Tungsten-silicon alloy powder and preparation method thereof

Through batch mixing and multiple calcining treatment combined with ball milling steps, tungsten silicon alloy powder with uniform particle size and excellent performance was prepared, solving the problems of uneven particle size of tungsten silicon alloy powder and waste of raw materials in powder metallurgy, achieving low cost It also has excellent performance and is suitable for vacuum sputtering targets in the semiconductor industry.

CN119035557APending Publication Date: 2024-11-29KONFOONG MATERIALS INTERNATIONAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411177396.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the field of powder metallurgy, how to effectively prepare tungsten silicon alloy powder with high density and uniform particle size, reduce raw material waste and improve product performance, especially in the semiconductor industry, the performance requirements are high when used in vacuum sputtering targets.

Method used

By adding tungsten powder and silicon powder in batches for mixing, and performing multiple step calcining treatments under an oxygen-free environment, combined with the ball milling step, the particle size distribution of tungsten silicon alloy powder is controlled to achieve uniform particle size and performance optimization.

Benefits of technology

The particle size uniformity and tungsten silicon alloy powder are achieved and the uniformity of tungsten silicon ratio are reduced, raw material consumption and production costs are reduced, and the use requirements of tungsten silicon alloy targets are met, and there are excellent industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119035557A_ABST
    Figure CN119035557A_ABST
Patent Text Reader

Abstract

The invention provides tungsten-silicon alloy powder and a preparation method thereof, and the preparation method comprises the following steps: (1) adding silicon powder into tungsten powder in at least three batches so as to mix the tungsten powder and the silicon powder, and calcining to obtain a tungsten-silicon alloy; and (2) carrying out ball milling on the tungsten-silicon alloy obtained in the step (1) to obtain the tungsten-silicon alloy powder. According to the tungsten-silicon alloy powder and the preparation method thereof, uniform distribution of tungsten and silicon elements can be achieved, the obtained tungsten-silicon alloy powder is uniform in particle size, the use requirement for preparing a tungsten-silicon alloy target material is met, and the tungsten-silicon alloy powder and the preparation method thereof have excellent industrial application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of powder metallurgy and relates to a tungsten-silicon alloy, and in particular to a tungsten-silicon alloy powder and a preparation method thereof. Background Art

[0002] The semiconductor industry is the core industry of the information age. With the development of the semiconductor industry, integrated circuits, as the main products of the semiconductor industry, are gradually becoming more multifunctional and refined. Sputtered thin films are one of the important components of semiconductor components and are generally obtained by sputtering targets. Tungsten silicon alloy target is a new type of alloy target. As a good conductor for vacuum sputtering, it can be used in the field of electronic gate materials and electronic thin films. Tungsten silicon thin films have the characteristics of high electrical conductivity, good thermal stability and excellent chemical corrosion resistance, and are widely used in the field of integrated circuits.

[0003] In order to make the tungsten silicon alloy target material play a good role in vacuum sputtering, it is generally required that the tungsten silicon target material has a high density, no internal defects, and the internal free silicon is small and evenly distributed. Therefore, it is necessary to improve the performance of the target material from the raw material.

[0004] Alloy powder is the main raw material for preparing target materials. In the field of powder metallurgy, the powder particle size seriously affects the various properties of powder metallurgy products. How to obtain alloy powder with uniform particle size has always been a difficult problem in the field of powder metallurgy. In addition, W and Si can react to obtain tungsten silicon alloy, but the melting points of Si and W are quite different. Preparation through smelting will lead to a large amount of volatilization of silicon and cause waste of raw materials. How to prepare tungsten silicon alloy more efficiently is also particularly important.

[0005] Using alloy powder to prepare corresponding alloy blocks can greatly improve the quality and performance of products, increase the degree of alloying of products, and improve the hardness and wear resistance of materials, thereby extending their service life and reliability. In addition, alloy powder can also reduce the difficulty of product preparation, reduce the consumption and waste of raw materials, and reduce production costs.

