Efficient heat exchange control method for tundish of thick slab continuous casting machine

By increasing the temperature of steel on the water and adjusting the intermediate chartered vehicle movement and crystallizer operation, the problem of low heat exchange success rate of the thick slab continuous casting machine is solved, efficient heat exchange is achieved, and production efficiency and casting rate are improved.

CN119035481APending Publication Date: 2024-11-29SHANDONG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411159033.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The tundra heat exchange rate and low efficiency of thick slab continuous casting machine have low tundra heat exchange rate, resulting in high production efficiency and cost problems.

Method used

By increasing the temperature of steel on the steel during the heat exchange stop pouring furnace, heating the standby tundra, and stop heating the standby tundra during the pouring process, moving the chartered vehicle to a certain distance from the pouring position, slow down the speed and wait for the steel water liquid After the surface reaches the stop-water liquid level, switch it and use high-temperature steel water for heat exchange to ensure that there is no cold steel crust in the liquid surface in the crystallizer. Adjust the crystallizer pull speed and the water in the roller to achieve efficient heat exchange.

Benefits of technology

The success rate and efficiency of the tundra heat exchange of thick slab continuous casting machine is improved, production costs are saved, and the passing rate of casting is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a control method for the heat exchange process of a tundish of a continuous casting machine. According to the efficient heat exchange control method for the tundish of the thick slab continuous casting machine, the production efficiency of the thick slab continuous casting machine can be improved, the success rate of heat exchange is increased, the production cost is saved, and the qualification rate of casting blanks is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of heat exchange process of a tundish of a thick slab continuous casting machine, and relates to a control method for the heat exchange process of a tundish of a continuous casting machine, and in particular to a high-efficiency heat exchange control method for a tundish of a thick slab continuous casting machine. Background Art

[0002] Faced with overcapacity and increasingly severe competition in the homogeneity of high-end products, efficient and low-cost production has become a powerful way for modern steel companies to seek development. The efficient heat exchange process of the tundish of the continuous casting machine has the advantages of long continuous casting cycle, high molten steel recovery rate, low manufacturing cost, and low labor intensity, and is widely used in large domestic steel mills. At present, the heat exchange method used by thick slab continuous casting machines is mostly heat exchange by plugging connectors. Due to many restrictive factors, the probability of failure is relatively high.

[0003] Therefore, how to find a more suitable way to solve the above-mentioned technical problems existing in the existing process has become one of the urgent problems to be solved by many front-line researchers in the industry. Summary of the invention

[0004] In view of this, the technical problem to be solved by the present invention is to provide a control method for the heat exchange process of the tundish of a continuous casting machine, in particular, a high-efficiency heat exchange control method for the tundish of a thick slab continuous casting machine. The control method provided by the present invention can improve the production efficiency of the thick slab continuous casting machine, improve the success rate of heat exchange, save production costs, and improve the qualified rate of the casting.

[0005] The present invention provides a method for controlling a heat exchange process of a tundish of a continuous casting machine, comprising the following steps:

[0006] 1) Increase the upper temperature of the molten steel poured into the tundish in use when the heat exchange furnace is stopped, and heat the tundish to be used;

[0007] 2) During the pouring process of the hot exchange stop pouring furnace, when the remaining molten steel in the tundish reaches a certain amount, stop heating the standby tundish, move the tundish car carrying the standby tundish to a certain distance from the pouring position and wait, and slow down the pulling speed of the crystallizer during the movement;

[0008] 3) When the molten steel level in the tundish in use reaches the stop-pouring level, the mold pulling speed is returned to zero, the tundish car carrying the tundish in use is driven away from the pouring position, and the tundish car carrying the standby tundish is driven into the pouring position; at the same time, the pouring of the large ladle of the hot-switching stop-pouring furnace is completed, and the large ladle of the hot-switching start-pouring furnace is transferred to the pouring position to wait;

[0009] 4) After the standby tundish is opened to the pouring position, the hot-swap ladle water inlet for the pouring furnace is hung and the ladle slide is fully opened to pour the molten steel in the ladle into the standby tundish;

[0010] The molten steel in the ladle is the molten steel from the hot-exchange pouring furnace;

[0011] The upper temperature of the molten steel in the hot-exchange pouring furnace is higher than the upper temperature of the molten steel in the subsequent continuous pouring furnaces;

[0012] 5) When the molten steel in the standby tundish reaches the tundish pouring conditions, pour the molten steel in the standby tundish into the crystallizer. After the crystallizer meets the conditions, start the crystallizer pulling speed and maintain it for a certain period of time, then increase the crystallizer pulling speed and adjust the crystallizer full roller water for heat exchange and pouring.

