Preparation method and application of coal gasification grey water dispersing agent

Through the synthesis and dispersion of polyacrylic scale-resistance corrosion inhibitor, the scale-condensation and corrosion problems of gasified ash water are solved, the dispersion and scale-resistance performance is improved, and the cost-effective grey water treatment is achieved.

CN119038769AInactive Publication Date: 2024-11-29RENQIU ANGYU CHEMICAL CO LTD

Patent Information

Application Number
CN202411181761.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing coal gasified ash water dispersants have scaling problems when dealing with coal gasified ash water with high hardness, high alkalinity and high pH, ​​and are insufficient in scale resistance and dispersion performance, and some products have high costs, dust generation and Problem of insufficient corrosiveness.

Method used

Polyacrylic acid scale-resistance corrosion inhibitor is used to synthesize it by reaction under a nitrogen atmosphere, and it is uniformly dispersed with deionized water to form a water-soluble copolymer with strong adsorption and chelation capabilities, and uses the acidity and philtrum of carboxylic acid groups and sulfonic acid groups. The water property improves dispersion properties and prevents particles from coagulation through the repulsion of the quaternary ammonium salt, reducing precipitation.

Benefits of technology

Effectively prevent the tendency of scaling in the gray water system, reduce corrosion to the pipeline, improve dispersion and scale resistance, avoid the formation of new pollution sources, and reduce production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005012380880000051
    Figure BDA0005012380880000051
  • Figure BDA0005012380880000052
    Figure BDA0005012380880000052
  • Figure BDA0005012380880000053
    Figure BDA0005012380880000053
Patent Text Reader

Abstract

The invention relates to the technical field of grey water dispersing agents, and discloses a preparation method and application of a coal gasification grey water dispersing agent. Sulfonic acid groups and carboxylic acid groups in a polyacrylic acid scale and corrosion inhibitor enhance the hydrophilicity of a copolymer, have stronger adsorption and chelation capabilities on iron ions, calcium ions and the like, and prevent suspended particles from being condensed into large particles to be deposited; therefore, the dispersing performance of grey water is improved; a long-chain hydrophobic group in the structure enables anions and cations to have repulsive interaction, so that the probability of mutual collision of precipitated particles can be reduced, and aggregation and precipitation are reduced; meanwhile, N atoms in the naphthenic imidazoline structure have electron donating capacity, can form coordinate bonds with metal to generate chemical adsorption, and are adsorbed on the surface of the metal, so that the activation energy of corrosion reaction is increased, and the corrosion speed is slowed down; and the long-chain alkyl is perpendicular to the metal surface to form a hydrophobic protective film covering the metal surface, so that the corrosion inhibition effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ash water dispersants, and in particular to a preparation method and application of a coal gasification ash water dispersant. Background Art

[0002] Coal gasification ash water is a kind of wastewater generated in the coal gasification process, which mainly comes from the coal gasification furnace and the coal gas preliminary purification system. In the coal chemical industry, the water-coal slurry gasification process uses coal ash with a high melting point. In order to lower the ash melting point of coal, a flux calcium carbonate is added, which decomposes at high temperature to generate calcium oxide. A part of the calcium oxide reacts with silica, alumina, etc. in the coal, lowering the ash melting point of the coal. The remaining calcium oxide dissolves in the coal gas washing water, greatly increasing the calcium hardness and alkalinity in the coal gas washing water, making the ash water a severely scaling water with high hardness, high alkalinity and high pH value. Therefore, a large amount of scaling will occur in the coal gasification ash water system, resulting in system blockage, reduced heat transfer efficiency and increased energy consumption. In order to solve this problem, scale inhibitors and dispersants are usually used to treat the ash water to prevent scaling.

[0003] Coal gasification ash water dispersant is a chemical substance specially used in the coal gasification process to treat ash water and prevent scaling of equipment and pipelines. Existing scale inhibitors still have certain technical problems, such as there are many types of scale inhibitors, the added pure water only accounts for about 30%, and the cost of the agent is relatively high; the production raw materials of some scale inhibitors are solid powder, which is easy to generate dust during the production process, and the mixing time is long, and the production cycle is long; the existing technology scale inhibitors generally only study the scale inhibition performance, and do not study the dispersion performance; the invention patent CN100384762C discloses a polymer ash water stabilizer, which uses a sulfonate copolymer, aminotri(methylenephosphonic acid), hydroxyethyldiphosphonic acid, and polymaleic anhydride for compound use, but because the types and contents of the components are not completely matched, the treatment of some harsh water quality is not ideal, and it has no corrosion inhibition effect, and a large amount of phosphorus-containing compounds will be discharged, forming new pollution.

[0004] Copolymer dispersants are new water treatment agents developed in recent years. Their phosphorus-free formula will not cause secondary pollution, but their single treatment effect is not ideal, the dosage is large and the price is high, which is not economical. Therefore, they are often used in combination with other treatment agents. Therefore, it has become an urgent problem to be solved in coal chemical production to prepare a dispersant that can effectively prevent the scaling tendency in various gray water systems and slow down the scale inhibition, and can slow down the corrosion of the gray water system to the pipeline, and will not form new pollution. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a preparation method and application of a coal gasification ash water dispersant, which has a good dispersing effect on suspended solids in ash water, prevents scaling tendency in the ash water system, reduces corrosion to pipelines, and has excellent corrosion inhibition performance.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] A method for preparing a coal gasification ash water dispersant is carried out according to the following steps:

[0008] 3-15 parts by weight of polyacrylic acid scale inhibitor and corrosion inhibitor are evenly dispersed in 100 parts by weight of deionized water to obtain a coal gasification ash water dispersant.