[0006] Therefore, it is necessary to provide a preparation method that can regulate the quality and performance of alloy powders. Summary of the invention

[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing tungsten silicon alloy powder. The preparation method provided by the present invention has low cost and can effectively control the particle size of the alloy powder, thereby reducing the consumption and waste of raw materials and achieving the effect of reducing costs and increasing efficiency.

[0008] To achieve this object, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing tungsten silicon alloy powder, the preparation method comprising the following steps:

[0010] (1) adding silicon powder to tungsten powder in at least three batches to mix the tungsten powder and silicon powder, and then calcining the mixture to obtain a tungsten-silicon alloy;

[0011] (2) ball milling the tungsten silicon alloy obtained in step (1) to obtain the tungsten silicon alloy powder.

[0012] In the present invention, silicon powder is added in at least three batches to mix tungsten powder and silicon powder, so that uniform mixing of silicon powder and tungsten powder can be achieved in the mixing stage, and then a reasonable staged calcination treatment process route is designed through the binary alloy phase diagram of tungsten and silicon to obtain a tungsten-silicon alloy with a good looseness, and then combined with ball milling, the tungsten-silicon alloy powder is uniformly controllable, which can well meet the requirements of different products on powder particle size, thereby obtaining an alloy with excellent performance; and the preparation method provided by the present invention is low in cost and has excellent industrial application prospects.

[0013] As a preferred technical solution of the present invention, the mass ratio of tungsten powder to silicon powder in step (1) is 1:2-5, for example, it can be 1:2, 1:2.2, 1:2.3, 1:2.4, 1:2.5, 1:2.6, 1:2.8, 1:2.9, 1:3.0, 1:3.1, 1:3.2, 1:3.5, 1:3.8, 1:4.0, 1:4.2, 1:4.5, 1:4.8 or 1:5, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0014] As a preferred technical solution of the present invention, the mixing in step (1) is carried out using a V-type powder mixer.

[0015] Preferably, in the first batch of the at least three batches in step (1), the silicon powder accounts for 10-20% of the total silicon powder, for example, it can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19% or 20%, etc.; the silicon powder in the second batch accounts for 30-50% of the total silicon powder, for example, it can be 30%, 32%, 33%, 34%, 35%, 38%, 40%, 42%, 45%, 48% or 50%, etc.; the silicon powder in the third batch accounts for 10-50% of the total silicon powder, for example, it can be 10%, 12%, 15%, 18%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc.

[0016] The present invention preferably adopts the above-mentioned method to add in batches, which can better improve the powder mixing uniformity between tungsten powder and silicon powder.

[0017] Preferably, the interval time between any two batches is 0.5 to 1.5 h, for example, it can be 0.5 h, 0.6 h, 0.7 h, 0.8 h, 1.0 h, 1.2 h, 1.3 h or 1.5 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] Preferably, the mixing time in step (1) is 12 to 24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] The present invention achieves complete mixing of tungsten powder and silicon powder by a V-shaped powder mixer, but the mixing time should not be too long to avoid agglomeration of silicon powder.

[0020] As a preferred technical solution of the present invention, the particle size range of the tungsten powder in step (1) is ≤80 μm, for example, it can be 80 μm, 70 μm, 60 μm, 50 μm, 40 μm, 30 μm or 20 μm, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; preferably 50 to 60 μm.

[0021] Preferably, the particle size range of the silicon powder in step (1) is ≤100 μm, for example, it can be 100 μm, 90 μm, 80 μm, 70 μm, 60 μm, 50 μm, 40 μm, 30 μm or 20 μm, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; preferably, it is 60 to 80 μm.

[0022] As a preferred technical solution of the present invention, the calcination treatment in step (1) is carried out in an oxygen-free environment.

[0023] Preferably, the oxygen-free environment includes a nitrogen gas environment and / or an inert gas environment.

