Process method for manufacturing resin sand lined composite pipe by taking nodular cast iron pipe as base material

By forming a resin sand-lined composite tube on the ductile iron pipe, the chemical corrosion resistance of the resin sand mixed layer and the mechanical properties of the ductile iron are solved, and the problems of insufficient corrosion resistance and internal pressure resistance of the existing pipes are achieved. Efficient water conservancy and drainage applications overcome the shortcomings of traditional pipes and improve production efficiency.

CN119036903APending Publication Date: 2024-11-29GUANGDONG XINXING DUCTILE IRON PIPES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411153529.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing ductile iron pipes have shortcomings in corrosion resistance, internal pressure resistance and service life in the fields of water conservancy and water supply, and reinforced concrete pipes and fiberglass pipes have defects, making it difficult to meet the needs of various applications.

Method used

Using ductile iron pipes as the base material, through centrifugal casting technology and lining technology, resin sand-lined composite pipes are formed, and chemical corrosion resistance, wear resistance and mechanical properties of ductile iron are used in combination with fiberglass pipes. With corrosion resistance and internal pressure resistance, a process method is designed.

Benefits of technology

It realizes that the resin sand-lined composite pipe has high compressive strength, anti-float, anti-corrosion, resistance to internal pressure and low water flow resistance. It is suitable for a variety of water conservancy and drainage scenarios, overcomes the shortcomings of traditional pipes and improves production efficiency. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119036903A_ABST
    Figure CN119036903A_ABST
Patent Text Reader

Abstract

The invention discloses a process method for manufacturing a resin sand lined composite pipe by taking a nodular cast iron pipe as a base material, which comprises the following steps: weighing sand, unsaturated polyester resin, a curing agent and an accelerant, firstly stirring the unsaturated polyester resin and the curing agent, adding the accelerant, stirring, then adding the sand, and stirring to obtain resin mortar; the resin mortar is sprayed to the inner wall of the centrifugal nodular cast iron pipe to be cured and formed, and the resin sand lining composite pipe has the advantages of high compressive strength and floating resistance of a reinforced concrete pipe by means of the excellent chemical corrosion resistance, abrasion resistance and seawater microorganism adhesion resistance of the resin sand mixing layer and the good mechanical performance of nodular cast iron. And the glass fiber reinforced plastic pipe has the characteristics of corrosion resistance, internal pressure resistance and small water flow resistance, can be used for gravity flow drainage, can also be used for water drainage and pollution discharge under pressure, and is particularly suitable for a sewage treatment pipe network. And the defects of a reinforced concrete pipe and a glass steel pipe are overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite pipe manufacturing, in particular to a process for manufacturing a resin sand lined composite pipe using a ductile iron pipe as a base material. Background Art

[0002] Ductile iron pipes are widely used in water conservancy, water supply, drainage and other fields. With the development of the pipe industry, fiberglass pipes made of polyester resin and glass fiber, formed by centrifugal casting and winding, and reinforced concrete pipes are also widely used. These pipes are used in different scenarios according to the characteristics of the materials. Fiberglass pipes have the characteristics of corrosion resistance, internal pressure resistance, and low water flow resistance, but fiberglass pipes have problems such as deformation, aging, and chemical corrosion after long-term use. Reinforced concrete pipes have the characteristics of high compressive strength, anti-floating, and good durability, but reinforced concrete pipes have problems such as cracking, heavy weight, many joints, and complex construction when in use. Therefore, it is necessary to improve the production of pipes to meet the needs of various application conditions. Summary of the invention

[0003] The purpose of the present invention is to provide a process for manufacturing a resin sand lined composite pipe with a ductile iron pipe as a base material, so as to solve the problems raised in the above background technology.

[0004] To achieve the above object, the present invention provides the following technical solution: a method for manufacturing a resin sand lined composite pipe with a ductile iron pipe as a base material, comprising the following steps:

[0005] S1, obtaining a centrifugal ductile iron pipe through a centrifugal casting process, and screening the centrifugal ductile iron pipe that has passed the water pressure test;

[0006] S2, weigh the sand, unsaturated polyester resin, Trigonox V388 curing agent and ZF-Ⅱ unsaturated resin curing accelerator of corresponding proportion, first stir the unsaturated polyester resin and Trigonox V388 curing agent for 1-2 minutes, then add ZF-Ⅱ unsaturated resin curing accelerator and stir for 2-4 minutes, then add the sand of corresponding proportion and stir, stir the resin mortar fully, and stir for 5-10 minutes;

[0007] S3, put the prepared resin mortar into a distribution vehicle for standby use. The distribution vehicle has a stirring function to delay the setting time of the resin mortar;

[0008] S4, plugging both ends of the socket of the centrifugal ductile iron pipe;

[0009] S5, start the material distribution vehicle to extend the material distribution rod into the centrifugal ductile iron pipe, and evenly distribute the resin mortar on the inner wall of the centrifugal ductile iron pipe;

