Bimodal distribution flocculant and preparation method thereof

By using bimodal distributed flocculants, the synergistic effect of large and small molecule flocculants is used to solve the problem of extremely fine particles difficult to settle during red mud settlement in alumina production, improving the sedimentation efficiency and transparency, and reducing floating objects content.

CN119038720AActive Publication Date: 2024-11-29ZHENGZHOU NON FERROUS METALS RES INST CO LTD OF CHALCO
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411399172.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-29
Estimated Expiration
2044-10-09

AI Technical Summary

Technical Problem

During the production of alumina, the floating content of the red mud settled coarse liquid has a high degree of floating content, low clarity, and poor bottom flow compression performance. This is mainly due to the excessive goiter content in overseas bauxite, which makes it difficult for extremely fine particles to settle.

Method used

Using a bimodal distribution flocculant, consisting of a macromolecular flocculant and a small molecule reinforcement, the extremely fine particles are captured through the small molecule reinforcement and promote initial aggregation. The macromolecular flocculant then passes through the bridge of long-chain structure and oxygen-oxamic acid groups. The bonding action forms large and stable flocs, improving the settlement efficiency.

Benefits of technology

It significantly improves the sedimentation efficiency of extremely fine particles, reduces the floating content, and improves the transparency and sedimentation speed of the red mud settlement process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038720A_ABST
    Figure CN119038720A_ABST
Patent Text Reader

Abstract

The invention provides a bimodal distribution flocculant and a preparation method thereof, and belongs to the field of flocculants. The bimodal distribution flocculating agent is composed of a macromolecular flocculating agent and a micromolecular reinforcing agent; wherein the macromolecular flocculating agent and the micromolecular reinforcing agent are hydroxamic acid flocculating agents; the molecular weight of the macromolecular flocculant is more than or equal to 5 million, and the molecular weight of the micromolecular enhancer is less than or equal to 60 million. According to the invention, a macromolecular flocculant and a micromolecular enhancer form a bimodal distribution flocculant. In the red mud sedimentation crude liquid treatment process, firstly, a micromolecule reinforcing agent is used for capturing superfine particles and promoting the superfine particles to primarily aggregate, so that small flocs are formed; then, the macromolecular flocculant is used for further bridging the small flocs into large and stable flocs under the bridging action of a long-chain structure and a hydroxamic acid group; the increase and stabilization of floccules are beneficial to accelerating the settling process, improving the settling efficiency of superfine particles and reducing the content of suspended matters. Therefore, the sedimentation efficiency of superfine particles of the flocculating agent in the red mud sedimentation process is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of flocculants, and in particular to a bimodal distribution flocculant and a preparation method thereof. Background Art

[0002] In the alumina production process, the sedimentation separation of dissolved red mud and crude liquid is the most important solid-liquid separation process, which directly affects the production technical indicators and economic benefits. The key factors in the red mud separation process are the properties of the red mud slurry, that is, the mineral composition, particle size distribution and solution composition of the red mud. The particle size of Bayer red mud is generally fine. Studies have shown that particles <0.4mm account for more than 90%. It can be seen that the dissolved red mud slurry is a fine particle suspension, which has many similar properties to the colloidal dispersion system. In this suspension system, red mud particles are the dispersed phase and sodium aluminate solution is the dispersion medium. Red mud particles have an extremely diffuse surface, and its surface shows large residual valence forces, van der Waals forces and hydrogen bonds, which will cause solvation.

[0003] In recent years, as domestic bauxite resources have gradually been depleted, various aluminum companies have begun to use a large number of overseas bauxite such as Guinea to produce alumina. However, in the production process, there are problems such as opacity of red mud sedimentation crude liquid, high content of suspended matter, low clarity, and poor bottom flow compression performance, which have affected the normal production of some companies. The above problems arise because the content of goethite in these overseas mines is too high, and goethite is mostly present in the form of fine crystal clusters in bauxite. In the process of alumina production, due to grinding, dissolution and other processes, it will become extremely fine irregular particles, and the particle size can even be refined to between 2 and 10μm. It has high surface activity and severe solvation. Therefore, these extremely fine red mud particles are easy to form a stable suspension state in the slurry. Even if the goethite inside it is converted into hematite, it is difficult to change its sedimentation performance. Whether these extremely fine red mud particles can be captured and settled determines the content of suspended matter and transparency of the sedimentation crude liquid. Summary of the invention

[0004] The present application provides a bimodal distribution flocculant and a preparation method to solve the following technical problem: how to improve the settling efficiency of very fine particles of the flocculant during the red mud settling process.