[0024] As a preferred technical solution of the present invention, the heating rate of the primary calcination is 8 to 10°C / min, for example, it can be 8°C / min, 8.4°C / min, 8.8°C / min, 9.2°C / min, 9.6°C / min or 10°C / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] Preferably, the calcination temperature of the primary calcination is 900-1100°C, for example, 900°C, 950°C, 1000°C, 1050°C or 1100°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0026] Preferably, the holding time of the primary calcination is 50 to 70 min, for example, 50 min, 54 min, 58 min, 62 min, 66 min or 70 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0027] Preferably, the heating rate of the secondary calcination is 3 to 5°C / min, for example, 3°C / min, 3.4°C / min, 3.8°C / min, 4.2°C / min, 4.6°C / min or 5°C / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0028] Preferably, the calcination temperature of the secondary calcination is 1200-1280°C, for example, 1200°C, 1220°C, 1240°C, 1260°C or 1280°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, the holding time of the secondary calcination is 20 to 40 min, for example, 20 min, 24 min, 28 min, 32 min, 36 min or 40 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0030] Preferably, the heating rate of the three calcinations is 3 to 5°C / min, for example, 3°C / min, 3.4°C / min, 3.8°C / min, 4.2°C / min, 4.6°C / min or 5°C / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0031] Preferably, the calcination temperature of the three calcinations is 1320-1380°C, for example, 1320°C, 1340°C, 1360°C or 1380°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] Preferably, the holding time for the three calcinations is 5.5 to 6.5 h, for example, 5.5 h, 5.7 h, 5.9 h, 6.1 h, 6.3 h or 6.5 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0033] In the present invention, the temperature and holding time of the three calcinations need to be controlled within the above range, which can better match the binary alloy phase diagram between tungsten silicon powders, thereby obtaining a tungsten silicon alloy with moderate looseness, laying the foundation for subsequent ball milling to obtain tungsten silicon alloy powder with controllable particle size.

[0034] Preferably, the calcination process further includes a cooling process.

[0035] Preferably, the terminal temperature of the cooling treatment is 350-400°C, for example, 350°C, 360°C, 370°C, 380°C, 390°C or 400°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0036] The calcination treatment of the present invention is carried out in a high-temperature muffle furnace, and a tungsten silicon alloy with a good looseness is prepared by three consecutive step-wise calcination treatments.

[0037] As a preferred technical solution of the present invention, the ball milling in step (2) includes primary ball milling and secondary ball milling performed sequentially.

[0038] The present invention achieves crushing and grinding of the tungsten silicon alloy obtained in step (1) by ball milling to obtain alloy powder, thereby achieving uniform and controllable particle size of the alloy powder.

[0039] Preferably, the rotation speed of the primary ball milling is 100-150 r / min greater than that of the secondary ball milling, for example, it can be 100 r / min, 110 r / min, 120 r / min, 130 r / min, 140 r / min or 150 r / min, and the time of the primary ball milling is 1-1.5 h shorter than that of the secondary ball milling, for example, it can be 1 h, 1.1 h, 1.2 h, 1.3 h, 1.4 h or 1.5 h, etc.

[0040] As a preferred technical solution of the present invention, the rotation speed of the primary ball mill is 200-260r / min, for example, it can be 200r / min, 210r / min, 220r / min, 230r / min, 240r / min, 250r / min or 260r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0041] Preferably, the time of the first ball milling is 50 to 70 min, for example, 501 min, 54 min, 58 min, 62 min, 66 min or 70 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0042] Preferably, the rotation speed of the secondary ball milling is 100-120 r / min, for example, it can be 100 r / min, 104 r / min, 108 r / min, 112 r / min, 116 r / min or 120 r / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0043] Preferably, the secondary ball milling time is 2 to 3 hours, for example, 2 hours, 2.2 hours, 2.4 hours, 2.6 hours, 2.8 hours or 3 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0044] Preferably, the mass ratio of the grinding balls used in the ball milling in step (2) to the tungsten silicon alloy in step (1) is 3 to 5:1, for example, 3:1, 3.2:1, 3.4:1, 3.6:1, 3.8:1, 4:1, 4.2:1, 4.4:1, 4.6:1, 4.8:1 or 5:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable, preferably 4:1.

