of the positioning core head of the ceramic core and a large-size ceramic core with a magnetic positioning core head is prepared through photocuring technology, and precise positioning is achieved on the metal wax press mold using magnetic effect.
It improves the positioning accuracy and production efficiency of the ceramic core, reduces wear caused by physical contact, extends the service life of the mold, and achieves fast response and high-precision positioning.
Smart Images

Figure CN119035456A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of investment casting, and in particular provides a magnetic positioning method for a ceramic core. Background Art
[0002] Heavy-duty gas turbine blades generally have complex hollow air-cooling channels to achieve their target cooling effect. The above-mentioned air-cooling channels are currently mainly manufactured through a ceramic core precision casting process, which generally includes wax pressing, shell making, pouring, core removal and other post-processing. Among them, wax pressing is an important process to obtain the turbine blade shape and the dimensional accuracy of the internal hollow air-cooling channel.
[0003] At present, injection molding is the main way to form blade wax molds, which mainly includes three stages: positioning and clamping the ceramic core on the wax mold, filling and curing the wax material, and cooling and opening the wax mold. The positioning accuracy and efficiency of the ceramic core on the wax mold directly determine the dimensional accuracy of the blade cavity and production efficiency. At present, the ceramic core in the wax mold adopts the traditional slot positioning method, which has problems such as low positioning accuracy, difficulty in adjusting the positioning point, and easy wear of the positioning slot.
[0004] Therefore, how to improve the positioning method of the ceramic core on the wax injection mold becomes an urgent problem to be solved. Summary of the invention
[0005] The purpose of the present invention is to provide a magnetic positioning method for ceramic cores to solve the problems of low positioning accuracy, inconvenient operation and the like of large-size ceramic cores in the prior art.
[0006] In order to achieve the above object, the present invention provides a ceramic core magnetic positioning method, comprising:
[0007] Step 1: Determine the position of the positioning core head of the ceramic core to be positioned on the wax injection mold, and mark the area to be positioned on the positioning core head;
[0008] Step 2: Apply magnetic paint on the surface of the pre-positioning area of the positioning core head;
[0009] Step 3: solidify the magnetic material coated on the surface of the positioning area to obtain a large-sized ceramic core with a magnetic positioning core head;
[0010] Step 4: Position the large-size ceramic core on the metal wax mold using the magnetic positioning core head.
[0011] Preferably, the preparation method of the magnetic coating is:
[0012] Step 21: Weighing by weight percentage: 10-20wt% of Nd-Fe-B powder with an average particle size of 50 microns, 30-40wt% of Nd-Fe-B powder with an average particle size of 40 microns, and 40-60wt% of Nd-Fe-B powder with an average particle size of 20 microns, and uniformly mixing them to obtain a mixed powder;
[0013] Step 22: Dry the mixed powder at 110-130°C for 5-7h;
[0014] Step 23: Evenly mix the dried mixed powder and the photocurable resin to obtain a slurry, wherein the ratio of the mixed powder to the photocurable resin is 60-70:30-40 by weight percentage;
[0015] Step 24: homogenize the slurry to obtain magnetic coating.
[0016] Preferably, the light-curable resin is 8602UV glue, K2018 UV glue, or 9310UV glue.
[0017] Preferably, the magnetic coating is applied in step 2 by dipping, spraying with a spray gun or brushing.
[0018] Preferably, in step 2, the coating layer formed by applying the magnetic coating on the surface of the pre-positioning area of the positioning core head has a thickness of 0.15-0.5 mm.
[0019] Preferably, the curing in step 3 is performed by light curing, and the light curing parameters are: 110 mw / cm 2 The coating layer is irradiated with ultraviolet light for 3-30s.
[0020] The present invention provides a method for magnetic positioning of ceramic cores, which is applied to the wax pressing process of large-sized ceramic cores. By preparing a large-sized ceramic core with a magnetic positioning core head, the core can be accurately positioned on a metal wax pressing mold. Compared with the traditional slot positioning method, the magnetic positioning of the present invention has the following three advantages: (1) Fast response: The magnetic positioning technology has a fast response speed and can quickly locate and adjust the position of the ceramic core, thereby improving production efficiency and accuracy. (2) High-precision positioning: The magnetic positioning technology has a high positioning accuracy, which is very beneficial for ceramic cores that require high-precision positioning. (3) Non-contact positioning: The magnetic positioning technology does not require physical contact, which can reduce wear and errors caused by contact, and is more effective in protecting the ceramic core. It can also reduce mold wear and extend its service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work:
[0022] Figure 1 A schematic structural diagram of a large-sized ceramic core with a magnetic positioning core head provided by the present invention. DETAILED DESCRIPTION
[0023] The present invention will be further explained below in conjunction with specific implementation schemes, but the present invention is not limited thereto.