[0013] Preferably, in the step 1), the upper steel temperature is raised specifically by raising the upper steel temperature of the molten steel poured into the tundish in the hot exchange stop pouring furnace by 10°C based on the temperature of the continuous pouring furnace;

[0014] In the step 4), the upper temperature of the molten steel in the hot-exchange pouring furnace is higher than the upper temperature of the subsequent molten steel in the continuous pouring furnace, specifically, 20° C. higher than the upper temperature of the subsequent molten steel in the continuous pouring furnace.

[0015] Preferably, in step 2), the remaining amount is specifically 12-13 tons and / or the molten steel level in the tundish is reduced to 600 mm;

[0016] When stopping heating of the standby tundish, ensure that the stopper rod and the upper water inlet bowl of the tundish are not blocked by collapsed materials.

[0017] Preferably, in step 2), the certain distance is specifically 300 to 500 mm;

[0018] The speed reduction operation includes reducing the speed until the pulling speed returns to zero, and ensuring that the tundish car carrying the tundish to be used reaches the pouring position.

[0019] Preferably, the stop pouring liquid level is specifically when the molten steel level is 300 mm;

[0020] When the molten steel level reaches the stop-casting level, the mold pulling speed is reduced to 0.4 m / min;

[0021] The method further comprises one or more steps of closing the stopper rod, inserting the blind plate and setting the crystallizer pulling speed of the hot exchange pouring furnace before the tundish car carrying the tundish in use leaves the pouring position.

[0022] Preferably, when the ladle of the hot-swap pouring furnace is transferred to the pouring position to wait, the ladle arm of the pouring position is in a high position;

[0023] When the ladle slide plates are fully opened, the ladle arms fall down to a normal steel pouring position.

[0024] Preferably, the process of switching between the active tundish and the standby tundish also includes one or more steps of checking the liquid level in the crystallizer, checking the slag bars in the crystallizer, removing large slag bars in the crystallizer, ensuring that there is no cold steel crust on the liquid surface, placing fiber cotton on the narrow surface of the crystallizer, and centering the crystallizer and the standby tundish.

[0025] Preferably, during the heat exchange process of the tundish of the continuous casting machine, there is no need to remove the mold protection slag;

[0026] The conditions for starting pouring in the tundish are specifically that the molten steel in the tundish reaches 5 to 6 tons, and the liquid level of the molten steel in the tundish is above the side holes of the submerged nozzle.

[0027] Preferably, the crystallizer satisfies the condition that the liquid level in the crystallizer rises;

[0028] The maintaining for a certain period of time specifically refers to maintaining for 2 to 3 minutes.

[0029] Preferably, the crystallizer pulling speed is increased by 0.05 m / min every 40 seconds, and the speed is increased to 0.4 m / min and maintained for 1 minute;

[0030] The process of increasing the casting speed of the crystallizer also includes the steps of shallow slag replacement and molten steel level inspection in the crystallizer.

[0031] The present invention provides a control method for a tundish heat exchange process of a continuous casting machine, comprising the following steps: firstly, the upper steel temperature of the molten steel poured into the tundish in use during the heat exchange stop-casting furnace is increased to heat the standby tundish; then, during the pouring process of the heat exchange stop-casting furnace, when the molten steel in the tundish in use remains to a certain amount, the heating of the standby tundish is stopped, and the tundish car carrying the standby tundish is moved to a certain distance from the pouring position for waiting, and the pulling speed of the crystallizer is reduced during the movement; when the molten steel level in the tundish in use reaches the stop-casting level, the pulling speed of the crystallizer is returned to zero, the tundish car carrying the tundish in use is driven away from the pouring position, and the tundish car carrying the standby tundish is driven into the pouring position; and at the same time, the heat After the ladle pouring of the stopped pouring furnace is finished, the ladle of the hot-changing pouring furnace is transferred to the pouring position to wait; then, after the standby tundish is opened to the pouring position, the ladle water inlet of the hot-changing pouring furnace is hung and the ladle slide plate is fully opened, and the molten steel in the ladle is poured into the standby tundish; the molten steel in the ladle is the molten steel of the hot-changing pouring furnace; the upper steel temperature of the molten steel of the hot-changing pouring furnace is higher than the subsequent upper steel temperature of the continuous pouring furnace; finally, when the molten steel in the standby tundish reaches the tundish pouring condition, the molten steel in the standby tundish is poured into the crystallizer, and after the crystallizer meets the condition, the crystallizer pulling speed is turned on and maintained for a certain period of time, the crystallizer pulling speed is increased and the crystallizer is adjusted to have enough roller water, and pouring is performed after heat exchange. Compared with the prior art, in order to solve the problem of low success rate and low efficiency of heat exchange of the tundish of the thick slab continuous casting machine, the present invention studies the heat exchange process of the tundish of the thick slab continuous casting machine, and improves the success rate and efficiency of heat exchange of the tundish of the thick slab continuous casting machine.