[0045] The ball-to-material ratio in the ball mill of the present invention is 3-5:1, which is more conducive to obtaining tungsten silicon powder with uniform particle size.

[0046] Preferably, the grinding balls used in the ball milling in step (2) include zirconia balls.

[0047] As a preferred technical solution of the present invention, the method for preparing tungsten silicon alloy powder provided by the present invention comprises the following steps:

[0048] (1) In a V-type powder mixer, tungsten powder with a particle size of ≤80 μm is first added, and then silicon powder with a particle size of ≤100 μm is added to the tungsten powder in at least three batches to mix the tungsten powder and the silicon powder, wherein the silicon powder in the first batch of at least three batches accounts for 10-20% of the total silicon powder, the silicon powder in the second batch accounts for 30-50% of the total silicon powder, and the silicon powder in the third batch accounts for 10-50% of the total silicon powder, the interval time between any two batches is 0.5-1.5 hours, and the total mixing time is 12-24 hours, and then calcination is performed in an oxygen-free environment to obtain a tungsten silicon alloy;

[0049] The calcination treatment includes a primary calcination, a secondary calcination and a tertiary calcination performed in sequence; the heating rate of the primary calcination is 8-10°C / min, the calcination temperature is 900-1100°C, and the holding time is 50-70min; the heating rate of the secondary calcination is 3-5°C / min, the calcination temperature is 1200-1280°C, and the holding time is 20-40min; the heating rate of the tertiary calcination is 3-5°C / min, the calcination temperature is 1320-1380°C, and the holding time is 5.5-6.5h;

[0050] (2) mixing the grinding balls and the tungsten silicon alloy obtained in step (1) in a mass ratio of 3 to 5:1, and performing primary ball milling and secondary ball milling in sequence to obtain the tungsten silicon alloy powder;

[0051] The rotation speed of the first ball mill is 100-150r / min greater than that of the second ball mill, and the time of the first ball mill is 1-1.5h shorter than that of the second ball mill; the rotation speed of the first ball mill is 200-260r / min, and the time is 50-70min; the rotation speed of the second ball mill is 100-120r / min, and the time is 2-3h.

[0052] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0053] In a second aspect, the present invention provides a tungsten-silicon alloy powder, wherein the tungsten-silicon alloy powder is prepared by the preparation method of the tungsten-silicon alloy powder described in the first aspect.

[0054] Compared with the prior art, the present invention has the following beneficial effects:

[0055] (1) The tungsten-silicon alloy powder obtained by the method for preparing the tungsten-silicon alloy powder provided by the present invention has a uniform ratio of tungsten and silicon, a uniform particle size, and a narrow particle size distribution, which meets the use requirements for preparing tungsten-silicon alloy targets;

[0056] (2) The preparation method of the tungsten silicon alloy powder provided by the present invention has a simple process, low cost, and excellent industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 is a particle size distribution diagram of the tungsten silicon alloy powder obtained in step (2) of Example 1 of the present invention;

[0058] Figure 2 This is a microscopic enlarged image of the tungsten silicon alloy powder obtained in step (2) of Example 1 of the present invention. DETAILED DESCRIPTION

[0059] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0060] Example 1

[0061] This embodiment provides a method for preparing tungsten-silicon alloy powder, the preparation method comprising the following steps:

[0062] (1) Tungsten powder with a particle size of 60 μm and silicon powder with a particle size of 80 μm are mixed in a V-type powder mixer at a mass ratio of 1:3. The specific mixing process is as follows:

[0063] In a V-type powder mixer, first add tungsten powder, then add 20wt% silicon powder and mix at 700r / min for 1.5h, then add 50wt% silicon powder and mix at 500r / min for 1h, then add the remaining 30wt% silicon powder and mix at 400r / min for 12h;

