Preparation method and application of porous carbon material with improved rate capability

Through the preparation of porous carbon materials doped with hydroxymethylated alkali lignin and phosphorus nitrogen, the problem of structural collapse of lignin-based porous carbon materials in heat treatment is solved, and excellent rate performance and electrolyte ion migration ability are achieved, which improves the The current density and specific capacitance retention rate of the supercapacitor.

CN119038526AActive Publication Date: 2024-11-29FUJIAN XINSEN CARBON

Patent Information

Application Number
CN202411274878.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-29
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The existing lignin-based porous carbon materials are prone to collapse during the heat treatment process of carbonization, resulting in complex pore structure and defects, affecting the diffusion of electrolyte ions, and the rate performance of supercapacitors is poor.

Method used

Using hydroxymethylated alkali lignin as the carbon source, phenyldiethanolamine derivative as the nitrogen source, and tricarboxylic acid-containing phosphorus-containing compounds as the phosphorus source, the phosphorus-doped porous carbon materials are prepared through self-assembly and high-temperature carbonization processes. , forming a three-dimensional network structure with cross-connection, reducing the collapse of the heat treatment charcoal formation process.

Benefits of technology

It significantly improves the rate performance of porous carbon materials, provides excellent electrolyte ion migration channels, and improves the current density and specific capacitance retention rate of the supercapacitor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038526A_ABST
    Figure CN119038526A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a porous carbon material with improved rate capability, and the preparation method comprises the following steps: 1) dispersing alkali lignin into water, dropwise adding alkali liquor, stirring until the alkali lignin is completely dissolved, dropwise adding a formaldehyde solution for hydroxymethylation, adjusting the pH value to be close to neutral, carrying out reduced pressure distillation, filtering, and adjusting the concentration with water to obtain a solution A; taking the hydroxymethylated alkali lignin as a carbon source for later use; 2) dissolving a template agent in a solvent to obtain a template agent solution; 3) uniformly mixing a carbon source, a nitrogen source, a phosphorus source and the template agent solution, controlling the temperature to volatilize the solvent, then heating and curing, and grinding into powder to obtain a composite head product; 4) performing low-temperature roasting and high-temperature carbonization on the high-molecular composite head product in an inert atmosphere to obtain a porous carbon material; the nitrogen source is a phenyl diethanol amine derivative, and the phosphorus source is a tricarboxylic acid phosphorus-containing compound. The porous carbon material has excellent rate capability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of carbon materials, and in particular relates to a method for preparing a porous carbon material with improved rate performance and an application thereof. Background Art

[0002] With the depletion of oil resources and the deteriorating environment, the development and conservation of energy has become an important issue in today's world. Energy materials and energy storage devices, as the main components, are closely related to the economy, resources and environment, and have always been the focus of research in various countries. As many fields have increasingly higher requirements for the power density of energy storage devices, which has exceeded the tolerance of batteries, in this context, a new energy storage element with a power density and energy density between traditional capacitors and secondary batteries, supercapacitors, has developed rapidly.

[0003] According to the electrode materials used, they can be divided into carbon electrode supercapacitors, precious metal oxide electrode supercapacitors and conductive polymer electrode supercapacitors. Porous carbon material-based supercapacitors belong to carbon electrode supercapacitors. Because porous carbon has a good pore size distribution, large specific surface area, and good conductivity, electrolyte ions can migrate freely in the pores, can quickly form a double layer, weaken the capacitance dispersion effect, and have a strong charge and discharge capacity, making it an ideal electrode material for supercapacitors.

[0004] Lignin is an important component of plant cell walls and is widely found in plant materials such as wood, straw, fruit shells, and leaves. It has the characteristics of wide sources and abundant reserves. Using lignin as a carbon source and applying it to the preparation of porous carbon materials can not only maximize its value, but also save energy and resources.

[0005] For example, the patent CN109019590B discloses a lignin-based multi-level porous carbon material and a preparation method thereof, wherein the preparation method comprises: lignin pretreatment, preparation of a low eutectic solvent, thermal carbonization of the low eutectic solvent of lignin, preparation of a solvent thermal carbonization product, activation of the solvent thermal carbonization product, and preparation of a lignin-based multi-level porous carbon material.

[0006] Patent CN106744793B discloses an alkali lignin-based porous carbon material for supercapacitors, a preparation method and application thereof, wherein the crude purified alkali lignin from papermaking black liquor is mixed with a triblock polymer Pluronic F127 and Mg(CH 3 COO 2 ·4H 2O is mixed, formaldehyde and hydrochloric acid are added and stirred evenly to obtain a mixed solution; the mixed solution is placed in an oven to dry to obtain a dark brown solid; the dark brown solid is then placed in a tube furnace for carbonization reaction, and nitrogen or inert gas is continuously introduced after the reaction is completed to cool to room temperature; finally, acid washing and water washing are performed, and a black powdery porous carbon material is obtained after drying.