[0009] The preparation method of the polyacrylic acid scale inhibitor and corrosion inhibitor is as follows: under a nitrogen atmosphere, deionized water, 3-5 parts by weight of initiator ammonium persulfate, 4-6 parts by weight of emulsifier sodium dodecylbenzene sulfonate, and 8-12 parts by weight of OP-10 are added to a reaction bottle equipped with a dropping funnel, and stirred to dissolve; 100 parts by weight of methyl methacrylate, 30-45 parts by weight of butyl acrylate, 10-20 parts by weight of methacrylic acid and 2-10 parts by weight of a uniform mixture of the structural formula are added to the dropping funnel. To the mixture of octadecene imidazoline tribetaine, first add 1 / 3 of the mixture, react at 75-90°C for 1-3h, then add the remaining mixture and 0.5-1.2 parts by weight of NaHCO3 buffer, and continue to react for 2-4h at the same temperature. After the reaction, add ammonia water to adjust the pH to 7-8, and finally add 1-2 parts by weight of defoamer emulsified silicone oil to obtain a polyacrylic acid scale inhibitor.

[0010] Preferably, the preparation method of octadecene imidazoline tribetaine is carried out according to the following steps:

[0011] Step (1), under nitrogen atmosphere, add 3-(dimethylamino)propionic acid and acetonitrile to a reaction flask, stir evenly, add 18-bromo-1-octadecene, stir to react, after the reaction is completed, concentrate under reduced pressure, and purify by column chromatography to obtain an octadecene carboxylic acid intermediate.

[0012] Step (2), under a nitrogen atmosphere, octadecene carboxylic acid quaternary ammonium salt and 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt are added to a reaction flask equipped with a condenser and a water separator, and xylene is used as a water-carrying agent, and the reaction is carried out at 150-170° C. for 5-12 hours until no water flows out of the water separator, and then the temperature is raised to 220-240° C. and distilled under reduced pressure to obtain an octadecene imidazoline intermediate.

[0013] Step (3), under a nitrogen atmosphere, add octadecene imidazoline betaine and N,N-dimethylformamide to a reaction flask, stir evenly, add sodium chloroacetate, stir to react, after the reaction is completed, concentrate under reduced pressure, and purify by column chromatography to obtain octadecene imidazoline tribetaine.

[0014] Preferably, the molar amount of 18-bromo-1-octadecene in step (1) is 110-130% of the molar amount of 3-(dimethylamino)propionic acid.

[0015] Preferably, in step (1), the reaction temperature is 65-80° C. and the reaction time is 24-48 h.

[0016] Preferably, the molar amount of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt in step (2) is 120-150% of the molar amount of octadecenecarboxylic acid quaternary ammonium salt.

[0017] Preferably, the molar amount of sodium chloroacetate in step (3) is 250-320% of the molar amount of octadecene imidazoline betaine.

[0018] Preferably, in step (3), the reaction temperature is 110-130° C. and the reaction time is 3-8 h.

[0019] Preferably, the coal gasification ash water dispersant is used in ash water treatment.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The invention firstly carries out quaternization reaction on 3-(dimethylamino)propionic acid and 18-bromo-1-octadecene to obtain an octadecene carboxylic acid intermediate, then carries out cyclization reaction on 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt to obtain an octadecene imidazoline intermediate, then reacts with sodium chloroacetate to obtain an octadecene imidazoline tribetaine, then polymerizes with monomers such as methyl methacrylate and methacrylic acid to obtain a polyacrylic acid scale inhibitor and corrosion inhibitor, and finally uniformly disperses the polyacrylic acid in deionized water to obtain a coal gasification ash water dispersant.

[0022] The carboxylic acid group in the polyacrylic acid scale inhibitor and corrosion inhibitor has weak acidity and has stronger adsorption and chelating ability for iron ions, calcium ions, etc., and can form a water-soluble chelate with stable structure; the sulfonic acid group has strong acidity and stronger dispersing performance, which helps to dissolve scale. The sulfonic acid group and the carboxylic acid group enhance the hydrophilicity of the copolymer, ensure the long-term effectiveness of the dispersed scale inhibition, and improve the ability to resist cationic precipitation; at the same time, the quaternary ammonium salt cation has a repulsive force on suspended particles with the same positive charge, preventing the suspended particles from condensing into large particles and depositing, thereby improving the dispersion performance of the gray water; on the other hand, the long-chain hydrophobic groups in the polyacrylic acid scale inhibitor make there is a certain repulsive effect between anions and cations, avoiding the precipitation of calcium ions and scaling.

[0023] Polyacrylic acid scale and corrosion inhibitor has the function of adsorption and bridging, making SO4 2- with Ba 2+ , Ca 2+ and HCO3 - There is a certain mutual repulsion, and at the same time, the stretching of its molecular chain can reduce the probability of collision between precipitation particles, reduce aggregation and precipitation, and play a role in dispersing scale inhibition; in addition, the carboxylic acid group and sulfonic acid group in the molecular chain have stronger adsorption and chelating ability for barium ions, calcium ions, etc., and can form a water-soluble chelate with a stable structure, which is helpful for the dissolution of scale and better exerts the scale inhibition performance.