[0064] Then, calcination treatment is performed in an oxygen-free environment to obtain a tungsten-silicon alloy;

[0065] The calcination treatment includes a primary calcination, a secondary calcination, a tertiary calcination and a cooling treatment performed in sequence; the heating rate of the primary calcination is 9°C / min, the calcination temperature is 1050°C, and the holding time is 60min; the heating rate of the secondary calcination is 4°C / min, the calcination temperature is 1250°C, and the holding time is 30min; the heating rate of the tertiary calcination is 4°C / min, the calcination temperature is 1360°C, and the holding time is 6.0h;

[0066] (2) mixing the grinding balls and the tungsten silicon alloy obtained in step (1) in a mass ratio of 4:1 and performing primary ball milling and secondary ball milling in sequence to obtain the tungsten silicon alloy powder;

[0067] The rotation speed of the first ball milling is 230 r / min, and the time is 70 min; the rotation speed of the second ball milling is 110 r / min, and the time is 2 h.

[0068] The particle size distribution diagram of the tungsten silicon alloy powder obtained in step (2) of this embodiment is as follows: Figure 1 As shown, the microscopic enlarged image of the tungsten silicon alloy powder obtained in step (2) is as follows Figure 2 As shown, from Figures 1-2 It can be seen that the particle size distribution of the tungsten silicon alloy powder prepared in this embodiment is uniform, and the particle size range is within the range of 0.3 to 20 μm, and there is no large particle size exceeding 20 μm.

[0069] Example 2

[0070] This embodiment provides a method for preparing tungsten-silicon alloy powder, the preparation method comprising the following steps:

[0071] (1) Tungsten powder with a particle size of 60 μm and silicon powder with a particle size of 60 μm are mixed in a V-type powder mixer at a mass ratio of 1:15. The specific mixing process is as follows:

[0072] In a V-type powder mixer, first add tungsten powder, then add 10wt% silicon powder and mix at 800r / min for 1.5h, then add 40wt% silicon powder and mix at 600r / min for 1h, then add the remaining 30wt% silicon powder and mix at 450r / min for 1h, then add the remaining 20wt% silicon powder and mix at 300r / min for 18h;

[0073] Then, calcination treatment is performed in an oxygen-free environment to obtain a tungsten-silicon alloy;

[0074] The calcination treatment includes a primary calcination, a secondary calcination, a tertiary calcination and a cooling treatment performed in sequence; the heating rate of the primary calcination is 10°C / min, the calcination temperature is 900°C, and the holding time is 70min; the heating rate of the secondary calcination is 5°C / min, the calcination temperature is 1280°C, and the holding time is 20min; the heating rate of the tertiary calcination is 3°C / min, the calcination temperature is 1325°C, and the holding time is 6.5h;

[0075] (2) mixing the grinding balls and the tungsten silicon alloy obtained in step (1) in a mass ratio of 5:1 and performing primary ball milling and secondary ball milling in sequence to obtain the tungsten silicon alloy powder;

[0076] The rotation speed of the first ball milling is 260 r / min, and the time is 70 min; the rotation speed of the second ball milling is 110 r / min, and the time is 2.5 h.

[0077] Example 3

[0078] This embodiment provides a method for preparing tungsten-silicon alloy powder, the preparation method comprising the following steps:

[0079] (1) Tungsten powder with a particle size of 50 μm and silicon powder with a particle size of 80 μm are mixed in a V-type powder mixer at a mass ratio of 1:30. The specific mixing process is as follows:

[0080] In a V-type powder mixer, first add tungsten powder, then add 20wt% of tungsten powder and mix at 700r / min for 1.5h, then add 30wt% of silicon powder and mix at 550r / min for 1.5h, then add the remaining 50wt% of silicon powder and mix at 400r / min for 14h;

[0081] Then, calcination treatment is performed in an oxygen-free environment to obtain a tungsten-silicon alloy;