[0032] The present invention particularly designs a control method for the heat exchange process of the tundish of a continuous casting machine with specific steps and procedures, which is an efficient heat exchange control method for the tundish of a thick slab continuous casting machine. The control method provided by the present invention can improve the production efficiency of the thick slab continuous casting machine, improve the success rate of heat exchange, save production costs, and improve the qualified rate of the casting. DETAILED DESCRIPTION

[0033] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention rather than limiting the patent claims of the present invention.

[0034] The codes and abbreviations of all processes of the present invention are conventional codes and abbreviations in the field. Each code and abbreviation is clear and unambiguous in its relevant application field. Those skilled in the art can understand the function and process of the process based on the codes, abbreviations and corresponding expressions.

[0035] The present invention provides a method for controlling a heat exchange process of a tundish of a continuous casting machine, comprising the following steps:

[0036] 1) Increase the upper temperature of the molten steel poured into the tundish in use when the heat exchange furnace is stopped, and heat the tundish to be used;

[0037] 2) During the pouring process of the hot exchange stop pouring furnace, when the remaining molten steel in the tundish reaches a certain amount, stop heating the standby tundish, move the tundish car carrying the standby tundish to a certain distance from the pouring position and wait, and slow down the pulling speed of the crystallizer during the movement;

[0038] 3) When the molten steel level in the tundish in use reaches the stop-pouring level, the mold pulling speed is returned to zero, the tundish car carrying the tundish in use is driven away from the pouring position, and the tundish car carrying the standby tundish is driven into the pouring position; at the same time, the pouring of the large ladle of the hot-switching stop-pouring furnace is completed, and the large ladle of the hot-switching start-pouring furnace is transferred to the pouring position to wait;

[0039] 4) After the standby tundish is opened to the pouring position, the hot-swap ladle water inlet for the pouring furnace is hung and the ladle slide is fully opened to pour the molten steel in the ladle into the standby tundish;

[0040] The molten steel in the ladle is the molten steel from the hot-exchange pouring furnace;

[0041] The upper temperature of the molten steel in the hot-exchange pouring furnace is higher than the upper temperature of the molten steel in the subsequent continuous pouring furnaces;

[0042] 5) When the molten steel in the standby tundish reaches the tundish pouring conditions, pour the molten steel in the standby tundish into the crystallizer. After the crystallizer meets the conditions, start the crystallizer pulling speed and maintain it for a certain period of time, then increase the crystallizer pulling speed and adjust the crystallizer full roller water for heat exchange and pouring.

[0043] The present invention firstly increases the upper steel temperature of the molten steel poured into the tundish in use when the heat exchange furnace stops pouring, and heats the tundish to be used.

[0044] In the present invention, in the step 1), the upper steel temperature is preferably increased by 10° C. on the basis of the upper steel temperature of the molten steel poured into the tundish in the hot exchange stop pouring furnace.

[0045] In the present invention, during the pouring process of the hot exchange stop pouring furnace, when the molten steel in the used tundish remains to a certain amount, the heating of the standby tundish is stopped, and the tundish car carrying the standby tundish is moved to a certain distance from the pouring position to wait, and the pulling speed of the crystallizer is reduced during the movement.

[0046] In the present invention, in the step 2), the remaining certain amount is preferably 12-13 tons and / or the molten steel level in the tundish is reduced to 600 mm, more preferably 12.2-12.8 tons and / or the molten steel level in the tundish is reduced to 600 mm, more preferably 12.4-12.6 tons and / or the molten steel level in the tundish is reduced to 600 mm.