[0007] The above porous carbon materials are prepared by using lignin as raw material through catalytic activation method or soft template method, etc., which have large specific surface area and rich pore structure. However, since the structure of lignin itself is relatively loose and irregular, it is mainly composed of phenylpropane units connected by ether bonds and carbon-carbon bonds. This structure is prone to collapse during the heat treatment process, resulting in complex and defective pore structure, which is not conducive to the diffusion of electrolyte ions and the rate performance of supercapacitors is poor. Summary of the invention

[0008] In order to solve the above technical problems, the present invention provides a method for preparing a porous carbon material with improved rate performance and its application, using hydroxymethylated alkali lignin as a carbon source, phenyldiethanolamine derivatives as a nitrogen source, and tricarboxylic acid-based phosphorus-containing compounds as a phosphorus source, and using self-assembly, high-temperature carbonization and other processes to prepare a phosphorus-nitrogen doped porous carbon material with excellent rate performance.

[0009] To achieve the above object, the present invention adopts the following technical solutions:

[0010] A method for preparing a porous carbon material with improved rate performance comprises the following steps:

[0011] 1) dispersing alkali lignin into water, adding alkali solution dropwise, stirring until the alkali lignin is completely dissolved, adding formaldehyde solution dropwise for hydroxymethylation, adjusting the pH to be close to neutral, performing vacuum distillation, filtering, and adjusting the concentration with water to obtain hydroxymethylated alkali lignin as a carbon source for later use;

[0012] 2) dissolving the template in a solvent to obtain a template solution;

[0013] 3) mixing the carbon source, nitrogen source, phosphorus source and template solution uniformly, controlling the temperature to volatilize the solvent, then heating and curing, and grinding into powder to obtain a composite primary product;

[0014] 4) Under an inert atmosphere, the polymer composite primary product is subjected to low-temperature calcination and high-temperature carbonization to obtain a porous carbon material;

[0015] The nitrogen source is a phenyldiethanolamine derivative, and the phosphorus source is a tricarboxylic acid-based phosphorus-containing compound.

[0016] Step 1) The weight average molecular weight of the alkali lignin is 1000-3000. The mass ratio of the alkali lignin to water is 1:4-6. Lignin is an aggregate, and there are many polar groups in the structure, especially more hydroxyl groups, which form strong intramolecular and intermolecular hydrogen bonds. Therefore, lignin is insoluble in water and any solvent, but alkali lignin is degraded lignin and can be dissolved in dilute water, alkaline or neutral polar solvents. The alkali lignin is selected from at least one of wood pulp alkali lignin, bamboo pulp alkali lignin, wheat straw pulp alkali lignin, reed pulp alkali lignin, bagasse pulp alkali lignin, and dragon beard grass pulp alkali lignin. The alkali solution is added dropwise to adjust the pH to 11-13; the alkali solution is a 30-40wt% sodium hydroxide solution or potassium hydroxide solution. The formaldehyde solution is a 30-40wt% formaldehyde aqueous solution. The mass ratio of the alkali lignin to the formaldehyde solution is 1:1.5-1.8. The formaldehyde solution is dripped in 0.5-1.5h, and the hydroxymethylation condition is to heat to 65-80℃ and react for 1-3h. The second pH adjustment is to adjust with a dilute hydrochloric acid solution with a concentration of 5-10wt%. The reduced pressure distillation is to distill under reduced pressure at a negative pressure of -0.090 to -0.098MPa and 35-55℃ for 3-5h. The filtration is to remove salt. The adjusted concentration is adjusted to 20-30wt%.

[0017] Step 2) The template is a nonionic surfactant, specifically selected from one or a combination of two or more of F127, P123, and Brij76. The solvent is selected from one or a combination of two of ethanol and isopropanol. The concentration of the template solution is 5-8wt%.

[0018] Step 3) the phenyldiethanolamine derivative is selected from one or a combination of two or more of N-benzyldiethanolamine, N-phenyldiethanolamine, N,N-dihydroxyethyl-m-toluidine, N,N-dihydroxyethyl-o-methylaniline; the tricarboxylic acid-based phosphorus-containing compound is selected from one or a combination of two or more of 2-phosphonobutane-1,2,4-tricarboxylic acid, 2-(phosphinoyl)propane-1,2,3-tricarboxylic acid, and 3-phospho-1,3,5-pentanetricarboxylic acid.