[0082] The calcination treatment includes a primary calcination, a secondary calcination, a tertiary calcination and a cooling treatment performed in sequence; the heating rate of the primary calcination is 9°C / min, the calcination temperature is 1100°C, and the holding time is 50min; the heating rate of the secondary calcination is 4.5°C / min, the calcination temperature is 1280°C, and the holding time is 25min; the heating rate of the tertiary calcination is 4°C / min, the calcination temperature is 1360°C, and the holding time is 5.5h;

[0083] (2) mixing the grinding balls and the tungsten silicon alloy obtained in step (1) in a mass ratio of 3:1 and performing primary ball milling and secondary ball milling in sequence to obtain the tungsten silicon alloy powder;

[0084] The rotation speed of the first ball milling is 220 r / min, and the time is 50 min; the rotation speed of the second ball milling is 120 r / min, and the time is 2.2 h.

[0085] Example 4

[0086] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0087] In this embodiment, the proportions of tungsten silicon powder in the three batches of step (1) are adjusted to 30wt%, 50wt% and 20wt%.

[0088] Example 5

[0089] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0090] In this embodiment, the proportions of silicon powder in the three batches in step (1) are adjusted to 5wt%, 50wt% and 45wt%.

[0091] Example 6

[0092] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0093] In this embodiment, step (1) is modified as follows: first add tungsten powder, then add 20wt% of silicon powder and mix at 700r / min for 0.3h, then add 50wt% of silicon powder and mix at 500r / min for 1h, and then add the remaining 30wt% of silicon powder and mix at 400r / min for 13.2h.

[0094] Example 7

[0095] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0096] In this embodiment, step (1) is modified as follows: first add tungsten powder, then add 20wt% of silicon powder and mix at 700r / min for 1.5h, then add 50wt% of silicon powder and mix at 500r / min for 2h, and then add the remaining 30wt% of silicon powder and mix at 400r / min for 11h.

[0097] Example 8

[0098] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0099] In this embodiment, the first calcination, second calcination, and third calcination in step (1) are adjusted to a single calcination, and the process is a heating rate of 4°C / min, a calcination temperature of 1360°C, and a holding time of 7.5h.

[0100] Example 9

[0101] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0102] In this embodiment, the first calcination, second calcination, and third calcination in step (1) are adjusted to second calcination. The specific process is to first perform a first calcination with a heating rate of 4°C / min, a calcination temperature of 1250°C, and a holding time of 90 min; and then perform a second calcination with a heating rate of 4°C / min, a calcination temperature of 1360°C, and a holding time of 6.0 h.

[0103] Example 10

[0104] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0105] In this embodiment, the rotation speed of the first ball milling in step (2) is 300 r / min.

[0106] Embodiment 11

[0107] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0108] In this embodiment, the rotation speed of the first ball milling in step (2) is 180 r / min.

[0109] Example 12

[0110] This embodiment provides a method for preparing tungsten-silicon alloy powder, which differs from the preparation method in Embodiment 1 only in that:

[0111] In this embodiment, the rotation speed of the ball mill in step (2) is adjusted to 110 r / min, and the overall time is 2 h 70 min.

[0112] Comparative Example 1

[0113] This comparative example provides a method for preparing tungsten silicon alloy powder, which differs from Example 1 only in that:

[0114] In this comparative example, silicon powder was added to tungsten powder in two batches (50% each time).

[0115] Comparative Example 2

[0116] This comparative example provides a method for preparing tungsten silicon alloy powder, which differs from Example 1 only in that:

[0117] In this comparative example, all tungsten powder and silicon powder were directly mixed.

[0118] Comparative Example 3

[0119] This comparative example provides a method for preparing tungsten silicon alloy powder, which differs from Example 1 only in that:

[0120] In this comparative example, tungsten powder was added to silicon powder in three batches, and the amount distributed in the batches was the same as that in Example 1.