[0024] Polyacrylic acid scale inhibitor contains cycloalkyl imidazoline structure, the N atom in its structure has the ability to donate electrons. Metals such as carbon steel have unoccupied empty d orbitals that are easy to accept electrons, so the heteroatom N can form a coordination bond with the metal to undergo chemical adsorption and adsorption on the metal surface. On the one hand, it changes the charge distribution and interface properties of the metal surface, stabilizing the energy state of the metal surface, thereby increasing the activation energy of the corrosion reaction and slowing down the corrosion rate; on the other hand, the long-chain alkyl in the adsorbed corrosion inhibitor is perpendicular to the metal surface, and can form a hydrophobic protective film covering the metal surface, hindering the transfer of charges or substances related to the corrosion reaction, thereby playing a role in corrosion inhibition. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] 3-(Dimethylamino)propionic acid, CAS number is 6300-04-5.

[0027] 18-Bromo-1-octadecene, CAS number is 172656-11-0.

[0028] 2-[(2-Aminoethyl)amino]ethanesulfonic acid sodium salt, CAS number is 34730-59-1.

[0029] Sodium chloroacetate, CAS number is 3926-62-3.

[0030] Example 1

[0031] (1) Under nitrogen atmosphere, 45 mmol of 3-(dimethylamino)propionic acid and 225 mL of acetonitrile were added to a reaction flask, stirred evenly, and then 54 mmol of 18-bromo-1-octadecene was added. The mixture was reacted at 70° C. for 32 h, concentrated under reduced pressure, and purified by column chromatography. The eluent was ethyl acetate and petroleum ether in a ratio of 1:5 to obtain an octadecene carboxylic acid intermediate. The preparation reaction formula is as follows:

[0032]

[0033] (2) Under nitrogen atmosphere, 40 mmol of quaternary ammonium salt of octadecene carboxylic acid and 55 mmol of sodium salt of 2-[(2-aminoethyl)amino]ethanesulfonic acid were added to a reaction flask equipped with a condenser and a water separator, and xylene was used as a water-carrying agent. The mixture was reacted at 160° C. for 8 h until no water flowed out of the water separator. The mixture was then heated to 230° C. and distilled under reduced pressure to obtain an octadecene imidazoline intermediate. The preparation reaction formula is as follows:

[0034]

[0035] (3) Under nitrogen atmosphere, 35 mmol of octadecene imidazoline betaine and 630 mL of N,N-dimethylformamide were added to the reaction flask, stirred evenly, and then 98 mmol of sodium chloroacetate was added. The mixture was reacted at 120° C. for 5 h, concentrated under reduced pressure, and purified by column chromatography. The eluent was ethyl acetate and petroleum ether in a ratio of 1:3 to obtain octadecene imidazoline tribetaine. The preparation reaction formula is as follows:

[0036]

[0037] (4) Under nitrogen atmosphere, 25 g of deionized water, 4 g of initiator ammonium persulfate, 5 g of emulsifier sodium dodecylbenzene sulfonate, and 10 g of OP-10 were added to a reaction bottle equipped with a dropping funnel, and stirred to dissolve; a mixture of 100 g of methyl methacrylate, 35 g of butyl acrylate, 15 g of methacrylic acid, and 2 g of octadecene imidazoline tribetaine was added to the dropping funnel, 1 / 3 of the mixture was first added dropwise, and the mixture was reacted at 80° C. for 2 h, and then the remaining mixture and 0.9 g of NaHCO3 buffer were added dropwise, and the reaction was continued at the same temperature for 3 h. After the reaction was completed, ammonia water was added to adjust the pH to 8, and finally 1.5 g of defoaming agent emulsified silicone oil was added to obtain a polyacrylic acid scale inhibitor and corrosion inhibitor, and 3 g of the polyacrylic acid scale inhibitor and corrosion inhibitor were evenly dispersed in 100 g of deionized water to obtain a coal gasification ash water dispersant.

[0038] Example 2

[0039] (1) Under nitrogen atmosphere, 80 mmol of 3-(dimethylamino)propionic acid and 400 mL of acetonitrile were added to a reaction flask, stirred evenly, and then 88 mmol of 18-bromo-1-octadecene was added. The mixture was reacted at 80° C. for 24 h, concentrated under reduced pressure, and purified by column chromatography. The eluent was ethyl acetate and petroleum ether in a ratio of 1:5 to obtain an octadecene carboxylic acid intermediate.

[0040] (2) Under a nitrogen atmosphere, 75 mmol of quaternary ammonium salt of octadecene carboxylic acid and 90 mmol of sodium salt of 2-[(2-aminoethyl)amino]ethanesulfonic acid were added to a reaction flask equipped with a condenser and a water separator, and xylene was used as a water carrier. The mixture was reacted at 170° C. for 5 h until no water flowed out of the water separator. The mixture was then heated to 240° C. and distilled under reduced pressure to obtain an octadecene imidazoline intermediate.