[0005] In a first aspect, the present application provides a bimodal distribution flocculant, wherein the bimodal distribution flocculant is composed of a macromolecular flocculant and a small molecule enhancer; wherein:

[0006] The macromolecular flocculant and the small molecule enhancer are both hydroxamic acid flocculants;

[0007] The molecular weight of the macromolecular flocculant is ≥5 million, and the molecular weight of the small molecule reinforcing agent is ≤600,000.

[0008] Optionally, the mass ratio of the macromolecular flocculant to the small molecule enhancer is (1-6):1.

[0009] Optionally, the mass ratio of the macromolecular flocculant to the small molecule enhancer is (2-4):1.

[0010] In a second aspect, the present application provides a method for preparing the bimodal distribution flocculant according to any one embodiment of the first aspect, the method comprising:

[0011] Mixing polyacrylamide with a set molecular weight, a solvent and a hydroxylamine solution, and adjusting the pH to a first set pH, so as to perform a first water bath reaction under a first set reaction condition to obtain a macromolecular flocculant;

[0012] Mixing acrylamide, a solvent and an initiator to perform a polymerization reaction to obtain a mixed solution;

[0013] The mixed solution is mixed with a hydroxylamine solution, and the pH is adjusted to a second set pH, so as to perform a second water bath reaction under a second set reaction condition to obtain a small molecule enhancer;

[0014] The macromolecular flocculant and the small molecule reinforcing agent are compounded to obtain a bimodal distribution flocculant.

[0015] Optionally, the concentration of the polyacrylamide is 2% to 5%.

[0016] Optionally, the molar ratio of the polyacrylamide to hydroxylamine is 1:(1.2-1.8).

[0017] Optionally, the first set reaction conditions include: the protective atmosphere is nitrogen, the reaction temperature is 50°C to 80°C, the first set pH is 10 to 13, and the reaction time is 8h to 20h.

[0018] Optionally, the concentration of the acrylamide is 2% to 4%, the concentration of the initiator is 0.3% to 0.6%, and the initiator includes: one or more of ammonium persulfate and sodium bisulfite.

[0019] Optionally, the molar ratio of acrylamide to hydroxylamine is 1:(1.1-1.5).

[0020] Optionally, the second set reaction conditions include: the protective atmosphere is nitrogen, the reaction temperature is 50°C to 80°C, the second set pH is 10 to 13, and the reaction time is 5h to 10h.

[0021] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:

[0022] The present invention provides a bimodal distribution flocculant, which is composed of a macromolecular flocculant and a small molecule reinforcing agent; wherein the macromolecular flocculant and the small molecule reinforcing agent are both hydroxamic acid flocculants; the molecular weight of the macromolecular flocculant is ≥5 million, and the molecular weight of the small molecule reinforcing agent is ≤600,000. The present invention forms a bimodal distribution flocculant by a macromolecular flocculant and a small molecule reinforcing agent. In the process of treating red mud sedimentation crude liquid, the small molecule reinforcing agent is first used to capture ultrafine particles and promote their initial aggregation to form small flocs. Subsequently, the macromolecular flocculant further bridges these small flocs into large and stable flocs through the bridging action of its long chain structure and hydroxamic acid group. The enlargement and stabilization of the flocs help to accelerate the sedimentation process, improve the sedimentation efficiency of ultrafine particles, and reduce the content of suspended solids. Thereby, the sedimentation efficiency of ultrafine particles of the flocculant during the red mud sedimentation process is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.

[0024] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0025] Figure 1 A schematic flow chart of a method for preparing a bimodal distribution flocculant provided in an embodiment of the present application. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0027] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0028] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.

[0029] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0030] The present application provides a bimodal distribution flocculant, which is composed of a macromolecular flocculant and a small molecule enhancer; wherein:

[0031] The macromolecular flocculant and the small molecule enhancer are both hydroxamic acid flocculants;

[0032] The molecular weight of the macromolecular flocculant is ≥5 million, and the molecular weight of the small molecule reinforcing agent is ≤600,000.