[0019] The mass ratio of the carbon source, nitrogen source, phosphorus source and template solution is 3:0.5-1:0.8-1:10-12. The temperature control is to control the temperature at 20-40°C, and the temperature rise curing is to rise to 100-120°C for 12-36 hours.

[0020] The carboxyl groups on the phosphorus source react with the hydroxyl groups on the nitrogen source and the carbon source during the temperature-raising solidification process to form a cross-connected three-dimensional network structure, which can reduce the collapse of the heat treatment carbonization process.

[0021] In step 4), the low temperature calcination is performed by heating the temperature to 300-500°C at a speed of 1-3°C and maintaining the temperature for 1-2 hours, and the high temperature carbonization is performed by heating the temperature to 600-1000°C at a speed of 2-10°C and maintaining the temperature for 3-5 hours.

[0022] A porous carbon material with improved rate performance is prepared by the above method.

[0023] The present invention also provides the application of the porous carbon material with improved rate performance, wherein the porous carbon material is applied to supercapacitors.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention uses hydroxymethylated alkali lignin as a carbon source, phenyldiethanolamine derivatives as a nitrogen source, and tricarboxylic acid-based phosphorus-containing compounds as a phosphorus source, and uses self-assembly, high-temperature carbonization and other processes to prepare a phosphorus-nitrogen doped porous carbon material with excellent rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the pore size distribution curve of the porous carbon material prepared in Example 1. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with specific embodiments, but is not limited to the contents of the specification. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight. The reagents used are all commercially available reagents in the art.

[0028] Wood pulp alkali lignin was purchased from Xinyi Feihuang Chemical Co., Ltd. with a weight average molecular weight of 2500.

[0029] Example 1

[0030] 1) Dispersing 100 parts of wood pulp alkali lignin into 500 parts of water, adding 40wt% sodium hydroxide to adjust the pH to 11.5, stirring at a speed of 250r / min until the solution is completely dissolved, adding 180 parts of 37wt% formaldehyde solution to carry out hydroxymethylation, and the dripping is completed for 1h, and the pH is adjusted to neutral with a 5wt% dilute hydrochloric acid solution, and the vacuum distillation is carried out at 35°C under a negative pressure of -0.098MPa for 3h, filtering to remove the precipitated sodium chloride, and adding water to adjust the concentration to 20wt%, to obtain hydroxymethylated alkali lignin and use it as a carbon source for standby use;

[0031] 2) dissolving 8 parts of template F127 in 92 parts of ethanol to obtain a template F127 solution with a concentration of 8 wt%;

[0032] 3) 30 parts of carbon source, 5 parts of nitrogen source N-benzyldiethanolamine, 10 parts of phosphorus source 2-phosphonobutane-1,2,4-tricarboxylic acid, and 10 parts of template F127 solution were mixed evenly, the temperature was controlled at 40°C for 48 hours to evaporate the water, then the temperature was raised to 100°C for curing for 16 hours, and finally ground into powder to obtain a composite primary product;

[0033] 4) Under a nitrogen atmosphere, the polymer composite primary product is added to a tubular furnace, the temperature is increased to 400°C at a rate of 1°C / min, and the product is calcined at 400°C for 1.5 h, the temperature is increased to 700°C at a rate of 1°C / min, and the product is carbonized at 700°C for 4 h to obtain a porous carbon material.

[0034] Example 2

[0035] The rest is the same as Example 1, except that in step 3), 2-(phosphinoyl)propane-1,2,3-tricarboxylic acid is used instead of 2-phosphonobutane-1,2,4-tricarboxylic acid with an equal mass.

[0036] Example 3

[0037] The rest is the same as Example 1, except that, in step 3), the amount of 2-phosphonobutane-1,2,4-tricarboxylic acid used is 8 parts.

[0038] Example 4

[0039] The rest is the same as Example 1, except that, in step 3), the amount of 2-phosphonobutane-1,2,4-tricarboxylic acid used is 12 parts.

[0040] Example 5

[0041] The rest is the same as Example 1, except that, in step 3), the amount of 2-phosphonobutane-1,2,4-tricarboxylic acid used is 6 parts.

[0042] Example 6

[0043] The rest is the same as Example 1, except that, in step 3), 20 parts of carbon source, 10 parts of nitrogen source N-benzyldiethanolamine, 10 parts of phosphorus source 2-phosphonobutane-1,2,4-tricarboxylic acid, and 12 parts of template F127 solution are mixed evenly, the temperature is controlled at 40°C for 48 hours to evaporate the water, then the temperature is raised to 100°C for curing for 16 hours, and finally ground into powder to obtain a composite primary product.