[0041] (3) Under nitrogen atmosphere, 70 mmol of octadecene imidazoline betaine and 1050 mL of N,N-dimethylformamide were added to a reaction flask, stirred evenly, and then 175 mmol of sodium chloroacetate was added. The mixture was reacted at 130° C. for 3 h, concentrated under reduced pressure, and purified by column chromatography. The eluent was ethyl acetate and petroleum ether in a ratio of 1:3 to obtain octadecene imidazoline tribetaine.

[0042] (4) Under nitrogen atmosphere, 20 g of deionized water, 5 g of initiator ammonium persulfate, 4 g of emulsifier sodium dodecylbenzene sulfonate, and 8 g of OP-10 were added to a reaction bottle equipped with a dropping funnel, and stirred to dissolve; a uniformly mixed solution of 100 g of methyl methacrylate, 30 g of butyl acrylate, 10 g of methacrylic acid, and 4 g of octadecene imidazoline tribetaine was added to the dropping funnel, 1 / 3 of the mixture was first added dropwise, and the mixture was reacted at 90° C. for 1 h, and then the remaining mixture and 0.5 g of NaHCO3 buffer were added dropwise, and the reaction was continued at the same temperature for 3 h. After the reaction was completed, ammonia water was added to adjust the pH to 7, and finally 1 g of defoaming agent emulsified silicone oil was added to obtain a polyacrylic acid scale inhibitor and corrosion inhibitor, and 6 g of the polyacrylic acid scale inhibitor and corrosion inhibitor were uniformly dispersed in 100 g of deionized water to obtain a coal gasification ash water dispersant.

[0043] Example 3

[0044] (1) Under nitrogen atmosphere, 35 mmol of 3-(dimethylamino)propionic acid and 350 mL of acetonitrile were added to a reaction flask, stirred evenly, and then 45.5 mmol of 18-bromo-1-octadecene was added. The mixture was reacted at 65° C. for 48 h, concentrated under reduced pressure, and purified by column chromatography with an eluent of ethyl acetate and petroleum ether in a ratio of 1:5 to obtain an octadecene carboxylic acid intermediate.

[0045] (2) Under a nitrogen atmosphere, 32 mmol of quaternary ammonium salt of octadecene carboxylic acid and 48 mmol of sodium salt of 2-[(2-aminoethyl)amino]ethanesulfonic acid were added to a reaction flask equipped with a condenser and a water separator, and xylene was used as a water carrier. The mixture was reacted at 150° C. for 12 h until no water flowed out of the water separator. The mixture was then heated to 220° C. and distilled under reduced pressure to obtain an octadecene imidazoline intermediate.

[0046] (3) Under nitrogen atmosphere, 30 mmol of octadecene imidazoline betaine and 600 mL of N,N-dimethylformamide were added to a reaction flask, stirred evenly, and then 96 mmol of sodium chloroacetate was added. The mixture was reacted at 110° C. for 8 h, concentrated under reduced pressure, and purified by column chromatography. The eluent was ethyl acetate and petroleum ether in a ratio of 1:3 to obtain octadecene imidazoline tribetaine.

[0047] (4) Under nitrogen atmosphere, 30 g of deionized water, 5 g of initiator ammonium persulfate, 6 g of emulsifier sodium dodecylbenzene sulfonate, and 12 g of OP-10 were added to a reaction bottle equipped with a dropping funnel, and stirred to dissolve; a uniformly mixed solution of 100 g of methyl methacrylate, 45 g of butyl acrylate, 20 g of methacrylic acid, and 6 g of octadecene imidazoline tribetaine was added to the dropping funnel, 1 / 3 of the mixture was first added dropwise, and the mixture was reacted at 75° C. for 3 h, and then the remaining mixture and 1.2 g of NaHCO3 buffer were added dropwise, and the reaction was continued at the same temperature for 4 h. After the reaction was completed, ammonia water was added to adjust the pH to 8, and finally 2 g of defoamer emulsified silicone oil was added to obtain a polyacrylic acid scale inhibitor and corrosion inhibitor, and 9 g of the polyacrylic acid scale inhibitor and corrosion inhibitor were uniformly dispersed in 100 g of deionized water to obtain a coal gasification ash water dispersant.

[0048] Example 4

[0049] (1) Under nitrogen atmosphere, 50 mmol of 3-(dimethylamino)propionic acid and 460 mL of acetonitrile were added to a reaction flask, stirred evenly, and then 58 mmol of 18-bromo-1-octadecene was added. The mixture was reacted at 75° C. for 42 h, concentrated under reduced pressure, and purified by column chromatography with an eluent of ethyl acetate and petroleum ether in a ratio of 1:5 to obtain an octadecene carboxylic acid intermediate.

[0050] (2) Under nitrogen atmosphere, 42 mmol of quaternary ammonium salt of octadecene carboxylate and 60.9 mmol of sodium salt of 2-[(2-aminoethyl)amino]ethanesulfonic acid were added to a reaction flask equipped with a condenser and a water separator, and xylene was used as a water carrier. The mixture was reacted at 165° C. for 10 h until no water flowed out of the water separator. The mixture was then heated to 235° C. and distilled under reduced pressure to obtain an octadecene imidazoline intermediate.

