Cement-based polymer waterproof mortar and preparation method thereof

By using hydrophobic modified zeolite and silane coupling agent to form a hydrophobic layer, and combining polymer monomers and photoinitiators to form a hyperbranched structure, the contradiction between the strength and impermeability of the polymer waterproof mortar is solved, and the compressive strength and resistance are significantly improved. Folding strength and impermeability enhance flexibility.

CN119038923AInactive Publication Date: 2024-11-29TAIXING FUTURE BUILDING MATERIALS TECH DEV CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411159706.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

When the existing polymer waterproof mortar increases strength, its anti-seepage properties and flexibility often decrease, and the water absorption of zeolite affects its anti-seepage properties.

Method used

Modified by hydrophobic modified zeolite and silane coupling agent to form a hydrophobic layer, reduce the porosity of the zeolite, and form a hyperbranched structure by polymerizing monomers and photoinitiators to improve the compressive strength, flexural strength and permeability of the mortar .

Benefits of technology

The compressive strength, flexural strength and permeability of cement-based polymer waterproof mortar are significantly improved, the water absorption rate is reduced, the flexibility is enhanced, and the strength decrease caused by conventional initiators is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005006088450000101
    Figure BDA0005006088450000101
Patent Text Reader

Abstract

The invention discloses cement-based polymer waterproof mortar and a preparation method thereof, and relates to the technical field of building materials. The cement-based polymer waterproof mortar comprises a first liquid material, a second liquid material and a powder material, the first liquid material comprises styrene-butadiene emulsion, water and a defoaming agent; the second liquid material comprises a polymeric monomer, an emulsifier, a water-based photoinitiator and water; the polymeric monomers comprise bis (glycerol carbonate) octylene diformate, 2, 4, 6-triallyloxy-1, 3, 5-triazine, sodium p-styrenesulfonate and hydroxyethyl methylacrylate; the powder material comprises cement, sand, fly ash, hydrophobic modified zeolite, cellulose ether, a dry powder water reducing agent and a dry powder defoaming agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a cement-based polymer waterproof mortar and a preparation method thereof. Background Art

[0002] With the advancement of construction technology, a new type of chemical building material is being applied and developed in China's construction industry at a rapid speed. This is polymer cement-based composite materials, and an important type of them is polymer waterproof mortar. Because polymer molecules have strong diffusion ability, they can penetrate into the pores and cracks on the surface of the base material and block the gaps. The filaments produced when the emulsion condenses can produce a bridging effect between the mortar and the matrix to form a mechanical bond. The polymer forms a film with high bonding force between the cement paste and the aggregate, and blocks the pores in the mortar, thereby greatly improving the performance of the mortar.

[0003] The comprehensive technical performance of polymer-modified waterproof mortar is good and the development prospects are optimistic. However, the mortar used in the project can only meet the requirements of a specific function. The improvement of a certain performance may lead to the decline of other performances. In particular, the problem of low strength in some research practices is more prominent. Therefore, how to improve the strength of mortar is still a concern for polymer waterproof mortar researchers.

[0004] Research has shown that adding some inorganic fillers to polymers can improve and enhance the properties of composite materials to a certain extent. Some technicians have used zeolites with porous lattice crystal structures to improve the performance of polymer waterproof mortars. However, zeolites have a large number of active components on their surface, and have adsorption and ion exchange properties, and have good water absorption effects, which can easily affect the anti-seepage performance of mortars.

[0005] Therefore, the applicant prepared a cement-based polymer waterproof mortar to solve the above problems. Summary of the invention

[0006] In order to solve the existing technical problems, the present invention provides a cement-based polymer waterproof mortar, comprising a first liquid material, a second liquid material and a powder material; the first liquid material comprises, by weight: 50 to 70 parts by weight of styrene-butadiene emulsion, 15 to 25 parts by weight of water, and 0.2 to 0.5 parts by weight of a defoamer; the defoamer is a defoamer FoamStarST2438;