[0033] The molecular weight of the macromolecular flocculant is ≥5 million, which ensures that it has good bridging ability and a wide range of intermolecular contact surfaces, which helps to form a larger floc structure in the suspension. The molecular weight of the small molecule reinforcing agent is ≤600,000. Compared with the macromolecular flocculant, the molecular weight of the small molecule reinforcing agent is smaller, so it can penetrate into the suspended particles more quickly, enhance the interaction force between the particles, and make the flocs more compact and not easy to break. At the same time, both the macromolecular flocculant and the small molecule reinforcing agent are hydroxamic acid flocculants. This consistency enables the two components to more efficiently exert their respective advantages when acting synergistically, avoiding unnecessary chemical reactions or mutual interference. Therefore, the present invention mixes the synthesized macromolecular flocculant with the small molecule reinforcing agent in a certain proportion to form a bimodal distribution flocculant. In the process of treating the crude liquid of red mud sedimentation, the small molecule reinforcing agent is first used to capture the extremely fine particles and promote their initial aggregation to form small flocs. Subsequently, the macromolecular flocculant further bridges these small flocs into large and stable flocs through the bridging action of its long chain structure and hydroxamic acid group. Finally, the enlargement and stabilization of the flocs help accelerate the sedimentation process, improve the sedimentation efficiency of very fine particles, and reduce the content of suspended solids. For example, the molecular weight of the macromolecular flocculant can be 5 million, 7 million, 8 million, 9 million, 10 million, 11 million, 12 million, 13 million, 14 million, etc., and the molecular weight of the small molecule enhancer can be 100,000, 200,000, 300,000, 400,000, 500,000, 600,000, etc.

[0034] In some embodiments, the mass ratio of the macromolecular flocculant to the small molecule enhancer is (1-6):1.

[0035] The mass ratio of the macromolecular flocculant to the small molecule reinforcing agent is limited to (1-6):1, which balances the bridging effect of the macromolecular flocculant and the particle capturing ability of the small molecule reinforcing agent. The macromolecular flocculant can form a larger floc structure, while the small molecule reinforcing agent can effectively capture and fix extremely fine particles, enhancing the overall flocculation effect. At the same time, the present invention can select different proportions of macromolecular flocculants and small molecule reinforcing agents according to the needs of sodium aluminate solutions composed of different red mud. Exemplarily, the mass ratio of the macromolecular flocculant to the small molecule reinforcing agent is 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, etc.

[0036] In some embodiments, the mass ratio of the macromolecular flocculant to the small molecule enhancer is (2-4):1.

[0037] Preferably, the mass ratio of the macromolecular flocculant to the small molecular enhancer is limited to (2-4):1, which can further enhance the overall flocculation effect.

[0038] Figure 1 A schematic flow chart of a method for preparing a bimodal distribution flocculant provided in an embodiment of the present application.

[0039] Based on a general inventive concept, see Figure 1 The present application provides a method for preparing a bimodal distribution flocculant according to any one of the embodiments of the first aspect, the method comprising:

[0040] S1, mixing polyacrylamide with a set molecular weight, a solvent and a hydroxylamine solution, and adjusting the pH to a first set pH, so as to perform a first water bath reaction under a first set reaction condition to obtain a macromolecular flocculant;

[0041] It should be noted that the molecular weight of polyacrylamide should be selected according to the molecular weight requirements of the target macromolecular flocculant. The reaction of polyacrylamide (PAM) and hydroxylamine (NH2OH) under alkaline conditions and water bath heating obtains a hydroxamic acid (RCONHOH) group on the molecular chain through a nucleophilic substitution reaction. The specific reaction principle is as follows: In an alkaline environment, hydroxylamine will first be converted into a hydroxylamine anion (NH2O-), which has a strong nucleophilicity and can attack the carbonyl (C=O) carbon atom on the polyacrylamide molecular chain to form an addition intermediate. Subsequently, this intermediate undergoes rearrangement and hydrolysis reactions to eventually generate a polyacrylamide derivative containing a hydroxamic acid group, thereby obtaining a macromolecular hydroxamic acid flocculant.

[0042] In some embodiments, the concentration of the polyacrylamide is 2% to 5%.

[0043] Limiting the mass concentration of polyacrylamide to 2% to 5% helps ensure that there are enough polyacrylamide molecules in the solvent to participate in the reaction, while avoiding the problem of uneven reaction or difficulty in control due to excessive concentration. Exemplarily, the concentration of polyacrylamide can be 2%, 2.5%, 3%, 4%, 4.5%, 5%, etc.

[0044] In some embodiments, the molar ratio of polyacrylamide to hydroxylamine is 1:(1.2-1.8).