[0047] In the present invention, when the heating of the standby tundish is stopped, it is preferably ensured that the stopper rod and the upper water inlet bowl of the tundish are not blocked by collapsed materials.

[0048] In the present invention, in the step 2), the certain distance is preferably 300 to 500 mm, more preferably 340 to 460 mm, and more preferably 380 to 420 mm.

[0049] In the present invention, the speed reduction operation preferably includes ensuring that the tundish car carrying the tundish to be used reaches the pouring position before the speed is reduced to zero.

[0050] Then, when the molten steel level in the tundish in use reaches the stop-casting liquid level, the pulling speed of the crystallizer is returned to zero, the tundish car carrying the tundish in use is driven away from the pouring position, and the tundish car carrying the standby tundish is driven into the pouring position; at the same time, the pouring of the large ladle of the hot-exchange stop-casting furnace is completed, and then the large ladle of the hot-exchange start-casting furnace is transferred to the pouring position to wait.

[0051] In the present invention, the stop pouring liquid level is preferably a molten steel liquid level of 300 mm.

[0052] In the present invention, when the molten steel level reaches the stop-casting level, the mold pulling speed is preferably reduced to 0.4 m / min;

[0053] In the present invention, the tundish car carrying the tundish preferably also includes one or more of the steps of closing the stopper rod, installing a blind plate, and setting the crystallizer pulling speed of the heat exchange casting furnace before leaving the pouring position, and more preferably includes multiple of the steps of closing the stopper rod, installing a blind plate, and setting the crystallizer pulling speed of the heat exchange casting furnace.

[0054] In the present invention, when the ladle of the hot-swap pouring furnace is transferred to the pouring position to wait, the ladle arm at the pouring position is preferably in a high position.

[0055] The present invention then opens the standby tundish to the pouring position, hangs the hot-swap ladle water inlet for the pouring furnace, and fully opens the ladle slide plate to pour the molten steel in the ladle into the standby tundish;

[0056] The molten steel in the ladle is the molten steel from the hot-exchange pouring furnace;

[0057] The upper temperature of the molten steel in the heat exchange pouring furnace is higher than the upper temperature of the molten steel in the subsequent continuous pouring furnaces.

[0058] In the present invention, in step 4), the upper temperature of the molten steel in the heat exchange first pouring furnace is higher than the upper temperature of the subsequent molten steel in the continuous pouring furnace, and preferably, is 20° C. higher than the upper temperature of the subsequent molten steel in the continuous pouring furnace.

[0059] In the present invention, when the ladle slide plate is fully opened, the ladle arm is preferably lowered to a normal steel pouring position.

[0060] Finally, when the molten steel in the standby tundish reaches the tundish pouring condition, the molten steel in the standby tundish is poured into the crystallizer. After the crystallizer meets the conditions, the pulling speed of the crystallizer is started and maintained for a certain period of time, the pulling speed of the crystallizer is increased and the water content of the crystallizer roller is adjusted to perform heat exchange and pouring.

[0061] In the present invention, the process of switching between the active tundish and the standby tundish preferably also includes one or more steps of checking the liquid level in the crystallizer, checking the slag bars in the crystallizer, removing large slag bars in the crystallizer, ensuring that there is no cold steel crust on the liquid surface, placing fiber cotton on the narrow surface of the crystallizer, and centering the crystallizer and the standby tundish, and more preferably includes multiple steps of checking the liquid level in the crystallizer, checking the slag bars in the crystallizer, removing large slag bars in the crystallizer, ensuring that there is no cold steel crust on the liquid surface, placing fiber cotton on the narrow surface of the crystallizer, and centering the crystallizer and the standby tundish.

[0062] In the present invention, during the heat exchange process of the tundish of the continuous casting machine, it is preferably not necessary to remove the mold protection slag.

[0063] In the present invention, the tundish pouring conditions are preferably that the molten steel in the tundish reaches 5 to 6 tons, and the molten steel level in the tundish submerges the side holes of the submerged nozzle, more preferably 5.2 to 5.8 tons, and more preferably 5.4 to 5.6 tons.

[0064] In the present invention, the crystallizer satisfies the condition that the liquid level in the crystallizer rises.