[0007] The second liquid material comprises, by weight, 25 to 35 parts by weight of polymerizable monomers, 6 to 11 parts by weight of emulsifiers, 0.5 to 4 parts by weight of aqueous photoinitiators, and 5 to 15 parts by weight of water; the aqueous initiator is any one of aqueous photoinitiator 2959 and aqueous photoinitiator TPO-1; the emulsifier is emulsifier OP-10;

[0008] The powder material comprises 100 parts by mass of cement, 300 parts by mass of sand, 0.25 parts by mass of fly ash, 32-40 parts by mass of hydrophobically modified zeolite, 1 part by mass of cellulose ether, 0.2 parts by mass of dry powder water reducing agent, and 0.2 parts by mass of dry powder defoaming agent.

[0009] Furthermore, the mass ratio of the first liquid material, the second liquid material and the powder material is 1:0.5:4.2.

[0010] Furthermore, the polymerization monomers include bis(glycerol carbonate) octenedicarboxylate, 2,4,6-triallyloxy-1,3,5-triazine, sodium p-styrene sulfonate, and hydroxyethyl methacrylate.

[0011] Furthermore, the hydrophobically modified zeolite is obtained by immersing zeolite in a silane emulsion, filtering, drying and grinding.

[0012] Furthermore, the silane emulsion is obtained by mixing γ-aminopropyltriethoxysilane, polyvinyl alcohol, isobutyltriethoxysilane, a composite emulsification system of Span 80 and OP-10, and water.

[0013] The present invention also provides a method for preparing a cement-based polymer waterproof mortar, comprising the following preparation steps:

[0014] (1) 100 parts by mass of cement, 300 parts by mass of sand, 0.25 parts by mass of fly ash, 1 part by mass of cellulose ether, 0.2 parts by mass of dry powder water reducing agent, and 0.2 parts by mass of dry powder defoaming agent were stirred and mixed to obtain a premixed powder;

[0015] (2) 50 to 70 parts by weight of styrene butadiene emulsion and 15 to 25 parts by weight of water are stirred and mixed at 300 r / min for 1 to 3 minutes, and then 0.2 to 0.5 parts by weight of a defoamer is added, and the stirring and mixing is continued for 1 to 3 minutes to obtain a first liquid material;

[0016] (3) Under light-proof conditions, 25 to 35 parts by weight of polymerizable monomer, 6 to 11 parts by weight of emulsifier, and 5 to 15 parts by weight of water were stirred and mixed at 300 r / min for 1 to 3 minutes, and then 0.5 to 4 parts by weight of aqueous photoinitiator were added, and the stirring and mixing was continued for 1 to 3 minutes to obtain a second liquid material;

[0017] (4) 32 to 40 parts by weight of the hydrophobically modified zeolite and the second liquid material are stirred at 1500 to 1800 r / min for 10 to 20 minutes, and then 0.03 times of 1,5,7-triazabicyclo[4,4,0]dec-5-ene in the second liquid material is added, the temperature is raised to 140° C., and the reaction is stirred for 18 to 24 hours. During this period, water is continuously added to ensure that the mass of the water is 3.8 times that of the hydrophobically modified zeolite. After naturally cooling to room temperature, a premix is ​​obtained;

[0018] (5) The premixed powder and the first liquid material are mixed, stirred at 100 to 300 r / min for 5 to 7 minutes, and then the premix is ​​added, stirred at 500 to 800 r / min for 10 to 30 minutes, poured, vibrated, and light-cured, and standard curing is performed for 10 to 15 days to obtain a cement-based polymer waterproof mortar.

[0019] Furthermore, the preparation method of the hydrophobically modified zeolite is as follows: immerse zeolite particles with a particle size of 6 to 10 mm in a silane emulsion of 50 to 100 times their mass for 12 hours, then filter, dry and grind. During grinding, the zeolite particles of each particle size are first crushed to 2 mm, and then put into a ball mill for ball milling for 40 minutes to obtain a hydrophobically modified zeolite with a particle size of 0.1 to 2000 μm; the silane emulsion is obtained by mixing γ-aminopropyltriethoxysilane, polyvinyl alcohol, isobutyltriethoxysilane, Span 80 and OP-10 composite emulsion system, and water in a volume ratio of 13 to 15:18 to 20:12 to 15:9 to 11:50 to 60; the mass ratio of Span 80 and OP-10 in the Span 80 and OP-10 composite emulsion system is 4:1.

