Preparation method of super-hydrophilic precipitated silica for silicone rubber

By preparing superhydrophilic precipitated silica in silicone rubber, the problem of insufficient mechanical strength of silicone rubber is solved, its tensile strength, hardness and wear resistance are improved, and superhydrophilic properties are given to it, which is suitable for many fields Application.

CN119038564APending Publication Date: 2024-11-29QUECHEN SILICON CHEM
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410865570.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Due to the small mechanical strength of silicone rubber, its tensile strength, hardness, wear resistance and tear resistance are poor, which limits its further application in many fields.

Method used

A method for preparing superhydrophilic precipitated silica for silicone rubber is adopted. By dissolving solid sodium silicate into a water glass solution and heating and stirring with sulfuric acid solution in a reactor, the pH value and feeding time are controlled to form super philippines. Silica particles of water and glycerol is added during the beating stage to increase its polarity.

Benefits of technology

It significantly improves the tensile strength, hardness, wear resistance and tear resistance of silicone rubber, enhances its compressive performance and elastic recovery, and gives it super hydrophilic properties, and is suitable for medical, food and construction fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a preparation method of super-hydrophilic precipitated silica for silicone rubber, which belongs to silica preparation and comprises the following steps: selecting solid sodium silicate with modulus of 2.5, dissolving the solid sodium silicate into a sodium silicate solution with concentration of 20wt%, and preparing a sulfuric acid solution with concentration of 10wt%; s2, adding the reaction initial solution obtained in the step S1 to 1 / 6-1 / 5 of the volume of the reaction kettle, heating to 50 DEG C, and controlling the stirring speed at 100 r / min; silicon dioxide is used as a reinforcing agent to be added into the silicon rubber, the tensile strength, hardness, wear resistance and tear resistance of the silicon rubber can be remarkably improved due to the special structure and surface characteristics of the silicon dioxide, and the compression resistance of the silicon rubber can be improved by the silicon dioxide; and the compression deformation rate and the elastic recovery of the silicone rubber are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of silicon dioxide preparation, and in particular relates to a method for preparing super-hydrophilic precipitated silicon dioxide for silicone rubber. Background Art

[0002] Silicone rubber has excellent high and low temperature resistance, good electrical insulation, excellent chemical resistance and weather resistance, so silicone rubber has been used in many fields such as medicine and health, aerospace, electronics and electrical, wires and cables, etc. Silicone rubber is divided into heat vulcanized type (high temperature vulcanized silicone HTV) and room temperature vulcanized type (RTV). High temperature silicone rubber is mainly used to manufacture various silicone rubber products, while room temperature silicone rubber is mainly used as adhesive, potting material or mold.

[0003] Another characteristic of silicone rubber is that it has almost no mechanical strength. Due to the low mechanical strength of silicone rubber, the tensile strength, hardness, wear resistance and tear resistance of silicone rubber may be poor, thus limiting its further application. For this reason, we propose a method for preparing super hydrophilic precipitated silica for silicone rubber. Summary of the invention

[0004] The present invention provides a method for preparing super-hydrophilic precipitated silica for silicone rubber, so as to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing super-hydrophilic precipitated silica for silicone rubber, comprising the following steps:

[0006] S1. Select solid sodium silicate with a modulus of 2.5 to 3.5, dissolve the solid sodium silicate into a water glass solution, and prepare a sulfuric acid solution;

[0007] S2, adding the water glass solution obtained in step S1 as the initial reaction liquid into the reaction kettle, and heating and stirring;

[0008] S3, adding the water glass solution and sulfuric acid solution prepared in step S1 into the reactor in sequence, stirring, and controlling the feeding time;

[0009] S4, after the addition of S3 is completed, sulfuric acid solution is continued to be added dropwise to the suspension for acidification, and the residual water glass solution in the suspension continues to react with the sulfuric acid solution until the pH value of the reaction system is controlled within the range of 5 to 7;

[0010] S5. After the precipitation reaction in S4 is completed, the reaction system is further aged in the reactor for 10 to 20 minutes;

[0011] S6. After aging, the slurry is filtered and washed with industrial water. The content of sodium sulfate in the filter cake is determined by the conductivity of the washing water, and the sodium sulfate content of the final product is controlled to be less than 2%. The solid content of the filter cake is controlled at 20% to 25%, and the filter cake is sent to a pulping machine to form a slurry.