[0045] The molar ratio of polyacrylamide to hydroxylamine is limited to 1:(1.2-1.8), thereby balancing the reaction efficiency and the generation of by-products. An excess of hydroxylamine over polyacrylamide can ensure that more amide groups in polyacrylamide are converted into hydroxamic acid groups, but too much hydroxylamine may also lead to unnecessary side reactions and cause excessive costs. Exemplarily, the molar ratio of polyacrylamide to hydroxylamine can be 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.75, 1:1.8, etc.

[0046] In some embodiments, the first set reaction conditions include: the protective atmosphere is nitrogen, the reaction temperature is 50°C to 80°C, the first set pH is 10 to 13, and the reaction time is 8h to 20h.

[0047] Limiting nitrogen as a protective atmosphere can eliminate the interference of oxygen on the reaction. Limiting the reaction temperature to 50°C to 80°C is conducive to the occurrence of hydroxylation reaction. Higher temperatures can accelerate the reaction rate, but may also increase the risk of side reactions; lower temperatures may prolong the reaction time. Limiting the reaction pH to 10-13 is the alkaline condition required for hydroxylation reaction. In this pH range, amide groups are more likely to react with hydroxylamine to generate hydroxamic acid groups. Limiting the reaction time to 8h to 20h can ensure that the reaction is fully carried out and achieve a higher conversion rate. Exemplarily, the reaction temperature can be 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, etc., the first set pH can be 10, 10.5, 11, 11.5, 12, 12.5, 13, etc., and the reaction time can be 8h, 9h, 10h, 11h, 13h, 15h, 17h, 19h, 20h, etc.

[0048] The invention can prepare a macromolecular flocculant with expected molecular weight, high content of hydroxamic acid groups and good flocculation performance by precisely controlling the concentration of polyacrylamide, the molar ratio of polyacrylamide to hydroxylamine and the conditions of the first water bath reaction (including protective atmosphere, reaction temperature, pH and reaction time).

[0049] S2, mixing acrylamide, a solvent and an initiator to perform a polymerization reaction to obtain a mixed solution;

[0050] On the oligomer or prepolymer of polyacrylamide, a small molecule reinforcing agent with a hydroxamic acid group is generated.

[0051] In some embodiments, the concentration of acrylamide is 2% to 4%, the concentration of the initiator is 0.3% to 0.6%, and the initiator includes one or more of ammonium persulfate and sodium bisulfite.

[0052] The mass concentration of acrylamide is limited to 2% to 4%, which can not only ensure the progress of the polymerization reaction, but also avoid the operational difficulties caused by excessive viscosity. The mass concentration of the initiator is limited to 0.3% to 0.6%, which is sufficient to initiate the polymerization reaction of acrylamide without introducing too many impurities. Ammonium persulfate and sodium bisulfite are commonly used free radical initiators, which can effectively generate free radicals to initiate monomer polymerization. Exemplarily, the concentration of acrylamide can be 2%, 2.5%, 3%, 3.5%, 4%, etc., and the concentration of the initiator can be 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, etc.

[0053] S3, mixing the mixed solution with a hydroxylamine solution, and adjusting the pH to a second set pH, to perform a second water bath reaction under a second set reaction condition, to obtain a small molecule enhancer;

[0054] In some embodiments, the molar ratio of acrylamide to hydroxylamine is 1:(1.1-1.5).

[0055] The molar ratio of acrylamide to hydroxylamine is limited to 1:(1.1-1.5), which ensures an excess of hydroxylamine, so that more amide groups in the polyacrylamide oligomer can be converted into hydroxamic acid groups. For example, the molar ratio of acrylamide to hydroxylamine can be 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, etc.

[0056] In some embodiments, the second set reaction conditions include: the protective atmosphere is nitrogen, the reaction temperature is 50° C. to 80° C., the second set pH is 10 to 13, and the reaction time is 5 h to 10 h.

[0057] S4, compounding the macromolecular flocculant and the small molecular reinforcing agent to obtain a bimodal distribution flocculant.

[0058] In some embodiments, the method further comprises:

[0059] The bimodal distribution flocculant is placed in a weakly alkaline aqueous solution until it is completely dissolved for sedimentation.