[0020] Furthermore, the polymerization monomer is obtained by mixing bis(glycerol carbonate) octenedicarboxylate, 2,4,6-triallyloxy-1,3,5-triazine, sodium p-styrene sulfonate, and hydroxyethyl methacrylate in a mass ratio of 2:1:1:3.

[0021] Further, the preparation method of the bis(carbonate glyceryl) octenedicarboxylate is as follows: under nitrogen protection, the catalyst 4-dimethylaminopyridine and octenedicarboxylic acid are mixed in a mass ratio of 1:3.3 to 3.4, and then 20 times the mass of octenedicarboxylic acid is added with dichloromethane to stir and dissolve, followed by adding 1.2 to 1.6 times the mass of octenedicarboxylic acid glyceryl carbonate and 8 to 10 times the mass of octenedicarboxylic acid. The mixture is stirred and dissolved, and then 7 to 9 times the mass of octenedicarboxylic acid in dichloromethane is added at -4 to 4°C at a rate of 5s / drop. The mixture is heated to 25°C for reaction for 15 to 17 hours, and then filtered. The filtrate is washed twice with 0.5N dilute hydrochloric acid and saturated sodium carbonate solution, which are 8 to 10 times the mass of octenedicarboxylic acid, respectively, and then dried with magnesium sulfate and concentrated in a vacuum drying oven at 50°C for 5 hours. The residual glycerol carbonate is then washed with water to remove the residual glycerol carbonate, and finally washed with n-hexane and dried to obtain bis(glycerol carbonate) octenedicarboxylate; wherein the mass ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide to dichloromethane in the dichloromethane solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide is 0.65:1.

[0022] Furthermore, the radiation light source for photocuring is OmniCure S1000UV, the radiation energy density is 6.5 mW / cm2, and the radiation curing time is 600 s.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The cement-based polymer waterproof mortar prepared by the present invention has high compressive strength, flexural strength, good impermeability and flexibility;

[0025] The present invention adopts silane coupling agents γ-aminopropyltriethoxysilane and isobutyltriethoxysilane to modify zeolite. The silane coupling agent forms a hydrophobic layer on the surface of the zeolite and the wall of the perforated holes, making it difficult for water molecules to enter the interior of the zeolite; part of the silane coupling agent penetrates into the interior of the zeolite to block part of the pores, thereby reducing the high porosity of the zeolite, thereby reducing the water absorption rate, and ensuring the impermeability of the waterproof mortar.

[0026] The present invention adds hydrophobic modified zeolite in the powder material, and the particle size range is 0.1-2000 μm. The hydrophobic modified zeolite is compounded with the second liquid material and filled into various levels of capillary pores in the mortar, thereby reducing the porosity of the mortar and making the pores inside the mortar more miniaturized. The microstructure of the mortar after hardening is improved, and the impermeability of the waterproof mortar is improved. At the same time, the silane functional groups on the surface of the zeolite are hydrolyzed to generate silicon hydroxyl groups, which dehydrate and condense with the hydroxyl groups on the surface of cement particles to form chemical bonds, and are adsorbed on the surface of cement particles in a chemically bonded manner to form a hydrophobic layer, thereby further improving the impermeability of the waterproof mortar. The aminosilane on the surface of the zeolite can both hydrogen bond with the cement particles and produce physical and chemical adsorption with polyvinyl alcohol. The aminosilane, alkoxysilane and PVA form an interpenetrating network with silicone gel, so that the cement slurry system is hard, dense and has a certain toughness, thereby ensuring the compressive strength of the waterproof mortar and improving the flexural strength of the waterproof mortar.

[0027] The hydrophobically modified zeolite of the present invention is first compounded with the second liquid material, and part of the amino groups on the surface of the hydrophobically modified zeolite react with the cyclic carbonate of di(carbonated glycerol) octenedicarboxylate in the second liquid material to form a polyurethane cross-linked network in the waterproof mortar, thereby enhancing the flexural strength and flexibility of the waterproof mortar.