[0065] In the present invention, the maintaining time is preferably 2 to 3 minutes, more preferably 2.2 to 2.8 minutes, and more preferably 2.4 to 2.6 minutes.

[0066] In the present invention, the crystallizer pulling speed is preferably increased by 0.05 m / min every 40 s, and the speed is increased to 0.4 m / min and maintained for 1 min.

[0067] In the present invention, the process of increasing the casting speed of the crystallizer preferably also includes the steps of shallow slag replacement and molten steel level inspection in the crystallizer.

[0068] The present invention is to complete and refine the overall technical solution, better ensure the controllability of the heat exchange process of the tundish of the continuous casting machine, and further improve the production efficiency and success rate of the heat exchange process of the tundish of the continuous casting machine. The above-mentioned high-efficiency heat exchange control method of the tundish of the thick slab continuous casting machine may specifically include the following contents:

[0069] The technical solution adopted by the present invention is a high-efficiency heat exchange control method for the tundish of a thick slab continuous casting machine, and the specific implementation steps are as follows:

[0070] 1. Contractor A is responsible for strengthening the inspection of the tundish baking process to prevent material collapse from affecting the baking effect of the tundish and the submerged nozzle.

[0071] 2. In order to deal with the problem of billet shell shrinkage during the heat exchange process, the steel temperature of the hot exchange stop pouring furnace is 10℃ higher than that of the continuous pouring furnace; the steel temperature of the hot exchange start pouring furnace is 20℃ higher than that of the continuous pouring furnace. The high superheat can effectively alleviate the thermal shrinkage and phase change shrinkage of the billet shell.

[0072] 3. During the pouring process of the heat exchange furnace, the contractor A performs slag discharge to avoid slag discharge accidents during the low liquid level pouring process of the tundish. The steelmaker A handles the slag bars in the crystallizer before the heat exchange to avoid explosion and leakage accidents during the heat exchange.

[0073] 4. When there are 12 to 13 tons of molten steel (molten steel level is 600mm) remaining in the tundish of the stopped pouring furnace, steel worker B will turn off the fire of the tundish to be replaced, lift the baking device, check and confirm the tundish stopper rod and the bowl of the upper water inlet to ensure that there is no blockage by collapsed material, and then open the tundish to be replaced to a position 300 to 500mm away from the pouring position tundish car and wait.

[0074] 5. The captain shall reduce the speed according to the casting speed system for stopping pouring, and flexibly control the speed reduction process according to the operation of the standby tundish to ensure that the standby tundish car (the tundish car carrying the tundish to be replaced) is in place before the casting speed returns to zero. When the molten steel level in the tundish reaches the stop casting standard (molten steel level 300mm), the casting speed is reduced to 0.4m / min, and the captain presses the stop button to return the casting speed to zero. After 2-3 seconds, the captain notifies steel worker A to manually close the stopper rod, and steel worker C to install the blind plate and immediately press the automatic start button on the tundish car to drive the tundish car away from the casting position. The casting speed is set to 0.2m / min as the starting casting speed for the next casting. (Set, but not turned on)

[0075] 6. After the hot-changing stop-casting furnace has finished pouring the ladle, ladle worker A will transfer the hot-changing start-casting furnace to the pouring position and wait, and keep the ladle arm at the pouring position in a high position. After the tundish is opened to the pouring position, steel worker B will assist ladle worker A to hang the ladle water inlet and open the ladle slide completely, and at the same time lower the ladle arm to the normal steel pouring position to start pouring the ladle.

[0076] 7. While the tundish is moving away from the tundish area, steel puller C opens the tundish to be used to the steel pouring position and aligns it. The captain directs the whole process to ensure seamless connection between the two vehicles.

[0077] 8. During the tundish switching process, steelworker A is responsible for checking the liquid level and slag bars in the crystallizer, hooking out all the large slag bars in the crystallizer, and checking the liquid level at a high frequency to keep the liquid surface free of cold steel crust. Fiber cotton is placed on the narrow surface of the crystallizer to prevent the splashing of molten steel when pouring. When the tundish to be replaced is in place, it is quickly centered and the tundish car is lowered. After the water inlet is centered, the captain notifies the large ladle worker A to start pouring the large ladle, and continues to lower the tundish car until the operation box displays 80. The protective slag does not need to be removed during the whole process.