[0060] The product prepared by the method for preparing a bimodal distribution flocculant is the above-mentioned bimodal distribution flocculant. The chemical composition and structure of the bimodal distribution flocculant prepared by the method for preparing a bimodal distribution flocculant can refer to the above-mentioned embodiment. Since the method for preparing a bimodal distribution flocculant adopts part or all of the technical solutions of the bimodal distribution flocculant embodiment, it at least has all the beneficial effects brought by the technical solutions of the bimodal distribution flocculant embodiment, which will not be described one by one here.

[0061] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.

[0062] Example 1

[0063] Weigh polyacrylamide with a molecular weight of 5 million, slowly add it to a beaker containing a certain amount of distilled water under stirring, the concentration is 3.55%, after complete dissolution, transfer the viscous solution to a 250mL three-necked flask, and place the reaction bottle in a constant temperature water bath at 50°C. Weigh a certain amount of hydroxylamine hydrochloride and sodium hydroxide in equal molar ratios and dissolve them in a certain amount of distilled water to obtain a neutralized hydroxylamine solution, add the hydroxylamine solution to the reaction bottle, the molar ratio of polyacrylamide to hydroxylamine is 1:1.5, and adjust the pH to about 12.5. Stir magnetically, pass 50mL / min high-purity N2 throughout the process, and react for 12h to synthesize a macromolecular hydroxamic acid flocculant.

[0064] Weigh acrylamide and slowly add it to a flask containing a certain amount of distilled water under stirring. The concentration of acrylamide is 2.5%. Add initiators: ammonium persulfate and sodium bisulfite. The concentration of initiator is 0.40%. The reaction time is 0.5h. Weigh a certain amount of hydroxylamine hydrochloride and sodium hydroxide in equal molar ratio and dissolve them in a certain amount of distilled water to obtain a neutralized hydroxylamine solution. Add the hydroxylamine solution to the flask. The molar ratio of acrylamide to hydroxylamine is 1:1.5. Adjust the pH to about 12.5. Pass 50mL / min high-purity N2 throughout the process. The reaction time is 6h. The enhancer with a molecular weight of about 400,000 is synthesized.

[0065] The two synthetic flocculants are compounded to form a flocculant product with bimodal distribution of size.

[0066] The bimodal distribution flocculant product was subjected to a sedimentation test. When the addition amount of the bimodal distribution flocculant was 85g / t, the mass ratio of the small molecule enhancer with a molecular weight of 400,000 to the macromolecular flocculant with a molecular weight of 5 million was 1:3, the sedimentation rate of the red mud sedimentation crude liquid was 27.81m / h, the 5min compression band height was 52mL, and the concentration of the suspended solids was only 0.26g / L. When 85g / t of the small molecule enhancer with a molecular weight of 400,000 was used alone, the red mud sedimentation crude liquid was difficult to settle; when 85g / t of the macromolecular flocculant with a molecular weight of 5 million was used alone, the sedimentation rate was 23.46m / h, the 5min compression band height was 51mL, and the concentration of the suspended solids was 0.45g / L. At this time, the sedimentation rate of the flocculant used on site by an alumina enterprise (the main component of the flocculant is a large molecular weight sodium polyacrylate anionic flocculant with a relatively uniform molecular weight distribution) was 15.08m / h, the 5-minute compression band height was 50mL, and the concentration of suspended matter was 0.87g / L.

[0067] Example 2

[0068] Weigh a polyacrylamide with a molecular weight of 14 million and slowly add it to a beaker containing a certain amount of distilled water under stirring. The concentration is 3.55%. After complete dissolution, transfer the viscous solution to a 250mL three-necked flask, and place the reaction bottle in a constant temperature water bath at a temperature of 50°C. Weigh a certain amount of hydroxylamine hydrochloride and sodium hydroxide in an equal molar ratio and dissolve them in a certain amount of distilled water to obtain a neutralized hydroxylamine solution. Add the hydroxylamine solution to the reaction bottle. The molar ratio of polyacrylamide to hydroxylamine is 1:1.5, and adjust the pH to about 12.5. Stir magnetically, pass 50mL / min high-purity N2 throughout the process, and the reaction time is 10h.

[0069] Weigh acrylamide and slowly add it to a flask containing a certain amount of distilled water under stirring. The concentration of acrylamide is 2.5%. Add 0.1% of initiator: ammonium persulfate and sodium bisulfite. The reaction time is 0.5h. Weigh a certain amount of equimolar ratio of hydroxylamine hydrochloride and sodium hydroxide and dissolve them in a certain amount of distilled water to obtain a neutralized hydroxylamine solution. Add the hydroxylamine solution to the flask. The molar ratio of polyacrylamide to hydroxylamine is 1:1.5. Adjust the pH to about 12.5. Pass 50mL / min of high-purity N2 throughout the process, and the reaction time is 8h. A small molecule enhancer with a molecular weight of about 500,000 was synthesized.