[0028] The present invention mixes a premixed powder and a first liquid, and then adds a premix of a hydrophobically modified zeolite and a second liquid. The polymerization monomer in the second liquid is quickly dispersed into the mixture of the premixed powder and the first liquid. Subsequently, a photoinitiator is used to perform a photocuring reaction to form a polyolefin cross-linked network with a hyperbranched structure, thereby avoiding the problem of a decrease in the strength of the waterproof mortar due to high-temperature curing of a conventional initiator and enhancing the mechanical properties of the waterproof mortar. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below in conjunction with examples, but the following examples should not be construed as limiting the present invention.

[0030] Some of the raw materials of the embodiments of the present invention and the comparative examples are as follows:

[0031] The cement is P·O42.5R silicate cement, the density of the cement is 3.07g / cm3, the residue on 80μm sieve is 4.8%, and the standard consistency is 26%;

[0032] The fly ash is Grade II fly ash from a power plant in Dongguan, which complies with the provisions of GB / T1596-2017 "Fly ash used in cement and concrete";

[0033] The sand is natural river sand with a particle size of 0.1 to 0.6 mm;

[0034] The water used shall be tap water that complies with the provisions of JGJ63-2006 "Standard for Water Used in Concrete Mixing";

[0035] The cellulose ether is P4123 from Hercules, hydroxypropyl methylcellulose, with a 2% aqueous solution viscosity of 40,000 cps (Brookfield RVT, 20° C., test average);

[0036] The dry powder water reducer is produced by BASF Melamine type sulfonated polycondensate powder;

[0037] The dry powder defoamer adopts P803 dry powder defoamer, with an active ingredient of 65%, containing liquid hydrocarbon, polyethylene glycol and inorganic carrier, which is a non-ionic surfactant suitable for cement dry-mixed mortar and is produced by MUNZING-CHEMIE of Germany.

[0038] The zeolite is natural zeolite from Henan Province. The blocky natural zeolite is ball-milled for 40 minutes to obtain natural zeolite powder, wherein the average particle size (D50) is 21 μm and the specific surface area is 1470 m2 / kg.

[0039] The styrene butadiene emulsion adopts BASF SD623 styrene butadiene emulsion;

[0040] The defoamer is BASF's defoamer FoamStarST2438;

[0041] The emulsifier is emulsifier OP-10;

[0042] The photoinitiator is water-based photoinitiator 2959;

[0043] Example 1

[0044] A method for preparing a cement-based polymer waterproof mortar, the preparation steps are as follows:

[0045] (1) 100 parts by mass of cement, 300 parts by mass of sand, 0.25 parts by mass of fly ash, 1 part by mass of cellulose ether, 0.2 parts by mass of dry powder water reducing agent, and 0.2 parts by mass of dry powder defoaming agent were stirred and mixed to obtain a premixed powder;

[0046] (2) 50 parts by weight of styrene butadiene emulsion and 15 parts by weight of water were stirred and mixed at 300 r / min for 1 min, and then 0.2 parts by weight of defoamer was added, and the stirring and mixing was continued for 1 min to obtain a first liquid material;

[0047] (3) Under light-proof conditions, 25 parts by weight of polymerizable monomer, 6 parts by weight of emulsifier, and 5 parts by weight of water were stirred and mixed at 300 r / min for 1 min, and then 0.5 parts by weight of aqueous photoinitiator was added, and the stirring and mixing was continued for 1 min to obtain a second liquid material;

[0048] (4) 32 parts by mass of the hydrophobically modified zeolite and the second liquid material were stirred at 1500 r / min for 10 min, and then 0.03 times of 1,5,7-triazabicyclo[4,4,0]dec-5-ene in the second liquid material was added, the temperature was raised to 140° C., and the reaction was stirred for 18 h. During this period, water was continuously added to ensure that the mass of the water was 3.8 times that of the hydrophobically modified zeolite. After naturally cooling to room temperature, a premix was obtained;

[0049] (5) The premixed powder and the first liquid material were mixed, stirred at 100 r / min for 5 min, and then the premix was added, stirred at 500 r / min for 10 min, poured, vibrated, and photocured, and standard curing was performed for 10 days to obtain a cement-based polymer waterproof mortar; the radiation light source for the photocuring was OmniCure S1000UV, the radiation energy density was 6.5 mW / cm2, and the radiation curing time was 600 s.