[0121] The particle size distribution test is used to measure the particle size range and particle size distribution of the tungsten silicon alloy powder, and the uniformity of the particle size distribution is judged based on the particle size distribution. When the difference between the minimum particle size and the maximum particle size exceeds 30μm, the particle size distribution is considered to be uneven. Five random samples are taken from the same batch of samples to detect the tungsten content. When the difference between the maximum and minimum tungsten contents in the five samples exceeds 10%, it is considered to be uneven. When the difference between the maximum and minimum tungsten contents is between 1% and 10% (excluding 10%), it is considered to be relatively uniform. When the difference between the maximum and minimum tungsten contents is within 1% (excluding 1%), the tungsten silicon component is considered to be uniform.

[0122] The test results of the tungsten-silicon alloy powder obtained by the preparation methods provided in the above embodiments and comparative examples are shown in Table 1.

[0123] Table 1

[0124]

[0125]

[0126] According to Table 1, we can know the following points:

[0127] (1) It can be seen from Examples 1 to 3 that the tungsten-silicon alloy powder prepared by the method for preparing the tungsten-silicon alloy powder provided by the present invention has a uniform ratio of tungsten to silicon, a uniform particle size, and a narrow particle size distribution, wherein the particle size distribution range is within 20 μm, and the maximum and minimum values ​​of the tungsten content in the tungsten-silicon component distribution differ by less than 1%, the tungsten-silicon component is uniform, and the application prospect is broad;

[0128] (2) It can be seen from Example 1, Examples 4 to 5, and Comparative Examples 1 to 3 that the uniformity of the components in the tungsten silicon alloy powder can be significantly improved by adding in batches and strictly controlling the proportion of silicon powder added in a single time;

[0129] (3) It can be seen from Example 1 and Examples 6 to 7 that when the time of the first mixing or the second mixing is too short, the particle size and component distribution uniformity of the final tungsten silicon powder will decrease. This shows that the present invention can better improve the particle size and component distribution uniformity of the tungsten silicon alloy powder by preferably controlling the mixing time in the batch mixing process within a reasonable range; By comparing Example 1 and Examples 10 to 12, it can be seen that the rotation speed of the ball mill has a great influence on the uniformity of the particle size distribution and component distribution of the tungsten silicon alloy;

[0130] (4) It can be seen from the combination of Example 1 and Examples 8 to 9 that only one calcination or two calcinations are performed in Examples 8 to 9, and high-temperature calcination is directly used, resulting in insufficient time for the tungsten silicon components to penetrate each other during the process of forming the alloy, which ultimately leads to a decrease in the uniformity of the components. This shows that the present invention preferably adopts the step of three calcinations to better improve the uniformity of the tungsten silicon alloy components.

[0131] In summary, the tungsten-silicon alloy powder preparation method provided by the present invention has uniform particle size, which meets the requirements for preparing tungsten-silicon alloy targets; and the preparation method has a simple process, low cost, and excellent industrial application prospects.

[0132] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing tungsten silicon alloy powder, characterized in that: The preparation method comprises the following steps: (1) adding silicon powder to tungsten powder in at least three batches to mix the tungsten powder and silicon powder, and then calcining the mixture to obtain a tungsten-silicon alloy; (2) ball milling the tungsten silicon alloy obtained in step (1) to obtain the tungsten silicon alloy powder.

2. The preparation method according to claim 1, characterized in that: The mass ratio of tungsten powder to silicon powder in step (1) is 1:2-5.