[0070] The two synthetic flocculants are compounded to form a flocculant product with bimodal distribution of size.

[0071] The bimodal distribution flocculant product was subjected to sedimentation test. When the addition amount of bimodal distribution flocculant is 85g / t, the mass ratio of the reinforcing agent with a molecular weight of 500,000 to the macromolecular flocculant with a molecular weight of 14 million is 1:3, the sedimentation velocity is 32.08m / h, the 5-minute compression zone height is 51mL, and the concentration of suspended matter is only 0.20g / L; when 85g / t of a small molecular weight reinforcing agent with a molecular weight of 500,000 is used alone, the crude red mud sedimentation liquid is difficult to settle; when 85g / t of a macromolecular flocculant with a molecular weight of 14 million is used alone, the sedimentation velocity of the crude red mud sedimentation liquid is 28.77m / h, the 5-minute compression zone height is 50mL, and the concentration of suspended matter is 0.39g / L; at this time, the sedimentation velocity of the flocculant used on site of an alumina enterprise (the main component of the flocculant is a macromolecular sodium polyacrylate anionic flocculant with a relatively uniform molecular weight distribution) is 15.08m / h, the 5-minute compression zone height is 50mL, and the concentration of suspended matter is 0.87g / L.

[0072] Example 3

[0073] Weigh a polyacrylamide with a molecular weight of 12 million and slowly add it to a beaker containing a certain amount of distilled water under stirring. The concentration is 3.20%. After complete dissolution, transfer the viscous solution to a 250mL three-necked flask, and place the reaction bottle in a constant temperature water bath at a temperature of 50°C. Weigh a certain amount of hydroxylamine hydrochloride and sodium hydroxide in an equal molar ratio and dissolve them in a certain amount of distilled water to obtain a neutralized hydroxylamine solution. Add the hydroxylamine solution to the reaction bottle. The molar ratio of polyacrylamide to hydroxylamine is 1:1.5, and adjust the pH to about 12.5. Stir magnetically, pass 50mL / min high-purity N2 throughout the process, and the reaction time is 12h.

[0074] Weigh acrylamide and slowly add it to a flask containing a certain amount of distilled water under stirring. The concentration of acrylamide is 2.5%. Add initiators: ammonium persulfate and sodium bisulfite. The concentration of initiator is 0.40%. The reaction time is 0.5h. Weigh a certain amount of hydroxylamine hydrochloride and sodium hydroxide in equal molar ratio and dissolve them in a certain amount of distilled water to obtain a neutralized hydroxylamine solution. Add the hydroxylamine solution to the flask. The molar ratio of acrylamide to hydroxylamine is 1:1.5. Adjust the pH to about 12.5. Pass 50mL / min high-purity N2 throughout the process. The reaction time is 6h. The enhancer with a molecular weight of about 400,000 is synthesized.

[0075] The two synthetic flocculants are compounded to form a flocculant product with bimodal distribution of size.

[0076] The bimodal distribution flocculant product was subjected to a sedimentation test. When the addition amount of the bimodal distribution flocculant was 160g / t, the mass ratio of the reinforcing agent with a molecular weight of 400,000 to the macromolecular flocculant with a molecular weight of 12 million was 1:3, the sedimentation rate was 34.84m / h, the 5-minute compression zone height was 53mL, and the concentration of the suspended solids was 0.32g / L; when 160g / t of the small molecular weight reinforcing agent with a molecular weight of 400,000 was used alone, the red mud sedimentation crude liquid was difficult to settle; when 160g / t of the 12 million molecular weight reinforcing agent was used alone, the red mud sedimentation crude liquid was difficult to settle. When using macromolecular flocculants, the sedimentation velocity of the crude red mud liquid was 32.58 m / h, the 5-min compression zone height was 51 mL, and the concentration of suspended solids was 0.36 g / L; while at this time, the sedimentation velocity of the flocculant used on site by an alumina enterprise (the main component of the flocculant is a macromolecular sodium polyacrylate anionic flocculant with a relatively uniform molecular weight distribution) was 27.05 m / h, the 5-min compression zone height was 51 mL, and the concentration of suspended solids was 0.75 g / L.