[0050] Wherein, the mass ratio of the first liquid material, the second liquid material and the powder material is 1:0.5:4.2;

[0051] The preparation method of the hydrophobically modified zeolite is as follows: immersing zeolite particles with a particle size of 6 mm in a silane emulsion of 50 times its mass for 12 hours, followed by filtering, drying and grinding. During grinding, the zeolite particles of each particle size are first crushed to 2 mm, and then put into a ball mill for ball milling for 40 minutes to obtain a hydrophobically modified zeolite with a particle size of 0.1 to 2000 μm; the silane emulsion is obtained by mixing γ-aminopropyl triethoxysilane, polyvinyl alcohol, isobutyl triethoxysilane, a composite emulsification system of Span 80 and OP-10, and water in a volume ratio of 13:18:12:9:50; the mass ratio of Span 80 to OP-10 in the composite emulsification system of Span 80 and OP-10 is 4:1;

[0052] The polymerization monomer is obtained by mixing bis(glycerol carbonate) octenyl dicarboxylate, 2,4,6-triallyloxy-1,3,5-triazine, sodium p-styrene sulfonate, and hydroxyethyl methacrylate in a mass ratio of 2:1:1:3;

[0053] The preparation method of the bis(carbonate glyceryl) octenedicarboxylate is as follows: under nitrogen protection, a catalyst 4-dimethylaminopyridine and octenedicarboxylic acid are mixed in a mass ratio of 1:3.3, and then dichloromethane with a mass of 20 times that of the octenedicarboxylic acid is added to stir and dissolve, and then glycerol carbonate with a mass of 1.2 times that of the octenedicarboxylic acid and dichloromethane with a mass of 8 times that of the octenedicarboxylic acid are added, and stirring and dissolving is continued, and then a dichloromethane solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide with a mass of 7 times that of the octenedicarboxylic acid is added at 0° C. at a rate of 5s / drop, and the temperature is raised. The mixture was reacted at 25°C for 15 hours, and then filtered. The filtrate was washed twice with 0.5N dilute hydrochloric acid and saturated sodium carbonate solution, respectively, which was 8 times the mass of octenedicarboxylic acid. The mixture was then dried with magnesium sulfate and concentrated in a vacuum drying oven at 50°C for 5 hours. The mixture was then washed with water to remove residual glycerol carbonate. The mixture was finally washed with n-hexane and dried to obtain bis(glycerol carbonate) octenedicarboxylate. The mass ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide to dichloromethane in the dichloromethane solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide was 0.65:1.

[0054] Example 2

[0055] A method for preparing a cement-based polymer waterproof mortar, the preparation steps are as follows:

[0056] (1) 100 parts by mass of cement, 300 parts by mass of sand, 0.25 parts by mass of fly ash, 1 part by mass of cellulose ether, 0.2 parts by mass of dry powder water reducing agent, and 0.2 parts by mass of dry powder defoaming agent were stirred and mixed to obtain a premixed powder;

[0057] (2) 60 parts by weight of styrene-butadiene emulsion and 20 parts by weight of water were stirred and mixed at 300 r / min for 2 min, and then 0.4 parts by weight of a defoamer was added, and the stirring and mixing was continued for 2 min to obtain a first liquid material;

[0058] (3) Under light-proof conditions, 30 parts by weight of polymerizable monomer, 9 parts by weight of emulsifier, and 10 parts by weight of water were stirred and mixed at 300 r / min for 2 min, and then 1.5 parts by weight of aqueous photoinitiator was added, and the stirring and mixing was continued for 2 min to obtain a second liquid material;