[0010] S6, start the coating machine to perform centrifugal coating, first control the coating machine pipe to rotate at a low gear, so that the resin mortar is evenly attached to the inner wall of the centrifugal ductile iron pipe, and then rotate the pipe at a high gear. Under the action of centrifugal force, the resin mortar is compacted and degassed on the inner wall of the centrifugal ductile iron pipe, so that the resin mortar is centrifugally formed;

[0011] S7, keeping the centrifugal ductile iron pipe rotating at a constant speed, and heating the centrifugal ductile iron pipe to solidify the resin mortar on the inner wall of the centrifugal ductile iron pipe;

[0012] S8, shut down the coating machine, remove the socket plug of the centrifugal ductile iron pipe, and obtain the resin sand lined composite pipe

[0013] Further, in S7, the temperature of the centrifugal ductile iron pipe is heated to 25-100° C. for 0.1-2 hours, so that the resin mortar on the inner wall of the centrifugal ductile iron pipe is cured and formed to form a tubular lining in the centrifugal ductile iron pipe to protect the centrifugal ductile iron pipe.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] (1) The process design of resin sand lined composite pipe is to use synthetic resin as the lining matrix and lining sand as the reinforcing material to form a resin sand mixed layer, making full use of the excellent chemical corrosion resistance, wear resistance, resistance to seawater microbial adhesion of the resin sand mixed layer and the good mechanical properties of ductile iron. The resin sand lined composite pipe has the advantages of high compressive strength and anti-floating of reinforced concrete pipes, and also has the characteristics of anti-corrosion, resistance to internal pressure, and small water flow resistance of glass fiber reinforced plastic pipes. It can be used for gravity flow drainage, as well as pressure drainage and sewage discharge, and is especially suitable for sewage treatment pipe networks. It overcomes the shortcomings of reinforced concrete pipes and glass fiber reinforced plastic pipes.

[0016] (2) According to the different resin quality selection, it can be adapted to high-quality drinking water and heavily polluted sewage pipelines. Compared with the traditional heavy anti-corrosion coating, it can save the internal grinding process of the cast pipe and improve the production efficiency of the special coating cast pipe. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is a process flow chart of the present invention;

[0018] Figure 2 It is a cross-sectional view of the resin sand lined composite pipe of the present invention.

[0019] In the figure: 1. Ductile iron pipe reinforcement layer; 2. Resin sand lining layer; 3. Resin layer. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example:

[0022] See also Figure 1-2 The present invention provides a technical solution: a manufacturing process of a resin sand lined composite pipe with a ductile iron pipe as a substrate, comprising a resin sand lining layer, a resin layer is arranged at the innermost of the resin sand lining layer, a ductile iron pipe reinforcement layer is arranged outside the resin sand lining layer, and a zinc spraying anti-corrosion layer and an outer surface paint layer are arranged on the outer surface of the ductile iron pipe reinforcement layer, which can isolate the ductile iron pipe from contact with external media, reduce the corrosion rate, and thus extend the service life;

[0023] (1) Ductile iron pipe reinforcement layer

[0024] Using centrifugal ductile iron pipe as a reinforcement layer can well enhance the rigidity of the composite pipe after forming. The carbon content of centrifugal ductile iron pipe is 3.3-3.6%, the silicon content is 3.3-3.5%, the chromium content is less than or equal to 0.03%, and the manganese content is less than or equal to 0.3%. The content of other elements refers to the composition of conventional ductile iron pipe.

[0025] (2) Resin layer

[0026] The resin layer is formed by solidifying and forming a mixed glue liquid of resin and sand under centrifugal action. The specific raw material composition is: resin 80-99%, curing agent content is less than or equal to 20%, and accelerator content is less than or equal to 20%.

[0027] (3) Resin sand mixed layer

[0028] The resin sand mixed layer is formed by solidifying the mixed glue of resin and sand, and its specific composition is 50-80% sand, 15-50% unsaturated polyester resin, 0.1-2.0% Trigonox V388 curing agent, and 0.1-2.0% ZF-Ⅱ unsaturated resin curing accelerator.

[0029] Production process

[0030] The first step: obtain the centrifugal ductile iron pipe through the centrifugal casting process as the reinforcement layer and the main base layer, inject water into the centrifugal ductile iron pipe and seal it, conduct water pressure testing on the centrifugal ductile iron pipe, and screen out qualified centrifugal ductile iron pipes.

[0031] Step 2: Mix and prepare the resin mortar. Weigh the sand, unsaturated polyester resin, Trigonox V388 curing agent and ZF-Ⅱ unsaturated resin curing accelerator with corresponding proportions. First, stir the unsaturated polyester resin and Trigonox V388 curing agent for 1-2 minutes, then add ZF-Ⅱ unsaturated resin curing accelerator and stir for 2-4 minutes, then add the sand with corresponding proportion and stir. Stir the resin mortar thoroughly for 5-10 minutes.

[0032] Step 3: Put the prepared resin mortar into the distribution car for standby use. During the standby process, the secondary stirring pipe in the distribution car continuously stirs the resin mortar to make it more fully stirred and delay the setting time of the resin mortar.

[0033] Step 4: Plug both ends of the socket of the centrifugal ductile iron pipe to prevent the resin mortar from flowing out during the subsequent laying.