[0051] (3) Under nitrogen atmosphere, 40 mmol of octadecene imidazoline betaine and 660 mL of N,N-dimethylformamide were added to a reaction flask, stirred evenly, and then 106 mmol of sodium chloroacetate was added. The mixture was reacted at 125° C. for 6 h, concentrated under reduced pressure, and purified by column chromatography. The eluent was ethyl acetate and petroleum ether in a ratio of 1:3 to obtain octadecene imidazoline tribetaine.

[0052] (4) Under nitrogen atmosphere, 28 g of deionized water, 3.5 g of initiator ammonium persulfate, 5 g of emulsifier sodium dodecylbenzene sulfonate, and 11 g of OP-10 were added to a reaction bottle equipped with a dropping funnel, and stirred to dissolve; a uniformly mixed solution of 100 g of methyl methacrylate, 40 g of butyl acrylate, 12 g of methacrylic acid, and 8 g of octadecene imidazoline tribetaine was added to the dropping funnel, 1 / 3 of the mixture was first added dropwise, and the mixture was reacted at 85° C. for 2 h, and then the remaining mixture and 0.8 g of NaHCO3 buffer were added dropwise, and the reaction was continued at the same temperature for 3 h. After the reaction was completed, ammonia water was added to adjust the pH to 7, and finally 1.5 g of defoamer emulsified silicone oil was added to obtain a polyacrylic acid scale inhibitor and corrosion inhibitor, and 12 g of the polyacrylic acid scale inhibitor and corrosion inhibitor were uniformly dispersed in 100 g of deionized water to obtain a coal gasification ash water dispersant.

[0053] Example 5

[0054] (1) Under nitrogen atmosphere, 25 mmol of 3-(dimethylamino)propionic acid and 195 mL of acetonitrile were added to a reaction flask, stirred evenly, and then 30.5 mmol of 18-bromo-1-octadecene was added. The mixture was reacted at 70° C. for 48 h, concentrated under reduced pressure, and purified by column chromatography with an eluent of ethyl acetate and petroleum ether in a ratio of 1:5 to obtain an octadecene carboxylic acid intermediate.

[0055] (2) Under a nitrogen atmosphere, 20 mmol of quaternary ammonium salt of octadecene carboxylic acid and 29 mmol of sodium salt of 2-[(2-aminoethyl)amino]ethanesulfonic acid were added to a reaction flask equipped with a condenser and a water separator, and xylene was used as a water carrier. The mixture was reacted at 165° C. for 12 h until no water flowed out of the water separator. The mixture was then heated to 235° C. and distilled under reduced pressure to obtain an octadecene imidazoline intermediate.

[0056] (3) Under nitrogen atmosphere, 15 mmol of octadecene imidazoline betaine and 240 mL of N,N-dimethylformamide were added to a reaction flask, stirred evenly, and then 42 mmol of sodium chloroacetate was added. The mixture was reacted at 130° C. for 8 h, concentrated under reduced pressure, and purified by column chromatography. The eluent was ethyl acetate and petroleum ether in a ratio of 1:3 to obtain octadecene imidazoline tribetaine.

[0057] (4) Under nitrogen atmosphere, 30 g of deionized water, 4 g of initiator ammonium persulfate, 6 g of emulsifier sodium dodecylbenzene sulfonate, and 9 g of OP-10 were added to a reaction bottle equipped with a dropping funnel, and stirred to dissolve; a uniformly mixed solution of 100 g of methyl methacrylate, 42 g of butyl acrylate, 15 g of methacrylic acid and 10 g of octadecene imidazoline tribetaine was added to the dropping funnel, 1 / 3 of the mixture was first added dropwise, and the mixture was reacted at 90° C. for 2 h, and then the remaining mixture and 0.8 g of NaHCO3 buffer were added dropwise, and the reaction was continued at the same temperature for 4 h. After the reaction was completed, ammonia water was added to adjust the pH to 8, and finally 1.2 g of defoaming agent emulsified silicone oil was added to obtain a polyacrylic acid scale inhibitor and corrosion inhibitor, and 15 g of the polyacrylic acid scale inhibitor and corrosion inhibitor were uniformly dispersed in 100 g of deionized water to obtain a coal gasification ash water dispersant.

[0058] Comparative Example 1

[0059] Under a nitrogen atmosphere, 25 g of deionized water, 4 g of initiator ammonium persulfate, 5 g of emulsifier sodium dodecylbenzene sulfonate, and 10 g of OP-10 were added to a reaction bottle equipped with a dropping funnel, and stirred to dissolve; a mixture of 100 g of methyl methacrylate, 35 g of butyl acrylate, 15 g of methacrylic acid and 2 g of octadecene carboxylic acid intermediate (prepared in Example 1) was added to the dropping funnel, 1 / 3 of the mixture was first added dropwise, and the reaction was carried out at 80° C. for 2 h, and then the remaining mixture and 0.9 g of NaHCO3 buffer were added dropwise. At the same temperature, the reaction was continued for 3 h. After the reaction was completed, ammonia water was added to adjust the pH to 8, and finally 1.5 g of defoamer emulsified silicone oil was added to obtain a polyacrylic acid scale inhibitor and corrosion inhibitor. 3 g of the polyacrylic acid scale inhibitor and corrosion inhibitor were evenly dispersed in 100 g of deionized water to obtain a coal gasification ash water dispersant.

