Method for carrying out cold isostatic pressing on hard alloy pressed blank with small thickness
By placing the cemented carbide pressing blank with a small thickness on the surface of the tempered glass and wrapping it in a tin foil insulation bag for cold isostatic pressure, the pollution and deformation problems caused by the hydraulic system are solved, and the density and strength of the cemented carbide pressing blank is improved. , ensuring the quality and pass rate of the product.
Patent Information
- Application Number
- CN202411197035.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-29
AI Technical Summary
During the cold isostatic pressing process, existing hydraulic systems are prone to contamination of cemented carbide pressure and deformation or cracking of small-thick pressing blanks, and cannot effectively deal with cemented carbide pressure blanks with a thickness of less than or equal to 10mm.
Place the cemented carbide pressing blank with a small thickness on the evenly arranged through-hole tempered glass surface, put it in a tin foil insulation bag, and wrap it with waterproof plastic, and then perform cold isostatic pressure.
The density and strength of the cemented carbide blank is improved, the appearance is kept flat, the product quality and qualification rate are improved, and the liquid penetration and deformation and cracking are avoided.
Smart Images

Figure CN119035548A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cemented carbide, and in particular relates to a method for cold isostatic pressing of a cemented carbide blank with a small thickness. Background Art
[0002] The production and preparation process of cemented carbide is mainly as follows: raw material preparation - mixture preparation - molding and pressing of green sheets - high temperature sintering - processing. Molding and pressing of green sheets is a process for forming cemented carbide. The mixture powder is compacted to obtain green sheets that meet the requirements of density uniformity, shape and dimensional accuracy. This process is intended to give the green sheets a certain strength. Cold isostatic pressing is a process after molding and pressing of green sheets. It is implemented using a cold isostatic press. The pressure system usually uses a hydraulic system to provide high pressure. By applying high pressure and low temperature, the density of the green sheet can be increased, the uniformity of the green sheet can be improved, and its shape and dimensional accuracy can be controlled. This process can obtain high-density and high-strength green sheets, providing a good foundation for subsequent sintering and processing.
[0003] There are some disadvantages in the cold isostatic pressing using hydraulic system in production applications, including: (1) Liquid will penetrate the product: The liquid used in the hydraulic system may penetrate into the compact during high-pressure operation, causing the compact to be contaminated, the density of the compact to deteriorate, and even the composition to be changed by the liquid, which can easily cause the compact to crack during sintering, making the produced cemented carbide unqualified. (2) It is impossible to press cemented carbide compacts with small thickness (≤10mm): Due to the working principle of the hydraulic system, the hydraulic pressure will generate a large lateral force during the transmission process, and the strength of cemented carbide compacts with small thickness is relatively small, which may cause them to deform or crack during the cold isostatic pressing process. Summary of the invention
[0004] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a method for cold isostatic pressing of a cemented carbide compact with a small thickness.
[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0006] A method for cold isostatic pressing of a cemented carbide compact with a small thickness comprises the following steps:
[0007] S1. placing a cemented carbide compact with a small thickness on a tempered glass surface having through holes evenly arranged in the thickness direction;
[0008] S2. Put the tempered glass with the hard alloy compact placed on the surface into a tin foil insulation bag;
[0009] S3, wrap the tin foil insulation bag containing the tempered glass with the hard alloy pressed blank placed on the surface with waterproof plastic;
[0010] S4, then put it into a cold isostatic press for cold isostatic pressing.
[0011] As a preferred embodiment of the method for cold isostatic pressing of a cemented carbide compact with a small thickness described in the present invention, in the step S1, the thickness of the cemented carbide compact is ≤10 mm.
[0012] As a preferred embodiment of the method for cold isostatic pressing of a cemented carbide blank with a small thickness described in the present invention, in the step S1, the thickness of the tempered glass is 10 to 15 mm.
[0013] As a preferred embodiment of the method for cold isostatic pressing of a cemented carbide blank with a small thickness described in the present invention, in the step S1, the diameter of the through hole is 2 to 6 mm.
[0014] As a preferred embodiment of the method for cold isostatic pressing of a cemented carbide blank with a small thickness described in the present invention, in the step S1, the contact surface between the cemented carbide blank and the tempered glass should be the surface with the largest area.
[0015] As a preferred embodiment of the method for cold isostatic pressing of a cemented carbide blank with a small thickness described in the present invention, in the step S1, the surface area of the tempered glass is larger than the area of any surface of the cemented carbide blank.