[0034] Step 5: Start the feeding car to extend the feeding rod into the centrifugal ductile iron pipe, and the resin mortar is evenly beaten into the inner wall of the centrifugal ductile iron pipe.

[0035] Step 6: Start the coating machine for centrifugal lining. First, control the coating machine pipe to rotate slowly at a low gear to make the resin mortar initially and evenly adhere to the inner wall of the centrifugal ductile iron pipe. Then rotate the pipe at a high speed at a high gear. Under the action of centrifugal force, the resin mortar is compacted and degassed on the inner wall of the centrifugal ductile iron pipe, so that the resin mortar is centrifugally formed.

[0036] Step 7: Keep the centrifugal ductile iron pipe rotating at a constant speed, and heat the centrifugal ductile iron pipe to make the temperature of the centrifugal ductile iron pipe reach 25-100°C. The heating time is 0.1-2h to solidify the resin mortar on the inner wall of the centrifugal ductile iron pipe.

[0037] Step 8: Shut down the coating machine, remove the socket plug of the centrifugal ductile iron pipe, obtain the resin sand lined composite pipe, and test the resin sand lined composite pipe to screen out qualified resin sand lined composite pipes. If there are defects inside the resin sand lined composite pipe, use resin mortar to repair it. Qualified resin sand lined composite pipes are guaranteed and stored in the warehouse.

[0038] The composite pipe of centrifugal ductile iron pipe and resin sand is formed, which makes full use of the excellent chemical corrosion resistance, wear resistance, resistance to seawater microorganism adhesion of the resin sand mixed layer and the good mechanical properties of ductile iron, and also has the characteristics of anti-corrosion, resistance to internal pressure, and small water flow resistance of FRP pipe. It can be used for gravity flow drainage, as well as pressure drainage and sewage discharge, and is especially suitable for sewage treatment pipe network. It overcomes the shortcomings of reinforced concrete pipes and FRP pipes and has a wider range of applications.

[0039] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for manufacturing a resin sand lined composite pipe with a ductile iron pipe as a base material, characterized in that: The following steps are involved: S1, a centrifugal ductile iron pipe is obtained by a centrifugal casting process; S2, weighing sand, unsaturated polyester resin, curing agent and accelerator, first stirring the unsaturated polyester resin and curing agent for 1-2 minutes, then adding the accelerator and stirring for 2-4 minutes, then adding sand and stirring, and fully stirring the resin mortar for 5-10 minutes to obtain resin mortar; S3, put the prepared resin mortar into the spreading vehicle for standby use; S4, plugging both ends of the socket of the centrifugal ductile iron pipe; S5, start the material distribution vehicle to extend the material distribution rod into the centrifugal ductile iron pipe, and evenly distribute the resin mortar on the inner wall of the centrifugal ductile iron pipe; S6, start the coating machine to perform centrifugal coating, first control the coating machine pipe to rotate at a low gear, so that the resin mortar is evenly attached to the inner wall of the centrifugal ductile iron pipe, and then rotate the pipe at a high gear. Under the action of centrifugal force, the resin mortar is compacted and degassed on the inner wall of the centrifugal ductile iron pipe, so that the resin mortar is centrifugally formed; S7, keeping the centrifugal ductile iron pipe rotating at a constant speed, and heating the centrifugal ductile iron pipe to solidify the resin mortar on the inner wall of the centrifugal ductile iron pipe; S8, shut down the coating machine, remove the centrifugal ductile iron pipe socket plug, and obtain the resin sand lined composite pipe.

2. The method for manufacturing a resin sand lined composite pipe with a ductile iron pipe as a base material according to claim 1, characterized in that: In S1, a water pressure test is performed on the centrifugal ductile iron pipe to screen qualified centrifugal ductile iron pipes.

3. The method for manufacturing a resin sand lined composite pipe with a ductile iron pipe as a base material according to claim 1, characterized in that: In S2, the curing agent is Trigonox V388 curing agent, and the accelerator is ZF-Ⅱ type unsaturated resin curing accelerator.

4. The method for manufacturing a resin sand lined composite pipe with a ductile iron pipe as a base material according to claim 1, characterized in that: In S3, during the preparation of the resin mortar, the secondary stirring pipe in the spreading vehicle is continuously stirred to prevent the resin mortar from solidifying.

5. The process for manufacturing a resin sand lined composite pipe with a ductile iron pipe as a base material according to claim 1, characterized in that: In S7, the centrifugal ductile iron pipe is heated to a temperature of 25-100°C for a heating time of 0.1-2h.

6. The method for manufacturing a resin sand lined composite pipe with a ductile iron pipe as a base material according to claim 1, characterized in that: In S1, the carbon content of the centrifugal ductile iron pipe is 3.3-3.6%, the silicon content is 3.3-3.5%, the chromium content is less than or equal to 0.03%, and the manganese content is less than or equal to 0.3%.

7. The method for manufacturing a resin sand lined composite pipe with a ductile iron pipe as a base material according to claim 1, characterized in that: In S2, the proportion of the resin mortar is as follows: 50-80% sand, 15-50% unsaturated polyester resin, 0.1-2.0% curing agent, and 0.1-2.0% accelerator.