[0060] Comparative Example 2

[0061] Under a nitrogen atmosphere, 25 g of deionized water, 4 g of initiator ammonium persulfate, 5 g of emulsifier sodium dodecylbenzene sulfonate, and 10 g of OP-10 were added to a reaction bottle equipped with a dropping funnel, and stirred to dissolve; a mixture of 100 g of methyl methacrylate, 35 g of butyl acrylate, 15 g of methacrylic acid and 2 g of octadecene imidazoline intermediate (prepared in Example 1) was added to the dropping funnel, 1 / 3 of the mixture was first added dropwise, and the reaction was carried out at 80° C. for 2 h, and then the remaining mixture and 0.9 g of NaHCO3 buffer were added dropwise. At the same temperature, the reaction was continued for 3 h. After the reaction was completed, ammonia water was added to adjust the pH to 8, and finally 1.5 g of defoamer emulsified silicone oil was added to obtain a polyacrylic acid scale inhibitor and corrosion inhibitor. 3 g of the polyacrylic acid scale inhibitor and corrosion inhibitor were evenly dispersed in 100 g of deionized water to obtain a coal gasification ash water dispersant.

[0062] Comparative Example 3

[0063] Under a nitrogen atmosphere, 25 g of deionized water, 4 g of initiator ammonium persulfate, 5 g of emulsifier sodium dodecylbenzene sulfonate, and 10 g of OP-10 were added to a reaction bottle equipped with a dropping funnel, and stirred to dissolve; a uniformly mixed solution of 100 g of methyl methacrylate, 35 g of butyl acrylate, and 15 g of methacrylic acid was added to the dropping funnel, 1 / 3 of the mixture was first added dropwise, and the reaction was carried out at 80°C for 2 h, and then the remaining mixture and 0.9 g of NaHCO3 buffer were added dropwise, and the reaction was continued for 3 h at the same temperature. After the reaction was completed, ammonia water was added to adjust the pH to 8, and finally 1.5 g of defoaming agent emulsified silicone oil was added to obtain a polyacrylic acid scale inhibitor and corrosion inhibitor, and 3 g of the polyacrylic acid scale inhibitor and corrosion inhibitor were uniformly dispersed in 100 g of deionized water to obtain a coal gasification ash water dispersant.

[0064] Dispersion performance test: 8 groups of Ca 2+ The solution with a mass concentration of 150 mg / L was added with 100 mg / L of the coal gasification ash water dispersant prepared in the examples and comparative examples, and ferrous sulfate heptahydrate was added to make Fe 2+ The concentration of 10 mg / L was adjusted to 500 mL, and a blank test was performed at the same time; the pH value of the solution was adjusted to 9 with sodium tetraborate; when the pH value was stable, it was stirred vigorously for 15 minutes, and then allowed to stand in a 50°C water bath for 5 hours, and the upper clear liquid was taken, and the transmittance T at 420 nm and 3 cm colorimetric cell was measured with a visible light spectrophotometer.

[0065] Table 1 Dispersion performance test

[0066] Transmittance T(%) Example 1 60.4 Example 2 55.1 Example 3 51.4 Example 4 47.3 Example 5 45.5 Comparative Example 1 71.0 Comparative Example 2 62.9 Comparative Example 3 84.2

[0067] The transmittance reflects the turbidity of the solution. The transmittance can be used to evaluate the performance of the polymer in dispersing iron oxide. Ferrous sulfate heptahydrate produces ferrous hydroxide in an alkaline solution and is then oxidized to iron oxide. If the polymer has poor dispersibility, the iron oxide will precipitate and the transmittance of the solution will be large. On the contrary, the smaller the transmittance, the better the dispersibility of the polymer. It can be seen from the test results in the above table that with the increase of the content of the polyacrylic acid scale inhibitor, the dispersibility of the coal gasification ash water dispersant gradually increases. The transmittance in Example 5 is only 45.5%, indicating that the dispersibility of iron oxide is good. This is because, on the one hand, the acidity of the carboxylic acid group in the polyacrylic acid scale inhibitor is weak. , it has stronger adsorption and chelating ability for iron ions, calcium ions, etc., and can form a water-soluble chelate with stable structure; the sulfonic acid group is more acidic and has stronger dispersing performance, which is helpful for scale dissolution. The sulfonic acid group and the carboxylic acid group enhance the hydrophilicity of the copolymer, ensure the long-term effectiveness of dispersion and scale inhibition, and improve the ability to resist cationic precipitation; at the same time, the quaternary ammonium salt cation has a repulsive force on suspended particles with the same positive charge, preventing the suspended particles from condensing into large particles and depositing, thereby improving the dispersion performance of the gray water; on the other hand, the long-chain hydrophobic groups in the polyacrylic acid scale and corrosion inhibitor make there is a certain repulsion between anions and cations, avoiding the precipitation and scaling of calcium ions.

[0068] Comparative Example 1 does not contain sulfonic acid groups, has limited adsorption and chelation properties for metal cations, and has a high light transmittance; Comparative Example 2 contains both carboxylic acid groups and sulfonic acid groups and long hydrophobic chains, and has better dispersibility; Comparative Example 3 does not contain the prepared octadecene imidazoline tribetaine, and has the worst dispersibility.