[0016] As a preferred embodiment of the method for cold isostatic pressing of a cemented carbide blank with a small thickness described in the present invention, in step S2, the surface layer of the tin foil insulation bag is a layer of waterproof aluminum film, and there is a layer of pearl cotton inside.
[0017] As a preferred embodiment of the method for cold isostatic pressing of a cemented carbide blank with a small thickness described in the present invention, in step S2, the tin foil insulation bag needs to be completely filled with the tempered glass with the cemented carbide blank placed on the surface, so that it is completely fitted with the tin foil insulation bag.
[0018] As a preferred embodiment of the method for cold isostatic pressing of a cemented carbide billet with a small thickness described in the present invention, in the step S3, when the waterproof plastic is wrapped, three layers are completely wrapped in the horizontal direction and the vertical direction respectively, and the waterproof plastic needs to be completely attached to the tin foil insulation bag during wrapping.
[0019] The beneficial effects of the present invention are as follows:
[0020] The present invention provides a method for cold isostatic pressing of a cemented carbide compact with a small thickness, wherein the cemented carbide compact with a small thickness is placed on the surface of a tempered glass having through holes evenly arranged in the thickness direction, the tempered glass with the cemented carbide compact placed on the surface is placed in a tin foil insulation bag, the tin foil insulation bag containing the tempered glass with the cemented carbide compact placed on the surface is wrapped with waterproof plastic, and then placed in a cold isostatic press for cold isostatic pressing. The present invention can improve the density and strength of the cemented carbide compact with a small thickness, maintain the flatness of the appearance, and improve the product quality and qualified rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0022] Figure 1 It is a schematic diagram of the structure of the tempered glass used in the present invention.
[0023] The realization of the effects, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0024] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The invention provides a method for cold isostatic pressing of a cemented carbide compact with a small thickness, which can improve the density and strength of the cemented carbide compact with a small thickness, maintain the flatness of the appearance, and improve the product quality and the qualified rate.
[0026] According to one aspect of the present invention, the present invention provides the following technical solution:
[0027] A method for cold isostatic pressing of a cemented carbide compact with a small thickness comprises the following steps:
[0028] S1. placing a cemented carbide compact with a small thickness on a tempered glass surface having through holes evenly arranged in the thickness direction;
[0029] S2. Put the tempered glass with the hard alloy compact placed on the surface into a tin foil insulation bag;
[0030] S3, wrap the tin foil insulation bag containing the tempered glass with the hard alloy pressed blank placed on the surface with waterproof plastic;
[0031] S4, then put it into a cold isostatic press for cold isostatic pressing.
[0032] The present invention places the thin cemented carbide compact on the surface of the tempered glass having evenly arranged through holes in the thickness direction, and the good strength and toughness of the tempered glass can protect the thin cemented carbide compact. Preferably, in step S1, the thickness of the cemented carbide compact is ≤10 mm.
[0033] Preferably, in step S1, the thickness of the tempered glass is 10-15 mm, the diameter of the through hole is 2-6 mm, the contact surface between the cemented carbide blank and the tempered glass should be the surface with the largest area, and the surface area of the tempered glass is larger than the area of any surface of the cemented carbide blank. The diameter of the through hole on the tempered glass should not be too large, and the diameter range is 2-6 mm. The area of the through hole is small and evenly arranged, which can disperse the pressure more evenly, so that the pressure impact of the cemented carbide blank with a small thickness during the cold isostatic pressing process is reduced, and no cracking and deformation will occur. The indentation on the contact surface with the tempered glass is also slight, and it can be processed flat in the subsequent semi-processing of the blank, and the processing time is also short.
[0034] Preferably, in step S2, the surface layer of the tinfoil insulation bag is a layer of waterproof aluminum film, and there is a layer of pearl cotton inside; the tinfoil insulation bag needs to be completely loaded with the tempered glass with the hard alloy compact placed on the surface, so that it is completely fitted with the tinfoil insulation bag. The tinfoil insulation bag used in the present invention is composed of the waterproof aluminum film on the surface and the thickened pearl cotton in the inner layer. The waterproof aluminum film on the surface can play a waterproof role, protecting the hard alloy compact from liquid penetration, and the thickened pearl cotton in the inner layer can play a buffering role, and once again reduce the pressure shock of the hard alloy compact with a small thickness during the cold isostatic pressing process. The tinfoil insulation bag is completely fitted so that the whole body will not cause creases under high pressure when subjected to cold isostatic pressing, affecting the appearance of the hard alloy compact.