[0078] 9. After 5-6 tons of molten steel in the tundish, the conditions for opening the tundish are met. The captain is responsible for observing the tonnage of the tundish and the position of the side hole of the submerged nozzle after the ladle is poured. When the liquid level is above the side hole and the upper edge of the side hole is 1 cm above the liquid level, the order to open the pouring is given. Steel worker A opens the stopper rod. After the captain confirms that the liquid level in the crystallizer has risen, he immediately presses the start button and fine-tunes the nozzle insertion depth according to the rolling of the liquid level in the crystallizer. The pulling speed is maintained at 0.2m / min for 2-3min, and the speed is increased by 0.05m / min every 40S to 0.4m / min for 1 minute. A group of steel workers simultaneously perform shallow slag replacement and molten steel level inspection operations in the crystallizer, and then operate according to the pouring speed increase standard.

[0079] 10. After the casting machine stops, the main controller A will report the time in 5 seconds. After restarting, he needs to report the time again and record the number of meters. One minute after starting, he will change the full roller water valve to 100% opening, and change it back to automatic after 2 meters. According to the casting speed control model calculation described in Article 9, the full roller water is opened to 100% when the reconnection line is 0.6m away from the lower mouth of the crystallizer, and the full roller water returns to normal after the reconnection line is 1.4m away from the lower mouth of the crystallizer.

[0080] 11. After the nozzle falls into place during the heat exchange process, immediately move the slag strips around the nozzle to the middle or remove them to ensure that the joints are well reconnected. Do not adjust the centering of the immersion nozzle before 0.6 meters after restarting.

[0081] The above content of the present invention provides a method for efficiently controlling heat exchange of the tundish of a thick slab continuous casting machine. The control method of the heat exchange process of the tundish of a continuous casting machine specially designed by the present invention with specific steps and procedures is a method for efficiently controlling heat exchange of the tundish of a thick slab continuous casting machine. The control method provided by the present invention can improve the production efficiency of the thick slab continuous casting machine, improve the success rate of heat exchange, save production costs, and improve the qualified rate of cast billets. The present invention studies the heat exchange process of the tundish of a thick slab continuous casting machine, and improves the success rate and efficiency of heat exchange of the tundish of a thick slab continuous casting machine.

[0082] In order to further illustrate the present invention, a control method for the heat exchange process of the tundish of a continuous casting machine provided by the present invention is described in detail below in combination with the embodiments. However, it should be understood that these embodiments are implemented on the premise of the technical scheme of the present invention, and detailed implementation methods and specific operating processes are given only to further illustrate the features and advantages of the present invention, rather than to limit the claims of the present invention. The protection scope of the present invention is not limited to the following embodiments.

[0083] Example

[0084] 1. Contractor A is responsible for strengthening the inspection of the tundish baking process to prevent material collapse from affecting the baking effect of the tundish and the submerged nozzle.

[0085] 2. In order to deal with the problem of billet shell shrinkage during the heat exchange process, the steel temperature of the hot exchange stop pouring furnace is 10℃ higher than that of the continuous pouring furnace; the steel temperature of the hot exchange start pouring furnace is 20℃ higher than that of the continuous pouring furnace. The high superheat can effectively alleviate the thermal shrinkage and phase change shrinkage of the billet shell.

[0086] 3. During the pouring process of the heat exchange furnace, the contractor A performs slag discharge to avoid slag discharge accidents during the low liquid level pouring process of the tundish. The steelmaker A handles the slag bars in the crystallizer before the heat exchange to avoid explosion and leakage accidents during the heat exchange.

[0087] 4. When there are 12 to 13 tons of molten steel (molten steel level is 600mm) remaining in the tundish of the stopped pouring furnace, steel worker B will turn off the fire of the tundish to be replaced, lift the baking device, check and confirm the tundish stopper rod and the bowl of the upper water inlet to ensure that there is no blockage by collapsed material, and then open the tundish to be replaced to a position 300 to 500mm away from the pouring position tundish car and wait.

[0088] 5. The captain reduces the speed according to the stop-casting speed system, and flexibly controls the speed reduction process according to the operation of the standby drying tundish, ensuring that the standby drying tundish car is in place before the pulling speed returns to zero. When the molten steel level in the tundish reaches the stop-casting standard (molten steel level 300mm), the pulling speed drops to 0.4m / min, and the captain presses the stop button to return the pulling speed to zero. After 2 to 3 seconds, the captain notifies steel worker A to manually close the stopper, and steel worker C to install the blind plate, and immediately presses the automatic start button on the tundish car to drive the tundish car away from the casting position. The pulling speed is set to 0.2m / min as the starting pulling speed for the next pouring.