3. The preparation method according to claim 1 or 2, characterized in that: The mixing in step (1) is carried out using a V-shaped powder mixer; Preferably, in the at least three batches in step (1), the silicon powder in the first batch accounts for 10-20% of the total silicon powder, the silicon powder in the second batch accounts for 30-50% of the total silicon powder, and the silicon powder in the third batch accounts for 10-50% of the total silicon powder; Preferably, the interval between any two batches is 0.5 to 1.5 h; Preferably, the total mixing time in step (1) is 12 to 24 hours.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The particle size of the tungsten powder in step (1) is ≤80 μm, preferably 50 to 60 μm; Preferably, the particle size of the silicon powder in step (1) is ≤100 μm, preferably 60 to 80 μm.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The calcination treatment in step (1) is carried out in an oxygen-free environment; Preferably, the oxygen-free environment includes a nitrogen gas environment and / or an inert gas environment.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The calcination treatment includes a primary calcination, a secondary calcination and a tertiary calcination performed sequentially; Preferably, the heating rate of the primary calcination is 8 to 10°C / min; Preferably, the calcination temperature of the primary calcination is 900-1100°C; Preferably, the holding time of the primary calcination is 50 to 70 minutes; Preferably, the heating rate of the secondary calcination is 3-5°C / min; Preferably, the calcination temperature of the secondary calcination is 1200-1280°C; Preferably, the holding time of the secondary calcination is 20 to 40 minutes; Preferably, the heating rate of the three calcinations is 3-5°C / min; Preferably, the calcination temperature of the three calcinations is 1320-1380°C; Preferably, the holding time for the three calcinations is 5.5 to 6.5 hours.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The ball milling in step (2) includes primary ball milling and secondary ball milling performed sequentially.

8. The preparation method according to claim 7, characterized in that: The speed of the first ball milling is 100-150 r / min greater than that of the second ball milling, and the time of the first ball milling is 1-1.5 h shorter than that of the second ball milling; Preferably, the rotation speed of the first ball milling is 200-260 r / min; Preferably, the time of the first ball milling is 50 to 70 minutes; Preferably, the rotation speed of the secondary ball milling is 100-120 r / min; Preferably, the secondary ball milling time is 2 to 3 hours; Preferably, the mass ratio of the grinding balls used in the ball milling in step (2) to the tungsten silicon alloy in step (1) is 3 to 5:1; Preferably, the grinding balls used in the ball milling in step (2) include zirconia balls.

9. The preparation method according to any one of claims 1 to 8, characterized in that: The preparation method comprises the following steps: (1) In a V-type powder mixer, tungsten powder with a particle size of ≤80 μm is first added, and then silicon powder with a particle size of ≤100 μm is added to the tungsten powder in at least three batches to mix the tungsten powder and the silicon powder, wherein the silicon powder in the first batch of at least three batches accounts for 10-20% of the total silicon powder, the silicon powder in the second batch accounts for 30-50% of the total silicon powder, and the silicon powder in the third batch accounts for 10-50% of the total silicon powder, the interval time between any two batches is 0.5-1.5 hours, and the total mixing time is 12-24 hours, and then calcination is performed in an oxygen-free environment to obtain a tungsten silicon alloy; The calcination treatment includes a primary calcination, a secondary calcination and a tertiary calcination performed in sequence; the heating rate of the primary calcination is 8-10°C / min, the calcination temperature is 900-1100°C, and the holding time is 50-70min; the heating rate of the secondary calcination is 3-5°C / min, the calcination temperature is 1200-1280°C, and the holding time is 20-40min; the heating rate of the tertiary calcination is 3-5°C / min, the calcination temperature is 1320-1380°C, and the holding time is 5.5-6.5h; (2) mixing the grinding balls and the tungsten silicon alloy obtained in step (1) in a mass ratio of 3 to 5:1, and performing primary ball milling and secondary ball milling in sequence to obtain the tungsten silicon alloy powder; The rotation speed of the first ball mill is 100-150r / min greater than that of the second ball mill, and the time of the first ball mill is 1-1.5h shorter than that of the second ball mill; the rotation speed of the first ball mill is 200-260r / min, and the time is 50-70min; the rotation speed of the second ball mill is 100-120r / min, and the time is 2-3h.

10. A tungsten silicon alloy powder, characterized in that: The tungsten-silicon alloy powder is prepared by the preparation method of the tungsten-silicon alloy powder according to any one of claims 1 to 9.