[0035] Preferably, in step S3, when the waterproof plastic is wrapped, three layers are completely wrapped in the horizontal direction and the vertical direction, and the waterproof plastic needs to be completely attached to the tinfoil insulation bag during wrapping. The present invention adopts the method of wrapping the waterproof plastic to enhance the overall waterproof effect, wherein the toughness of the waterproof plastic can make it stretch and shrink during the wrapping process, and the wrapping is tighter. The tinfoil insulation bag containing the cemented carbide compact and the tempered glass can be completely tightly wrapped by wrapping three layers in the horizontal direction and the vertical direction, which can completely protect it from being penetrated by liquids, and can also ensure that the surface is flat, and will not be creased under high pressure, affecting the appearance of the cemented carbide compact.
[0036] The technical solution of the present invention is further described below in conjunction with specific embodiments.
[0037] Example 1
[0038] A method for cold isostatic pressing of a cemented carbide compact with a small thickness comprises the following steps:
[0039] S1. Place the bottom surface of a 150 mm long, 150 mm wide, 10 mm thick cemented carbide compact with a length of 150 mm, a width of 150 mm, on the surface of a tempered glass in the middle of a 200 mm long, 200 mm wide surface with evenly arranged through holes in the thickness direction; the thickness of the tempered glass is 15 mm, and the diameter of the through holes is 4 mm;
[0040] S2. Put the tempered glass with the hard alloy pressed blank on the surface into a tinfoil insulation bag; the surface of the tinfoil insulation bag is a waterproof aluminum film, and there is a layer of pearl cotton inside. The tinfoil insulation bag needs to be completely filled with the tempered glass with the hard alloy pressed blank on the surface, so that it is completely fitted with the tinfoil insulation bag;
[0041] S3. Wrap the tinfoil insulation bag containing the tempered glass with the hard alloy pressed blank on the surface with waterproof plastic; when wrapping with waterproof plastic, completely wrap 3 layers in the horizontal direction and 3 layers in the vertical direction, and the waterproof plastic needs to completely fit the tinfoil insulation bag during wrapping;
[0042] S4, then put it into a cold isostatic press for cold isostatic pressing.
[0043] After cold isostatic pressing, the thickened waterproof plastic and tin foil insulation bag were removed, the cemented carbide compact was separated from the tempered glass, and the density and appearance of the cemented carbide compact were checked: the inspection found that the cemented carbide compact had no creases, no cracks and deformation, no liquid penetration, and the density and compactness of the compact were improved.
[0044] Example 2
[0045] A method for cold isostatic pressing of a cemented carbide compact with a small thickness comprises the following steps:
[0046] S1. Place the bottom surface of a columnar cemented carbide compact with a diameter of 100 mm and a thickness of 10 mm on the surface of a tempered glass in the middle of a surface with a length of 120 mm and a width of 120 mm and through holes evenly arranged in the thickness direction; the thickness of the tempered glass is 10 mm, and the diameter of the through holes is 4 mm;
[0047] S2. Put the tempered glass with the hard alloy pressed blank on the surface into a tinfoil insulation bag; the surface of the tinfoil insulation bag is a waterproof aluminum film, and there is a layer of pearl cotton inside. The tinfoil insulation bag needs to be completely filled with the tempered glass with the hard alloy pressed blank on the surface, so that it is completely fitted with the tinfoil insulation bag;
[0048] S3. Wrap the tinfoil insulation bag containing the tempered glass with the hard alloy pressed blank on the surface with waterproof plastic; when wrapping with waterproof plastic, completely wrap 3 layers in the horizontal direction and 3 layers in the vertical direction, and the waterproof plastic needs to completely fit the tinfoil insulation bag during wrapping;
[0049] S4, then put it into a cold isostatic press for cold isostatic pressing.
[0050] After cold isostatic pressing, the thickened waterproof plastic and tin foil insulation bag were removed, the cemented carbide compact was separated from the tempered glass, and the density and appearance of the cemented carbide compact were checked: the inspection found that the cemented carbide compact had no creases, no cracks and deformation, no liquid penetration, and the density and compactness of the compact were improved.
[0051] Comparative Example 1
[0052] The difference from Example 1 is that the cemented carbide compact is placed in a cold isostatic pressing rubber mold for cold isostatic pressing.
[0053] After cold isostatic pressing, the cemented carbide compact is taken out from the rubber mold and the density and appearance of the cemented carbide compact are checked: the inspection found that the cemented carbide compact has been broken and cracked under high pressure. This compact is unqualified and cannot be transferred to the next process.