[0069] Scale inhibition performance test: The test was conducted in accordance with standard HG / T 2024-2009. The principle of the method is that a certain amount of CaCl2 and BaCl2 reacts with a certain amount of NaHCO3 or Na2SO4 to form CaCO3 and BaSO4 precipitation. Before the reaction to form CaCO3 and BaSO4 precipitation, the prepared coal gasification dispersant and the unprepared coal gasification dispersant are added to the solution, and the solution is kept at a constant temperature for a period of time to determine the Ca content in the clear solution. 2+ and Ba 2+ Content, calculate the scale inhibition rate.

[0070] Preparation of CaCl2 solution: weigh 13.86g of anhydrous calcium chloride and dissolve it in water. 2+ 5mg / mL).

[0071] Preparation of NaHCO3 solution: weigh 9.92g of NaHCO3 and dissolve it in water. - Total 7.29 mg / mL).

[0072] Disodium ethylenediaminetetraacetic acid (EDTA) solution: 0.01 mol / L standard solution.

[0073] Calcium indicator: 0.2g calcium carboxylic acid is thoroughly mixed with 100g calcium chloride and ground to 40-50 mesh.

[0074] Test steps: Add 200mL of deionized water to a 250mL volumetric flask, and use a burette to add 10mL of 5mg / mL Ca 2+ The solution was added with 0.1 g of the coal gasification ash water dispersant prepared in the examples and comparative examples, and after being shaken well, 10 mL of HCO3 with a mass concentration of 7.29 mg / mL was added. - Solution was diluted to the mark with deionized water, shaken, and placed in a 250 mL stoppered conical flask and allowed to stand at 70 °C for 10 h. During the experiment, an experiment without adding dispersant was carried out at the same time, and the other steps were the same to obtain a blank solution 1.

[0075] The experiment was carried out without adding HCO3 - For the experiment of solution and dispersant, the rest of the steps are the same to obtain blank solution 2; take out each stoppered conical flask and let it stand to room temperature, take 50mL of deionized water into a clean conical flask, accurately transfer 25mL of filtrate, mix well, add 10mL of 4% sodium hydroxide solution and 3mL of calcium indicator, and add 0.01mol / L EDTA standard solution until it turns pure blue.

[0076] Scale inhibition rate = [ρ(Ca 2+ 2)-ρ(Ca 2+ 1)] / [ρ(Ca 2+ )-ρ(Ca 2+ 1)]×100%.

[0077] Where ρ(Ca 2+ ) is Ca added as coal gasification dispersant 2+ concentration, ρ(Ca 2+ 1) is the Ca in blank solution 1 2+ concentration, ρ(Ca 2+ 2) is the Ca in blank solution 2 2+ concentration.

[0078] BaSO4 scale inhibition test: add 200mL of deionized water to a 250mL volumetric flask, and use a burette to add 5mL of BaSO4 with a mass concentration of 2.81mg / mL. 2+ Solution, add 0.1g of coal gasification ash water dispersant prepared in the examples and comparative examples, shake well and add 5mL of SO4 with a mass concentration of 2.06mg / mL 2-solution, add deionized water to dilute to the mark, shake well, put into a 250mL stoppered conical flask, and let stand at 70℃ for 10h; the experiment without adding dispersant was carried out at the same time, and the other steps were the same to obtain blank solution 1; the experiment without adding SO4 2- The remaining steps of the experiment of solution and dispersant were the same to obtain blank solution 2.

[0079] Table 2 Scale inhibition performance test

[0080] Calcium carbonate resistance rate (%) Barium sulfate inhibition rate (%) Example 1 90.2 85.1 Example 2 93.1 89.2 Example 3 95.4 92.4 Example 4 98.0 95.3 Example 5 98.5 96.8 Comparative Example 1 65.1 60.7 Comparative Example 2 78.2 73.5 Comparative Example 3 53.6 45.6

[0081] From the test results in the above table, it can be seen that with the increase of the content of polyacrylic acid scale inhibitor, the scale inhibition performance of the coal gasification ash water dispersant is gradually enhanced. In implementation 4, the scale inhibition rate for calcium carbonate reaches 98.0%, and the scale inhibition rate for barium sulfate reaches 96.8%, indicating that the prepared polyacrylic acid scale inhibitor has the effect of adsorption and bridging, making SO4 2- with Ba 2+ , Ca 2 + and HCO3 - There is a certain mutual repulsion, and at the same time, the stretching of its molecular chain can reduce the probability of collision between precipitation particles, reduce aggregation and precipitation, and play a role in dispersing scale inhibition; in addition, the carboxylic acid group and sulfonic acid group in the molecular chain have stronger adsorption and chelating ability for barium ions, calcium ions, etc., and can form a water-soluble chelate with a stable structure, which is helpful for the dissolution of scale and better exerts the scale inhibition performance.

[0082] Corrosion inhibition performance test: According to GB / T 18175-2000 "Determination of corrosion inhibition performance of water treatment agents - Rotating coupon method", a 2000mL beaker was used, 1500mL of a 9.6% hydrochloric acid solution was added to each beaker, and then the coal gasification dispersants prepared in the examples and comparative examples were added respectively, and the beakers were placed in a rotating coupon corrosion tester. Standard carbon steel coupons and copper coupons were used in the experiment, and the test was run at 25°C and 75r / min for 8h. The corrosion inhibition rates of carbon steel and copper were calculated by the weight loss method.