[0012] S7, adding glycerol during the filter cake beating stage;

[0013] S8. Using hot air generated by a natural gas combustion furnace as a drying heat source, the slurry to which glycerol is added is dried to obtain granular silicon dioxide with a moisture content of 4% to 6%.

[0014] Furthermore, in step S1, the water glass solution is divided into two parts, one part is used as the initial reaction liquid, and the other part is used as an additive liquid having the same function as the sulfuric acid solution.

[0015] Furthermore, in step S1, the concentration of the water glass solution is 20wt% to 25wt%; the concentration of the sulfuric acid solution is 10wt% to 15wt%.

[0016] Furthermore, in the step S2, the volume of the initial liquid is added to 1 / 6 to 1 / 5 of the volume of the reactor, and the temperature is raised to a range of 50° C. to 70° C., and the stirring speed is controlled at 100 r / min to 200 r / min.

[0017] Furthermore, after the water glass solution and the sulfuric acid solution are added to the reactor in S3, the pH value in the reactor is ensured to be in the range of 9 to 11, the reaction temperature is maintained at 50° C. to 70° C., and the stirring speed is maintained at 100 r / min to 200 r / min until the reaction liquid reaches 2 / 3 of the volume of the reactor, and the feeding time is controlled in the range of 70 min to 80 min.

[0018] The beneficial effects of the present invention are:

[0019] By adding silica as a reinforcing agent to silicone rubber, the special structure and surface properties of silica make it possible to significantly improve the tensile strength, hardness, wear resistance and tear resistance of silicone rubber in silicone rubber, and silica can also improve the compressive properties of silicone rubber, improve the compression deformation rate and elastic recovery of silicone rubber, so that the silicone rubber can be used in the medical device industry, the silicone rubber surface can have better wettability to physiological fluids, and the accuracy and safety of surgical operations can be improved; if it is used in the food industry, it can make food processing sites easier to clean, thereby ensuring the hygiene and safety of food processing; if it is used in building sealing materials, the sealing materials can be more expansive and their water-sealing, air-sealing and sound-insulating capabilities can be enhanced, and propylene glycol is added in the pulping stage to increase the polarity of silica, so that the silicone rubber product has super hydrophilic properties and its surface contact angle is less than 10°. DETAILED DESCRIPTION

[0020] In order to further understand the content, features and effects of the present invention, the following embodiments are given.

[0021] Embodiment 1:

[0022] A method for preparing super-hydrophilic precipitated silica for silicone rubber comprises the following steps:

[0023] S1, select solid sodium silicate with a modulus of 2.5, dissolve the solid sodium silicate into a water glass solution with a concentration of 20wt%, and prepare a sulfuric acid solution with a concentration of 10wt%;

[0024] S2, adding the initial reaction solution obtained in step S1 to 1 / 6 to 1 / 5 of the volume of the reactor, and heating to 50°C, while controlling the stirring speed at 100r / min;

[0025] S3, the water glass solution and sulfuric acid solution prepared in step S1 are added to the reactor in sequence, the pH value in the reactor is ensured to be in the range of 9 to 11, the reaction temperature is maintained at 50° C. to 70° C., the stirring speed is maintained at 100 r / min, and the reaction liquid is stopped until it reaches 2 / 3 of the volume of the reactor, and the feeding time is controlled within the range of 70 min to 80 min;

[0026] S4, after the addition of S3 is completed, sulfuric acid solution is continued to be added dropwise to the suspension for acidification, and the residual water glass solution in the suspension continues to react with the sulfuric acid solution until the pH value of the reaction system is controlled within the range of 5 to 7;