[0089] 6. After the hot-changing stop-casting furnace has finished pouring the ladle, ladle worker A will transfer the hot-changing start-casting furnace to the pouring position and wait, and keep the ladle arm at the pouring position in a high position. After the tundish is opened to the pouring position, steel worker B will assist ladle worker A to hang the ladle water inlet and open the ladle slide completely, and at the same time lower the ladle arm to the normal steel pouring position to start pouring the ladle.

[0090] 7. While the tundish is moving away from the tundish area, steel puller C will move the tundish to be replaced to the steel pouring position and align it. The captain will direct the entire process to ensure seamless connection between the two vehicles.

[0091] 8. During the tundish switching process, steelworker A is responsible for checking the liquid level and slag bars in the crystallizer, hooking out all the large slag bars in the crystallizer, and checking the liquid level at a high frequency to keep the liquid surface free of cold steel crust. Fiber cotton is placed on the narrow surface of the crystallizer to prevent the splashing of molten steel when pouring. When the tundish to be replaced is in place, it is quickly centered and the tundish car is lowered. After the water inlet is centered, the captain notifies the large ladle worker A to start pouring the large ladle, and continues to lower the tundish car until the operation box displays 80. The protective slag does not need to be removed during the whole process.

[0092] 9. After 5-6 tons of molten steel in the tundish, the conditions for opening the tundish are met. The captain is responsible for observing the tonnage of the tundish and the position of the side hole of the submerged nozzle after the ladle is poured. When the liquid level is above the side hole and the upper edge of the side hole is 1 cm above the liquid level, the order to open the pouring is given. Steel worker A opens the stopper rod. After the captain confirms that the liquid level in the crystallizer has risen, he immediately presses the start button and fine-tunes the nozzle insertion depth according to the rolling of the liquid level in the crystallizer. The pulling speed is maintained at 0.2m / min for 2-3min, and the speed is increased by 0.05m / min every 40S to 0.4m / min for 1 minute. A group of steel workers simultaneously perform shallow slag replacement and molten steel level inspection operations in the crystallizer, and then operate according to the pouring speed increase standard.

[0093] 10. After the casting machine stops, the main controller A will report the time in 5 seconds. After restarting, he needs to report the time again and record the number of meters. One minute after starting, he will change the full roller water valve to 100% opening, and change it back to automatic after 2 meters. According to the casting speed control model calculation described in Article 9, the full roller water is opened to 100% when the reconnection line is 0.6m away from the lower mouth of the crystallizer, and the full roller water returns to normal after the reconnection line is 1.4m away from the lower mouth of the crystallizer.

[0094] 11. After the nozzle falls into place during the heat exchange process, immediately move the slag strips around the nozzle to the middle or remove them to ensure that the joints are well reconnected. Do not adjust the centering of the immersion nozzle before 0.6 meters after restarting.

[0095] 12. Regarding the handling requirements for abnormal billets, the main controller A is responsible for informing the fire cutter A of the shutdown meters. The fire cutter A will scrap the billets 1500mm before and after the reconnection. If the fixed length before scrap cutting cannot meet the plan, it will be handled as the remaining billets, and the adjacent billets will be put on the ground for finishing inspection.

[0096] The success rate of adopting the tundish heat exchange technical solution of the thick slab continuous casting machine in the above embodiment of the present invention is 100%, and the casting change time can be saved by 20 hours every month.