[0024] When using ceramic core precision casting process to manufacture heavy-duty gas turbine turbine blades, wax pressing is an important process to obtain qualified turbine blade shape and internal hollow air cooling channel dimensional accuracy. At present, ceramic cores in wax pressing molds all use traditional slot positioning methods, which have problems such as low positioning accuracy, difficulty in adjusting positioning points, and easy wear of positioning slots. To this end, this implementation scheme provides a magnetic positioning method for large-size ceramic core wax pressing process, and its process route is:
[0025] Step 1: Determine the specific positioning core head of the ceramic core product in the wax pressing process and mark the corresponding position;
[0026] Step 2, preparing a magnetic coating material, and coating the magnetic material on the surface of the positioning core head;
[0027] Step 3, curing the area treated in step 2 by light curing;
[0028] Step 4: Complete the large-sized ceramic core with magnetic positioning core head.
[0029] Wherein preparing magnetic coating material:
[0030] 1. Weigh 10-20wt% of Nd-Fe-B powder with an average particle size of 50 microns, 30-40wt% of Nd-Fe-B powder with an average particle size of 40 microns, and 40-60wt% of Nd-Fe-B powder with an average particle size of 20 microns, respectively, and mix the above powders evenly, and put them into a drying device and dry them at 120°C for 5 hours. Selecting Nd-Fe-B powders of different particle sizes in different proportions in the coating will affect the magnetic size of the magnetic coating material. A single powder particle size will cause more voids in the filling system, while when multiple particle sizes are mixed, small particles can fill the voids to the greatest extent and improve the magnetism. If the powder is too fine and the overall specific surface area is large, it will be easy to oxidize, resulting in a decrease in the magnetism of the magnetic coating material.
[0031] 2. The dried powder and the photocurable resin (8602UV glue) are mixed evenly at a weight percentage of 65:35 to form a slurry. The slurry is homogenized in a homogenizing and stirring device for 2 hours to form a magnetic coating material.
[0032] Apply magnetic material on the surface of the ceramic core wax positioning core head and solidify it: apply the magnetic coating material to the marked positioning core head position by dipping, spraying or brushing, and control the coating thickness to 0.15-0.5mm. Use 110mw / cm 2 The coating layer is irradiated with ultraviolet light for 3-30 seconds to achieve photocuring of the coating layer, thereby obtaining a large-sized ceramic core with a magnetic positioning core head.
[0033] Example 1
[0034] Determine the specific positioning core head of the ceramic core product in the wax pressing process and mark the corresponding position;
[0035] Preparation of magnetic coating material: Weigh 20wt% of Nd-Fe-B powder with an average particle size of 50 microns, 40wt% of Nd-Fe-B powder with an average particle size of 40 microns, and 40wt% of Nd-Fe-B powder with an average particle size of 20 microns respectively, mix the above powders evenly, and put them into a drying device to dry at 120°C for 5 hours. 2. Mix the above dried powders with light-curing resin (8602UV glue) at a weight percentage of 65:35 to form a slurry, and place the slurry in a homogenizing and stirring device for 2 hours to form a magnetic coating material.
[0036] Apply magnetic material on the surface of the ceramic core wax positioning core head and solidify it: apply the magnetic coating material to the marked positioning core head position by dipping, spraying or brushing, and control the coating thickness to 0.5mm. Use 110mw / cm 2 The coating layer is irradiated with ultraviolet light for 30 seconds to achieve photocuring of the coating layer, thereby obtaining a large-sized ceramic core with a magnetic positioning core head.
[0037] Example 2
[0038] Determine the specific positioning core head of the ceramic core product in the wax pressing process and mark the corresponding position;
[0039] Preparation of magnetic coating material: 1. Weigh 15wt% of Nd-Fe-B powder with an average particle size of 50 microns, 35wt% of Nd-Fe-B powder with an average particle size of 40 microns, and 50wt% of Nd-Fe-B powder with an average particle size of 20 microns, mix the above powders evenly, and put them into a drying equipment and dry them at 120°C for 5 hours.