[0059] (4) 36 parts by mass of the hydrophobically modified zeolite and the second liquid material were stirred at 1600 r / min for 15 min, and then 0.03 times of 1,5,7-triazabicyclo[4,4,0]dec-5-ene was added to the second liquid material, and the temperature was raised to 140° C. and stirred for reaction for 21 h. During this period, water was continuously added to ensure that the mass of the water was 3.8 times that of the hydrophobically modified zeolite. After naturally cooling to room temperature, a premix was obtained;

[0060] (5) The premixed powder and the first liquid material were mixed, stirred at 200 r / min for 6 min, and then the premix was added, stirred at 700 r / min for 20 min, poured, vibrated, and photocured, and standard curing was performed for 12 days to obtain a cement-based polymer waterproof mortar; the radiation light source for the photocuring was OmniCure S1000UV, the radiation energy density was 6.5 mW / cm2, and the radiation curing time was 600 s.

[0061] Wherein, the mass ratio of the first liquid material, the second liquid material and the powder material is 1:0.5:4.2;

[0062] The preparation method of the hydrophobically modified zeolite is as follows: immersing zeolite particles with a particle size of 8 mm in a silane emulsion of 75 times its mass for 12 hours, followed by filtering, drying and grinding. During grinding, the zeolite particles of each particle size are first crushed to 2 mm, and then put into a ball mill for ball milling for 40 minutes to obtain a hydrophobically modified zeolite with a particle size of 0.1 to 2000 μm; the silane emulsion is obtained by mixing γ-aminopropyl triethoxysilane, polyvinyl alcohol, isobutyl triethoxysilane, a composite emulsification system of Span 80 and OP-10, and water in a volume ratio of 14:19:13:10:55; the mass ratio of Span 80 to OP-10 in the composite emulsification system of Span 80 and OP-10 is 4:1;

[0063] The polymerization monomer is obtained by mixing bis(glycerol carbonate) octenyl dicarboxylate, 2,4,6-triallyloxy-1,3,5-triazine, sodium p-styrene sulfonate, and hydroxyethyl methacrylate in a mass ratio of 2:1:1:3;

[0064] The preparation method of the bis(carbonate glyceryl) octenedicarboxylate is as follows: under nitrogen protection, a catalyst 4-dimethylaminopyridine and octenedicarboxylic acid are mixed at a mass ratio of 1:3.35, and then dichloromethane with a mass of 20 times that of the octenedicarboxylic acid is added to stir and dissolve, and then glycerol carbonate with a mass of 1.4 times that of the octenedicarboxylic acid and dichloromethane with a mass of 9 times that of the octenedicarboxylic acid are added, and stirring and dissolving is continued, and then a dichloromethane solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide with a mass of 8 times that of the octenedicarboxylic acid is added at 0° C. at a rate of 5s / drop, and the temperature is raised. The mixture was reacted at 25°C for 16 hours, and then filtered. The filtrate was washed twice with 0.5N dilute hydrochloric acid (9 times the mass of octenedicarboxylic acid) and saturated sodium carbonate solution, and then dried with magnesium sulfate and concentrated in a vacuum drying oven at 50°C for 5 hours. The residual glycerol carbonate was then washed with water, and finally washed with n-hexane and dried to obtain bis(glycerol carbonate) octenedicarboxylate; wherein the mass ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide to dichloromethane in the dichloromethane solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide was 0.65:1.

[0065] Example 3

[0066] A method for preparing a cement-based polymer waterproof mortar, the preparation steps are as follows:

[0067] (1) 100 parts by mass of cement, 300 parts by mass of sand, 0.25 parts by mass of fly ash, 1 part by mass of cellulose ether, 0.2 parts by mass of dry powder water reducing agent, and 0.2 parts by mass of dry powder defoaming agent were stirred and mixed to obtain a premixed powder;

[0068] (2) 70 parts by weight of styrene butadiene emulsion and 25 parts by weight of water were stirred and mixed at 300 r / min for 3 min, and then 0.5 parts by weight of a defoamer was added, and the stirring and mixing was continued for 3 min to obtain a first liquid material;