[0083] Table 3 Corrosion inhibition performance test

[0084]

[0085] It can be seen from the test results in the above table that with the increase of the content of polyacrylic acid scale inhibitor and corrosion inhibitor, the corrosion inhibition performance of the coal gasification ash water dispersant is gradually enhanced, and it has a certain corrosion inhibition effect on carbon steel and copper; this is because the polyacrylic acid scale inhibitor and corrosion inhibitor contains a cycloalkyl imidazoline structure, and the N atom in its structure has the ability to donate electrons. Metals such as carbon steel have unoccupied empty d orbitals that are easy to accept electrons, so the heteroatom N can form a coordination bond with the metal to undergo chemical adsorption and adsorb on the metal surface. On the one hand, it changes the charge distribution and interface properties of the metal surface, stabilizes the energy state of the metal surface, thereby increasing the activation energy of the corrosion reaction and slowing down the corrosion rate; on the other hand, the long-chain alkyl in the adsorbed corrosion inhibitor is perpendicular to the metal surface, and can form a hydrophobic protective film covering the metal surface, hindering the transfer of charges or substances related to the corrosion reaction, thereby playing a role in corrosion inhibition; Comparative Examples 1 and 3 do not contain alkyl imidazoline structures and do not have corrosion inhibition performance.

[0086] The above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing a coal gasification ash water dispersant, It is characterized in that The preparation method is carried out according to the following steps: Dispersing 3-15 parts by weight of polyacrylic acid scale inhibitor and corrosion inhibitor uniformly in 100 parts by weight of deionized water to obtain a coal gasification ash water dispersant; The preparation method of the polyacrylic acid scale inhibitor and corrosion inhibitor comprises: adding deionized water, 3-5 parts by weight of initiator ammonium persulfate, 4-6 parts by weight of emulsifier sodium dodecylbenzene sulfonate, and 8-12 parts by weight of OP-10 to a reaction bottle equipped with a dropping funnel under a nitrogen atmosphere, and stirring to dissolve; adding 100 parts by weight of methyl methacrylate, 30-45 parts by weight of butyl acrylate, 10-20 parts by weight of methacrylic acid and 2-10 parts by weight of a uniformly mixed solution of the structural formula 1 / 3 of the mixture of octadecene imidazoline tribetaine was first added dropwise, and the mixture was reacted at 75-90°C for 1-3h, and then the remaining mixture and 0.5-1.2 parts by weight of NaHCO were added dropwise. 3 Buffer, at the same temperature, continue to react for 2-4 hours. After the reaction is completed, add ammonia water to adjust the pH to 7-8, and finally add 1-2 parts by weight of defoamer emulsified silicone oil to obtain a polyacrylic acid scale inhibitor.

2. The method for preparing the coal gasification ash water dispersant according to claim 1, It is characterized in that The preparation method of the octadecene imidazoline tribetaine is carried out according to the following steps: Step (1), under a nitrogen atmosphere, add 3-(dimethylamino)propionic acid and acetonitrile to a reaction flask, stir evenly, add 18-bromo-1-octadecene, stir to react, and after the reaction is completed, concentrate under reduced pressure, and purify by column chromatography to obtain an octadecene carboxylic acid intermediate; Step (2), under a nitrogen atmosphere, adding octadecene carboxylic acid quaternary ammonium salt and 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt to a reaction flask equipped with a condenser and a water separator, using xylene as a water-carrying agent, reacting at 150-170° C. for 5-12 hours until no water flows out of the water separator, then heating to 220-240° C. and distilling under reduced pressure to obtain an octadecene imidazoline intermediate; Step (3), under a nitrogen atmosphere, add octadecene imidazoline betaine and N,N-dimethylformamide to a reaction flask, stir evenly, add sodium chloroacetate, stir to react, after the reaction is completed, concentrate under reduced pressure, and purify by column chromatography to obtain octadecene imidazoline tribetaine.

3. The method for preparing the coal gasification ash water dispersant according to claim 2, It is characterized in that The molar amount of 18-bromo-1-octadecene in step (1) is 110-130% of the molar amount of 3-(dimethylamino)propionic acid.

4. The method for preparing the coal gasification ash water dispersant according to claim 2, It is characterized in that In the step (1), the reaction temperature is 65-80° C. and the reaction time is 24-48 hours.

5. The method for preparing the coal gasification ash water dispersant according to claim 2, It is characterized in that The molar amount of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt in step (2) is 120-150% of the molar amount of octadecenecarboxylic acid quaternary ammonium salt.

6. The method for preparing the coal gasification ash water dispersant according to claim 2, It is characterized in that The molar amount of sodium chloroacetate in step (3) is 250-320% of the molar amount of octadecene imidazoline betaine.

7. The method for preparing the coal gasification ash water dispersant according to claim 2, It is characterized in that In the step (3), the reaction temperature is 110-130° C. and the reaction time is 3-8 h.

8. Use of the coal gasification ash water dispersant obtained by the preparation method according to any one of claims 1 to 7 in ash water treatment.

Citation Information

Patent Citations

  • Polymer grey-water stabilizer

    CN100384762C

Cited By

  • Bactericidal corrosion inhibitor with oil displacement effect and preparation method thereof

    CN122405252A