[0040] The dried powder and the light-curing resin (8602UV glue) were mixed evenly at a weight percentage of 65:35 to form a slurry, and the slurry was homogenized in a homogenizing stirring device for 2 hours to prepare a magnetic coating material.
[0041] Apply magnetic material on the surface of the ceramic core wax positioning core head and solidify it: apply the magnetic coating material to the marked positioning core head position by dipping, spraying or brushing, and control the coating thickness to 0.2mm. Use 110mw / cm 2 The coating layer is irradiated with ultraviolet light for 20 seconds to achieve photocuring of the coating layer, thereby obtaining a large-sized ceramic core with a magnetic positioning core head.
[0042] Example 3
[0043] Determine the specific positioning core head of the ceramic core product in the wax pressing process and mark the corresponding position;
[0044] Preparation of magnetic coating material: 1. Weigh 10wt% Nd-Fe-B powder with an average particle size of 50 microns, 30wt% Nd-Fe-B powder with an average particle size of 40 microns, and 60wt% Nd-Fe-B powder with an average particle size of 20 microns, respectively, mix the above powders evenly, and put them into a drying equipment and dry them at 120°C for 5 hours.
[0045] The dried powder and the light-curing resin (8602UV glue) were mixed evenly at a weight percentage of 65:35 to form a slurry, and the slurry was homogenized in a homogenizing stirring device for 2 hours to prepare a magnetic coating material.
[0046] Apply magnetic material on the surface of the ceramic core wax positioning core head and solidify it: apply the magnetic coating material to the marked positioning core head position by dipping, spraying or brushing, and control the coating thickness to 0.15mm. Use 110mw / cm 2 The coating layer is irradiated with ultraviolet light for 3s to achieve photocuring of the coating layer, thereby obtaining a large-sized ceramic core with a magnetic positioning core head.
[0047] The detailed description of the present invention is written in a progressive manner, emphasizing the differences between the various implementations, and similar parts thereof can be referred to each other.
[0048] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A ceramic core magnetic positioning method, characterized in that: include: Step 1: Determine the position of the positioning core head of the ceramic core to be positioned on the wax injection mold, and mark the area to be positioned on the positioning core head; Step 2: Apply magnetic paint on the surface of the pre-positioning area of the positioning core head; Step 3: solidify the magnetic material coated on the surface of the positioning area to obtain a large-sized ceramic core with a magnetic positioning core head; Step 4: Position the large-size ceramic core on the metal wax mold using the magnetic positioning core head.
2. A ceramic core magnetic positioning method according to claim 1, characterized in that: The preparation method of the magnetic coating is: Step 21: Weighing by weight percentage: 10-20wt% of Nd-Fe-B powder with an average particle size of 50 microns, 30-40wt% of Nd-Fe-B powder with an average particle size of 40 microns, and 40-60wt% of Nd-Fe-B powder with an average particle size of 20 microns, and uniformly mixing them to obtain a mixed powder; Step 22: Dry the mixed powder at 110-130°C for 5-7h; Step 23: Evenly mix the dried mixed powder and the photocurable resin to obtain a slurry, wherein the ratio of the mixed powder to the photocurable resin is 60-70:30-40 by weight percentage; Step 24: homogenize the slurry to obtain magnetic coating.
3. A ceramic core magnetic positioning method according to claim 1, characterized in that: The light-curable resin is one of 8602UV glue, K2018 UV glue, and 9310UV glue.
4. A ceramic core magnetic positioning method according to claim 1, characterized in that: The magnetic coating is applied in step 2 by dipping, spraying with a spray gun or brushing.
5. A ceramic core magnetic positioning method according to claim 1, characterized in that: In step 2, the coating layer formed by applying the magnetic coating on the surface of the pre-positioning area of the positioning core head has a thickness of 0.15-0.5 mm.
6. A ceramic core magnetic positioning method according to claim 1, characterized in that: The curing in step 3 is performed by light curing, and the parameters of light curing are: 110mw / cm 2 The coating layer is irradiated with ultraviolet light for 3-30s.