[0097] The above is a detailed introduction to a method for controlling efficient heat exchange of a tundish of a thick slab continuous casting machine provided by the present invention. The principles and implementation methods of the present invention are described in detail using specific examples. The description of the above embodiments is only used to help understand the method and its core ideas of the present invention, including the best mode, and also enables any technician in the field to practice the present invention, including manufacturing and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present invention, the present invention can also be improved and modified in a number of ways, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A method for controlling heat exchange process of a tundish of a continuous casting machine, characterized in that: The following steps are involved: 1) Increase the upper temperature of the molten steel poured into the tundish in use when the heat exchange furnace is stopped, and heat the tundish to be used; 2) During the pouring process of the hot exchange stop pouring furnace, when the remaining molten steel in the tundish reaches a certain amount, stop heating the standby tundish, move the tundish car carrying the standby tundish to a certain distance from the pouring position and wait, and slow down the pulling speed of the crystallizer during the movement; 3) When the molten steel level in the tundish in use reaches the stop-pouring level, the mold pulling speed is returned to zero, the tundish car carrying the tundish in use is driven away from the pouring position, and the tundish car carrying the standby tundish is driven into the pouring position; at the same time, the pouring of the large ladle of the hot-switching stop-pouring furnace is completed, and the large ladle of the hot-switching start-pouring furnace is transferred to the pouring position to wait; 4) After the standby tundish is opened to the pouring position, the hot-swap ladle water inlet for the pouring furnace is hung and the ladle slide is fully opened to pour the molten steel in the ladle into the standby tundish; The molten steel in the ladle is the molten steel from the hot-exchange pouring furnace; The upper temperature of the molten steel in the hot-exchange pouring furnace is higher than the upper temperature of the molten steel in the subsequent continuous pouring furnaces; 5) When the molten steel in the standby tundish reaches the tundish pouring conditions, pour the molten steel in the standby tundish into the crystallizer. After the crystallizer meets the conditions, start the crystallizer pulling speed and maintain it for a certain period of time, then increase the crystallizer pulling speed and adjust the crystallizer full roller water for heat exchange and pouring.

2. The control method according to claim 1, characterized in that: In the step 1), the upper steel temperature is specifically raised by raising the upper steel temperature of the molten steel poured into the tundish in the hot exchange stop pouring furnace by 10°C based on the temperature of the continuous pouring furnace; In the step 4), the upper temperature of the molten steel in the hot-exchange pouring furnace is higher than the upper temperature of the subsequent molten steel in the continuous pouring furnace, specifically, 20° C. higher than the upper temperature of the subsequent molten steel in the continuous pouring furnace.

3. The control method according to claim 1, characterized in that: In the step 2), the remaining amount is specifically 12-13 tons and / or the molten steel level in the tundish is reduced to 600 mm; When stopping heating of the standby tundish, ensure that the stopper rod and the upper water inlet bowl of the tundish are not blocked by collapsed materials.

4. The control method according to claim 1, characterized in that: In the step 2), the certain distance is specifically 300 to 500 mm; The speed reduction operation includes reducing the speed until the pulling speed returns to zero, and ensuring that the tundish car carrying the tundish to be used reaches the pouring position.

5. The control method according to claim 1, characterized in that: The stop pouring liquid level is specifically when the molten steel level is 300mm; When the molten steel level reaches the stop-casting level, the mold pulling speed is reduced to 0.4 m / min; The method further comprises one or more steps of closing the stopper rod, inserting the blind plate and setting the crystallizer pulling speed of the hot exchange pouring furnace before the tundish car carrying the tundish in use leaves the pouring position.

6. The control method according to claim 1, characterized in that: When the ladle of the hot-changing pouring furnace is transferred to the pouring position to wait, the ladle arm of the pouring position is in a high position; When the ladle slide plates are fully opened, the ladle arms fall down to a normal steel pouring position.

7. The control method according to claim 1, characterized in that: The process of switching between the active tundish and the standby tundish also includes one or more steps of checking the liquid level in the crystallizer, checking the slag bars in the crystallizer, removing large slag bars in the crystallizer, ensuring that there is no cold steel crust on the liquid surface, placing fiber cotton on the narrow surface of the crystallizer, and centering the crystallizer and the standby tundish.

8. The control method according to claim 1, characterized in that: During the heat exchange process of the tundish of the continuous casting machine, there is no need to remove the mold protection slag; The conditions for starting pouring in the tundish are specifically that the molten steel in the tundish reaches 5 to 6 tons, and the liquid level of the molten steel in the tundish is above the side holes of the submerged nozzle.

9. The control method according to claim 1, characterized in that: The crystallizer satisfies the condition that the liquid level in the crystallizer rises; The maintaining for a certain period of time specifically refers to maintaining for 2 to 3 minutes.

10. The control method according to claim 1, characterized in that: The crystallizer pulling speed is increased by 0.05 m / min every 40 seconds, and the speed is increased to 0.4 m / min and maintained for 1 minute; The process of increasing the casting speed of the crystallizer also includes the steps of shallow slag replacement and molten steel level inspection in the crystallizer.