[0054] Comparative Example 2
[0055] The difference from Example 1 is that in step S2, the tin foil insulation bag does not completely fit the cemented carbide compact and the tempered glass.
[0056] After cold isostatic pressing, the thickened waterproof plastic and tin foil insulation bag were removed, the cemented carbide blank was separated from the tempered glass, and the density and appearance of the cemented carbide blank were checked: the inspection found that there were creases on the appearance of the cemented carbide blank, no cracks and deformation, no liquid penetration, the density and compactness of the blank were improved, and there were defects in the appearance.
[0057] Comparative Example 3
[0058] The difference from Example 1 is that in step S2, the tempered glass with the cemented carbide blank placed on the surface is placed in an EPP bag, the EPP bag is a layer of thickened EPP, the EPP bag just completely fills the cemented carbide blank and the tempered glass, and the EPP bag completely fits the cemented carbide blank and the tempered glass; and step S3 is not performed.
[0059] After cold isostatic pressing, the pearl cotton bag is removed, the cemented carbide blank is separated from the tempered glass, and the density and appearance of the cemented carbide blank are checked: the inspection found that there were creases on the appearance of the cemented carbide blank, no cracks or deformation occurred, the blank was penetrated by liquid, and the density and compactness of the blank were improved. This blank was unqualified, it was easy to crack during the sintering process, and it could not be transferred to the next process.
[0060] Comparative Example 4
[0061] The difference from Example 1 is that no tempered glass is used, and the hard alloy compact with a length of 150 mm, a width of 150 mm, and a thickness of 10 mm is directly placed in a tin foil insulation bag.
[0062] After cold isostatic pressing, the thickened waterproof plastic and tin foil insulation bag were removed, the cemented carbide blank was separated from the tempered glass, and the density and appearance of the cemented carbide blank were checked: the inspection found that the four corners of the cemented carbide blank were severely damaged and were unqualified products.
[0063] Comparative Example 5
[0064] The difference from Example 1 is that the tempered glass has no through hole.
[0065] After cold isostatic pressing, remove the thickened waterproof plastic and tin foil insulation bag, separate the cemented carbide compact from the tempered glass, and check the density and appearance of the cemented carbide compact: the cemented carbide compact and the tempered glass have been broken, the tempered glass cannot be used, and the compact is a defective product.
[0066] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for cold isostatic pressing of a cemented carbide compact with a small thickness, characterized in that: The steps include: S1. placing a cemented carbide compact with a small thickness on a tempered glass surface having through holes evenly arranged in the thickness direction; S2. Put the tempered glass with the hard alloy compact placed on the surface into a tin foil insulation bag; S3, wrap the tin foil insulation bag containing the tempered glass with the hard alloy pressed blank placed on the surface with waterproof plastic; S4, then put it into a cold isostatic press for cold isostatic pressing.
2. The method for cold isostatic pressing of a cemented carbide blank with a small thickness according to claim 1, characterized in that: In the step S1, the thickness of the cemented carbide compact is ≤10 mm.
3. The method for cold isostatic pressing of a cemented carbide blank with a small thickness according to claim 1, characterized in that: In the step S1, the thickness of the tempered glass is 10-15 mm.
4. The method for cold isostatic pressing of a cemented carbide blank with a small thickness according to claim 1, characterized in that: In the step S1, the diameter of the through hole is 2-6 mm.
5. The method for cold isostatic pressing of a cemented carbide blank with a small thickness according to claim 1, characterized in that: In the step S1, the contact surface between the cemented carbide compact and the tempered glass should be the surface with the largest area.
6. The method for cold isostatic pressing of a cemented carbide compact with a small thickness according to claim 1, characterized in that: In the step S1, the surface area of the tempered glass is larger than the area of any surface of the cemented carbide compact.
7. The method for cold isostatic pressing of a cemented carbide compact with a small thickness according to claim 1, characterized in that: In step S2, the surface layer of the tinfoil insulation bag is a layer of waterproof aluminum film, and there is a layer of pearl cotton inside.
8. The method for cold isostatic pressing of a cemented carbide compact with a small thickness according to claim 1, characterized in that: In step S2, the tinfoil insulation bag needs to be completely filled with the tempered glass with the hard alloy pressed blank placed on the surface, so that it is completely fitted with the tinfoil insulation bag.
9. The method for cold isostatic pressing of a cemented carbide blank with a small thickness according to claim 1, characterized in that: In step S3, when the waterproof plastic is wrapped, three layers are completely wrapped in the horizontal direction and the vertical direction respectively, and the waterproof plastic needs to completely fit the tin foil insulation bag during wrapping.