[0069] (3) Under light-proof conditions, 35 parts by weight of polymerizable monomer, 11 parts by weight of emulsifier, and 15 parts by weight of water were stirred and mixed at 300 r / min for 3 min, and then 4 parts by weight of aqueous photoinitiator were added, and the stirring and mixing was continued for 3 min to obtain a second liquid material;

[0070] (4) 40 parts by weight of the hydrophobically modified zeolite and the second liquid material were stirred at 1800 r / min for 20 min, and then 0.03 times of 1,5,7-triazabicyclo[4,4,0]dec-5-ene in the second liquid material was added, the temperature was raised to 140° C., and the reaction was stirred for 24 h. During this period, water was continuously added to ensure that the mass of the water was 3.8 times that of the hydrophobically modified zeolite. After naturally cooling to room temperature, a premix was obtained;

[0071] (5) The premixed powder and the first liquid material were mixed, stirred at 300 r / min for 7 min, and then the premix was added, stirred at 800 r / min for 30 min, poured, vibrated, and photocured, and standard curing was performed for 15 days to obtain a cement-based polymer waterproof mortar; the radiation light source for the photocuring was OmniCure S1000UV, the radiation energy density was 6.5 mW / cm2, and the radiation curing time was 600 s.

[0072] Wherein, the mass ratio of the first liquid material, the second liquid material and the powder material is 1:0.5:4.2;

[0073] The preparation method of the hydrophobically modified zeolite is as follows: immersing zeolite particles with a particle size of 10 mm in a silane emulsion of 100 times the mass of the zeolite particles for 12 hours, followed by filtering, drying and grinding. During the grinding, the zeolite particles of each particle size are first crushed to 2 mm, and then put into a ball mill for ball milling for 40 minutes to obtain a hydrophobically modified zeolite with a particle size of 0.1 to 2000 μm; the silane emulsion is obtained by mixing γ-aminopropyl triethoxysilane, polyvinyl alcohol, isobutyl triethoxysilane, a composite emulsification system of Span 80 and OP-10, and water in a volume ratio of 15:20:15:11:60; the mass ratio of Span 80 to OP-10 in the composite emulsification system of Span 80 and OP-10 is 4:1;

[0074] The polymerization monomer is obtained by mixing bis(glycerol carbonate) octenyl dicarboxylate, 2,4,6-triallyloxy-1,3,5-triazine, sodium p-styrene sulfonate, and hydroxyethyl methacrylate in a mass ratio of 2:1:1:3;

[0075] The preparation method of the bis(carbonate glyceryl) octenedicarboxylate is as follows: under nitrogen protection, a catalyst 4-dimethylaminopyridine and octenedicarboxylic acid are mixed in a mass ratio of 1:3.4, then dichloromethane with a mass of 20 times that of the octenedicarboxylic acid is added and stirred to dissolve, then glycerol carbonate with a mass of 1.6 times that of the octenedicarboxylic acid and dichloromethane with a mass of 10 times that of the octenedicarboxylic acid are added, stirring and dissolving is continued, then a dichloromethane solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide with a mass of 9 times that of the octenedicarboxylic acid is added at a rate of 5s / drop at 4°C, and the temperature is raised to 100°C. The mixture was reacted at 25°C for 17 hours, and then filtered. The filtrate was washed twice with 0.5N dilute hydrochloric acid and saturated sodium carbonate solution, respectively, which was 10 times the mass of octenedicarboxylic acid. The mixture was then dried with magnesium sulfate and concentrated in a vacuum drying oven at 50°C for 5 hours. The mixture was then washed with water to remove residual glycerol carbonate. The mixture was finally washed with n-hexane and dried to obtain bis(glycerol carbonate) octenedicarboxylate. The mass ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide to dichloromethane in the dichloromethane solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide was 0.65:1.

[0076] Comparative Example 1

[0077] The only difference between Comparative Example 1 and Example 2 is that the powder includes 100 parts by mass of cement, 300 parts by mass of sand, 0.25 parts by mass of fly ash, 32-40 parts by mass of zeolite, 1 part by mass of cellulose ether, 0.2 parts by mass of dry powder water reducer, and 0.2 parts by mass of dry powder defoamer, and the remaining steps and ingredients are the same as those in Example 2.