[0027] S5. After the precipitation reaction in S4 is completed, the reaction system is aged in the reactor for 10 minutes;

[0028] S6. After aging, the slurry is filtered and washed with industrial water. The sodium sulfate content in the filter cake is determined by the conductivity of the washing water, and the sodium sulfate content of the final product is controlled to be less than 2%. The solid content of the filter cake is controlled at 20% to 25%, and it is directly sent to the pulping machine to form a thick slurry;

[0029] S7, adding glycerol during the filter cake beating stage;

[0030] S8. Using hot air generated by a natural gas combustion furnace as a drying heat source, the slurry to which glycerol is added is dried to obtain granular silicon dioxide with a moisture content of 4% to 6%.

[0031] Embodiment 2:

[0032] S1, select solid sodium silicate with a modulus of 3.0, dissolve the solid sodium silicate into a water glass solution with a concentration of 22wt%, and prepare a sulfuric acid solution with a concentration of 12wt%;

[0033] S2, adding the initial reaction solution obtained in step S1 to 1 / 6 to 1 / 5 of the volume of the reactor, and heating to 60°C, while controlling the stirring speed at 150r / min;

[0034] S3, the water glass solution and sulfuric acid solution prepared in step S1 are added to the reactor in sequence, the pH value in the reactor is ensured to be in the range of 9 to 11, the reaction temperature is maintained at 50°C to 70°C, the stirring speed is maintained at 150r / min, and the reaction is stopped until the reaction solution reaches 2 / 3 of the volume of the reactor, and the feeding time is controlled within the range of 70min to 80min;

[0035] S4, after the addition of S3 is completed, sulfuric acid solution is continued to be added dropwise to the suspension for acidification, and the residual water glass solution in the suspension continues to react with the sulfuric acid solution until the pH value of the reaction system is controlled within the range of 5 to 7;

[0036] S5. After the precipitation reaction in S4 is completed, the reaction system is aged in the reactor for 15 minutes;

[0037] S6. After aging, the slurry is filtered and washed with industrial water. The sodium sulfate content in the filter cake is determined by the conductivity of the washing water, and the sodium sulfate content of the final product is controlled to be less than 2%. The solid content of the filter cake is controlled at 20% to 25%, and it is directly sent to the pulping machine to form a thick slurry;

[0038] S7, adding glycerol during the filter cake beating stage;

[0039] S8. Using hot air generated by a natural gas combustion furnace as a drying heat source, the slurry to which glycerol is added is dried to obtain granular silicon dioxide with a moisture content of 4% to 6%.

[0040] Embodiment three:

[0041] S1, select solid sodium silicate with a modulus of 3.5, dissolve the solid sodium silicate into a water glass solution with a concentration of 25wt%, and prepare a sulfuric acid solution with a concentration of 15wt%;

[0042] S2, adding the initial reaction solution obtained in step S1 to 1 / 6 to 1 / 5 of the volume of the reactor, and heating to 70°C, while controlling the stirring speed at 200r / min;

[0043] S3, the water glass solution and sulfuric acid solution prepared in step S1 are added to the reactor in sequence, the pH value in the reactor is ensured to be in the range of 9 to 11, the reaction temperature is maintained at 50° C. to 70° C., the stirring speed is maintained at 200 r / min, and the reaction liquid is stopped until it reaches 2 / 3 of the volume of the reactor, and the feeding time is controlled within the range of 70 min to 80 min;

[0044] S4, after the addition of S3 is completed, sulfuric acid solution is continued to be added dropwise to the suspension for acidification, and the residual water glass solution in the suspension continues to react with the sulfuric acid solution until the pH value of the reaction system is controlled within the range of 5 to 7;

[0045] S5. After the precipitation reaction in S4 is completed, the reaction system is further aged in the reactor for 20 minutes;

[0046] S6. After aging, the slurry is filtered and washed with industrial water. The sodium sulfate content in the filter cake is determined by the conductivity of the washing water, and the sodium sulfate content of the final product is controlled to be less than 2%. The solid content of the filter cake is controlled at 20% to 25%, and it is directly sent to the pulping machine to form a thick slurry;

[0047] S7, adding glycerol during the filter cake beating stage;

[0048] S8. Using hot air generated by a natural gas combustion furnace as a drying heat source, the slurry to which glycerol is added is dried to obtain granular silicon dioxide with a moisture content of 4% to 6%.