[0077] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0078] In the embodiment of the present invention, a macromolecular flocculant (molecular weight ≥ 5 million) is first synthesized by an aqueous solution modification method to ensure a high content of hydroxamic acid groups in the molecule, and then a small molecule enhancer (molecular weight ≤ 600,000) is synthesized by single-molecule polymerization modification of acrylamide. As a sedimentation process enhancer, it helps to capture very fine particles, first granulate, and then produce a flocculation effect through the bridging action of macromolecular flocs, thereby effectively improving and regulating its sedimentation process, and finally forming a high-efficiency flocculant with different molecular weight distributions.

[0079] In the embodiment of the present invention, two flocculants with different molecular weights are selected for combined use according to different red mud compositions. The problem that the extremely fine particles formed after the dissolution of goethite in the sedimentation process are difficult to settle is solved, and the sedimentation efficiency of the flocculant is improved. This method can not only quickly settle, but also make the resulting solution transparent, reduce the content of suspended solids, and is simple and convenient to use with high sedimentation efficiency.

[0080] In the embodiment of the present invention, the sedimentation speed of the red mud sedimentation crude liquid is ≥25m / h, the 5min compression belt height is ≤55mL, and the concentration of suspended matter is ≤0.35g / L. The method of the present invention can quickly and effectively reduce the content of suspended matter in the sedimentation crude liquid, achieve a better sedimentation effect, and can timely guide the production of alumina.

[0081] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A bimodal distribution flocculant, characterized in that: The bimodal distribution flocculant is composed of a macromolecular flocculant and a small molecular enhancer; wherein, The macromolecular flocculant and the small molecule enhancer are both hydroxamic acid flocculants; The molecular weight of the macromolecular flocculant is ≥5 million, and the molecular weight of the small molecule reinforcing agent is ≤600,000.

2. The bimodal distribution flocculant according to claim 1, characterized in that The mass ratio of the macromolecular flocculant to the small molecule reinforcing agent is (1-6):

1.

3. The bimodal distribution flocculant according to claim 2, characterized in that: The mass ratio of the macromolecular flocculant to the small molecule reinforcing agent is (2-4):

1.

4. A method for preparing a bimodal distribution flocculant according to any one of claims 1 to 3, characterized in that: The method comprises: Mixing polyacrylamide with a set molecular weight, a solvent and a hydroxylamine solution, and adjusting the pH to a first set pH, so as to perform a first water bath reaction under a first set reaction condition to obtain a macromolecular flocculant; Mixing acrylamide, a solvent and an initiator to perform a polymerization reaction to obtain a mixed solution; The mixed solution is mixed with a hydroxylamine solution, and the pH is adjusted to a second set pH, so as to perform a second water bath reaction under a second set reaction condition to obtain a small molecule enhancer; The macromolecular flocculant and the small molecule reinforcing agent are compounded to obtain a bimodal distribution flocculant.

5. The method according to claim 4, characterized in that The concentration of the polyacrylamide is 2% to 5%.

6. The method according to claim 4, characterized in that The molar ratio of the polyacrylamide to the hydroxylamine is 1:(1.2-1.8).

7. The method according to claim 4, characterized in that The first set reaction conditions include: the protective atmosphere is nitrogen, the reaction temperature is 50° C. to 80° C., the first set pH is 10 to 13, and the reaction time is 8 h to 20 h.

8. The method according to claim 4, characterized in that The concentration of the acrylamide is 2% to 4%, the concentration of the initiator is 0.3% to 0.6%, and the initiator includes one or more of ammonium persulfate and sodium bisulfite.

9. The method according to claim 4, characterized in that The molar ratio of acrylamide to hydroxylamine is 1:(1.1-1.5).

10. The method according to claim 4, characterized in that The second set reaction conditions include: the protective atmosphere is nitrogen, the reaction temperature is 50° C. to 80° C., the second set pH is 10 to 13, and the reaction time is 5 h to 10 h.

Citation Information

Patent Citations

  • Method for preparing flocculant for efficient settling separation of high-silicon and high-iron type red mud generated through Bayer process

    CN103819592A

  • Method for separating superfine molecular sieve from alkaline superfine molecular sieve synthesis mother liquor

    CN116199234A

  • Preparation method of high-activity and high-stability hydroxamic acid type polyacrylamide inverse emulsion