[0044] Comparative Example 1

[0045] The rest is the same as Example 1, except that N-ethyldiethanolamine of equal mass is used to replace N-benzyldiethanolamine.

[0046] Comparative Example 2

[0047] The rest is the same as Example 1, except that an equal mass of propanetricarboxylic acid is used to replace 2-phosphonobutane-1,2,4-tricarboxylic acid.

[0048] Preparation of working electrode

[0049] Application Example 1

[0050] The porous carbon material, conductive graphite and polytetrafluoroethylene emulsion of Example 1 were mixed in a mass ratio of 8:1:1, an appropriate amount of anhydrous ethanol was added as a dispersant, and an ultrasonic dispersant was used for 30 minutes to mix them evenly. The obtained slurry was placed in a blast drying oven at 80°C and steamed until it became viscous. The slurry was evenly coated on a disc-shaped nickel foam with a brush and placed in a vacuum drying oven at 80°C for 12 hours. A fully dried electrode sheet was pressed at a pressure of 12MPa for 60s using a manual powder tablet press to obtain an active material mass of 3mg / cm 2 working electrode.

[0051] Application Example 2

[0052] The rest is the same as Application Example 1, except that the porous carbon material is prepared according to Example 2-6.

[0053] Comparative Application Example 1-2

[0054] The rest is the same as Application Example 1, except that the porous carbon material is prepared according to Comparative Example 1-2.

[0055] The porous carbon materials prepared in the above-mentioned embodiments and comparative examples were subjected to the following pore structure and specific surface area performance tests, and the working electrodes prepared in the application examples and comparative application examples were subjected to rate performance tests:

[0056] 1. Pore structure and specific surface area: measured by NOVA 1000e pore structure specific surface area tester. The sample was degassed at 350℃ for 2h, and liquid nitrogen was used as the adsorption medium at 77K and relative pressure (P / P 0 )10 -6 N in the range of -1 2 The specific surface area was calculated by the BET equation.

[0057] 2. Rate performance: The metal Pt electrode was used as the counter electrode, the Hg / HgO electrode was used as the reference electrode, and the electrolyte was a 6 mol / L KOH solution. The working electrode was immersed in a 6 mol / L KOH solution for 24 hours before testing. The constant current charge and discharge test of the electrode was performed using the electrochemical workstation CHI660C of Shanghai Chenhua Instrument Co., Ltd., with current densities of 0.5 A / g and 20 A / g, and the specific capacitance retention rate at a current density of 20 A / g compared to 0.5 A / g was calculated.

[0058] The specific capacitance is calculated based on the charge and discharge test. The specific capacitance at different current densities is calculated using the following formula:

[0059] C=I*Δt / (m*ΔV)

[0060] Where I is the discharge current, A; Δt is the discharge time, s; m is the mass of the active material, g; ΔV is the actual discharge potential drop, V.

[0061] Table 1 Performance test results

[0062]

[0063] Depend on Figure 1 It can be seen that the porous carbon material prepared by the present invention has a bimodal pore structure, one of which is sharper and distributed in the micropore area, and is concentrated at about 1.5-2nm, and the other peak is distributed in the mesopore area, and is concentrated at about 10-15nm. This bimodal pore size distribution makes it have both concentrated and rich mesopores and a large specific surface area. A large number of mesopores provide a good channel for the rapid migration of ions. It can be seen from Table 1 that the porous carbon material prepared by the present invention has a high specific surface area and an appropriate pore structure. When it is applied to a supercapacitor with a current density of 0.5A / g, the specific capacitance of the preferred application example is as high as 397.6A / g, and it has a good transport capacity for ions; when the current density increases to 20A / g, the specific capacitance value retention rate is as high as 71.8%, which is smaller than the specific capacitance attenuation of comparative application example 1 and comparative application example 2, showing good rate performance, which is mainly attributed to its high mesoporosity and specific surface area.

[0064] Comparative Application Example 1 uses an equal amount of N-ethyldiethanolamine to replace N-benzyldiethanolamine, and its rate performance is poor. It is speculated that the formed pore structure is not strong, and a large number of micropores will still collapse after heat treatment. Comparative Application Example 2 uses an equal amount of propane tricarboxylic acid to replace 2-phosphonic acid butane-1,2,4-tricarboxylic acid, and its rate performance is also poor. It is speculated that the specific surface area is small, the pore structure is not rich, and the wettability to the electrolyte is poor.