[0049] Table 1 Silicon dioxide of Examples 1 to 3

[0050]

[0051] It can be seen from the above embodiments that the method of the present invention can achieve the preparation of silica with a BET of 200-300 m2 / g, a median diameter (D50) of 10-20 um, a pore volume of 1.5-2.0 cm3 / g, and a silica content of 95% to 98%.

[0052] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing super-hydrophilic precipitated silica for silicone rubber, characterized in that: The following steps are involved: S1. Select solid sodium silicate with a modulus of 2.5 to 3.5, dissolve the solid sodium silicate into a water glass solution, and prepare a sulfuric acid solution; S2, adding the water glass solution obtained in step S1 as the initial reaction liquid into the reaction kettle, and heating and stirring; S3, adding the water glass solution and sulfuric acid solution prepared in step S1 into the reactor in sequence, stirring, and controlling the feeding time; S4, after the addition of S3 is completed, sulfuric acid solution is continued to be added dropwise to the suspension for acidification, and the residual water glass solution in the suspension continues to react with the sulfuric acid solution until the pH value of the reaction system is controlled within the range of 5 to 7; S5. After the precipitation reaction in S4 is completed, the reaction system is further aged in the reactor for 10 to 20 minutes; S6. After aging, the slurry is filtered and washed with industrial water. The content of sodium sulfate in the filter cake is determined by the conductivity of the washing water, and the sodium sulfate content of the final product is controlled to be less than 2%. The solid content of the filter cake is controlled at 20% to 25%, and the filter cake is sent to a pulping machine to form a slurry. S7, adding glycerol during the filter cake beating stage; S8. Using hot air generated by a natural gas combustion furnace as a drying heat source, the slurry to which glycerol is added is dried to obtain granular silicon dioxide with a moisture content of 4% to 6%.

2. The method for preparing super-hydrophilic precipitated silica for silicone rubber according to claim 1, characterized in that: In the step S1, the water glass solution is divided into two parts, one part is used as the initial reaction liquid, and the other part is used as the additive liquid with the same function as the sulfuric acid solution.

3. The method for preparing super hydrophilic precipitated silica for silicone rubber according to claim 1, characterized in that: In the step S1, the concentration of the water glass solution is 20wt% to 25wt%; the concentration of the sulfuric acid solution is 10wt% to 15wt%.

4. The method for preparing super-hydrophilic precipitated silica for silicone rubber according to claim 1, characterized in that: In the step S2, the volume of the initial liquid is added to 1 / 6 to 1 / 5 of the volume of the reactor, and the temperature is raised to a range of 50° C. to 70° C., and the stirring speed is controlled at 100 r / min to 200 r / min.

5. The method for preparing super hydrophilic precipitated silica for silicone rubber according to claim 1, characterized in that: After the water glass solution and the sulfuric acid solution are added to the reactor in S3, the pH value in the reactor is ensured to be in the range of 9 to 11, the reaction temperature is maintained at 50° C. to 70° C., and the stirring speed is maintained at 100 r / min to 200 r / min until the reaction liquid reaches 2 / 3 of the volume of the reactor, and the feeding time is controlled in the range of 70 min to 80 min.

Citation Information

Patent Citations

  • Process for producing deposition white carbon black for silicon rubber

    CN101402457A

  • Preparation method of silica

    CN102020284A

  • Precipitated silicon dioxide, and preparation method and application thereof

    CN104291342A

  • Precipitated silicon dioxide with low silanol, preparation method and use thereof

    CN104291345A

  • Synthesis process of slow-release high-adsorption silicon dioxide

    CN115159533A