[0065] It can be clearly seen from the application examples and comparative application examples that the nitrogen source and phosphorus source of the present invention have a significant synergistic effect of improving the rate performance of alkali lignin.

[0066] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.

Claims

1. A method for preparing a porous carbon material with improved rate performance, characterized in that: The steps include: 1) dispersing alkali lignin into water, adding alkali solution dropwise, stirring until the alkali lignin is completely dissolved, adding formaldehyde solution dropwise for hydroxymethylation, adjusting the pH to be close to neutral, performing vacuum distillation, filtering, and adjusting the concentration with water to obtain hydroxymethylated alkali lignin as a carbon source for later use; 2) dissolving the template in a solvent to obtain a template solution; 3) mixing the carbon source, nitrogen source, phosphorus source and template solution uniformly, controlling the temperature to volatilize the solvent, then heating and curing, and grinding into powder to obtain a composite primary product; 4) Under an inert atmosphere, the polymer composite primary product is subjected to low-temperature calcination and high-temperature carbonization to obtain a porous carbon material; The nitrogen source is a phenyldiethanolamine derivative, and the phosphorus source is a tricarboxylic acid-based phosphorus-containing compound.

2. The method for preparing a porous carbon material with improved rate performance according to claim 1, characterized in that: Step 1) The weight average molecular weight of the alkali lignin is 1000-3000; the mass ratio of the alkali lignin to water is 1:4-6.

3. The method for preparing a porous carbon material with improved rate performance according to claim 1, characterized in that: Step 1) the pH value of the step is adjusted to 11-13 by adding alkaline solution; the concentration of the step is adjusted to 20-30 wt%.

4. The method for preparing a porous carbon material with improved rate performance according to claim 1, characterized in that: Step 1) The alkali lignin is selected from at least one of wood pulp alkali lignin, bamboo pulp alkali lignin, wheat straw pulp alkali lignin, reed pulp alkali lignin, bagasse pulp alkali lignin, and sedge pulp alkali lignin; Step 2) The template is a non-ionic surfactant, specifically selected from one or a combination of two or more of F127, P123, and Brij76; the solvent is selected from one or a combination of two of ethanol and isopropanol; the concentration of the template solution is 5-8wt%.

5. The method for preparing a porous carbon material with improved rate performance according to claim 1, characterized in that: The phenyldiethanolamine derivative is selected from one or a combination of two or more of N-benzyldiethanolamine, N-phenyldiethanolamine, N,N-dihydroxyethyl-m-toluidine, and N,N-dihydroxyethyl-o-methylaniline; the tricarboxylic acid-based phosphorus-containing compound is selected from one or a combination of two or more of 2-phosphonobutane-1,2,4-tricarboxylic acid, 2-(phosphinoyl)propane-1,2,3-tricarboxylic acid, and 3-phospho-1,3,5-pentanetricarboxylic acid.

6. The method for preparing a porous carbon material with improved rate performance according to claim 1, characterized in that: The mass ratio of the carbon source, the nitrogen source, the phosphorus source and the template solution is 3:0.5-1:0.8-1:10-12.

7. The method for preparing a porous carbon material with improved rate performance according to claim 1, characterized in that: Step 3) The temperature control is to control the temperature at 20-40°C, and the temperature rise curing is to rise to 100-120°C for 12-36 hours.

8. The method for preparing a porous carbon material with improved rate performance according to claim 1, characterized in that: In step 4), the low temperature calcination is performed by heating the temperature to 300-500°C at a speed of 1-3°C and maintaining the temperature for 1-2 hours, and the high temperature carbonization is performed by heating the temperature to 600-1000°C at a speed of 2-10°C and maintaining the temperature for 3-5 hours.

9. A porous carbon material with improved rate performance, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the porous carbon material obtained by the preparation method according to any one of claims 1 to 8 or the porous carbon material according to claim 9, characterized in that: Used in supercapacitors.

Citation Information

Patent Citations

  • A porous carbon material for alkali lignin-based supercapacitors, its preparation method and application

    CN106744793B

  • Lignin-based hierarchical porous carbon materials and their preparation methods

    CN109019590B

  • Graphitized carbon material and preparation method thereof, and supercapacitor

    CN104944419A

  • Preparation method for biomass-based nitrogen-doped thin layer graphitized carbon material

    CN108285143A

  • Lignin porous carbon with even pore channels and preparation method thereof and application in lithium ion battery anode material

    CN108751160A

Cited By

  • Preparation method of high-strength composite bipolar plate

    CN119252961A

  • Activated carbon for high-magnification supercapacitor and preparation method

    CN121215442A