[0078] Comparative Example 2

[0079] The only difference between Comparative Example 2 and Example 2 is that the zeolite is modified by immersing in a silane emulsion obtained by mixing polyvinyl alcohol, isobutyltriethoxysilane, Span 80 and OP-10 composite emulsification system and water; the remaining steps and ingredients are the same as those in Example 2.

[0080] Comparative Example 3

[0081] The only difference between Comparative Example 3 and Example 2 is that the second liquid material includes 25 to 35 parts by weight of polymerizable monomers, 6 to 11 parts by weight of emulsifiers, 0.5 to 4 parts by weight of initiator ammonium persulfate, and 5 to 15 parts by weight of water; step (5) adopts high temperature curing, and the remaining steps and ingredients are the same as those in Example 2.

[0082] Comparative Example 4

[0083] The difference between Comparative Example 4 and Example 2 is that the polymerization monomers used are only 2,4,6-triallyloxy-1,3,5-triazine, sodium p-styrene sulfonate, and hydroxyethyl methacrylate; the remaining steps and ingredients are the same as those in Example 2.

[0084] Comparative Example 5

[0085] The difference between Comparative Example 5 and Example 2 is that the polymerization monomers only use bis(glycerol carbonate) octenyl dicarboxylate, sodium p-styrene sulfonate, and hydroxyethyl methacrylate; the remaining steps and ingredients are the same as those in Example 2.

[0086] Comparative Example 6

[0087] The only difference between Comparative Example 6 and Example 2 is that the cement-based polymer waterproof mortar is prepared by mixing only the first liquid material and the second liquid material; the remaining steps and ingredients are the same as those in Example 2.

[0088] Effect example

[0089] Table 1 below shows the performance test analysis results of the cement-based polymer waterproof mortars prepared by Examples 1 to 3 and Comparative Examples 1 to 8 of the present invention.

[0090] Table 1

[0091]

[0092] From Table 1, it can be found that the cement-based polymer waterproof mortar prepared in the embodiment has high compressive strength and flexural strength, good impermeability and flexibility; compared with Comparative Examples 1 and 2, Example 2 shows that the cement-based polymer waterproof mortar prepared by using the hydrophobically modified zeolite prepared by the silane coupling agent KH550 has high compressive strength and flexural strength, and good flexibility; compared with Comparative Example 3, Example 2 shows that the compressive strength of the cement-based polymer waterproof mortar prepared by photocuring with a photoinitiator is , high flexural strength, good impermeability and flexibility, and low water absorption; Compared with Comparative Examples 4 and 5, Example 2 found that the cement-based polymer waterproof mortar prepared with bis(glycerol carbonate) octenedicarboxylate and 2,4,6-triallyloxy-1,3,5-triazine had high compressive strength and flexural strength, good impermeability and flexibility; Compared with Comparative Example 6, Example 2 found that the cement-based polymer waterproof mortar prepared with the second liquid material had high compressive strength and flexural strength, good impermeability and flexibility, and low water absorption.

[0093] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

Claims

1. A cement-based polymer waterproof mortar, characterized in that: It comprises a first liquid material, a second liquid material and a powder material; the first liquid material comprises, by weight: 50 to 70 parts by weight of styrene-butadiene emulsion, 15 to 25 parts by weight of water, and 0.2 to 0.5 parts by weight of a defoamer; The second liquid material comprises, by weight, 25 to 35 parts by weight of a polymerizable monomer, 6 to 11 parts by weight of an emulsifier, 0.5 to 4 parts by weight of an aqueous photoinitiator, and 5 to 15 parts by weight of water; The powder material comprises 100 parts by mass of cement, 300 parts by mass of sand, 0.25 parts by mass of fly ash, 32-40 parts by mass of hydrophobically modified zeolite, 1 part by mass of cellulose ether, 0.2 parts by mass of dry powder water reducing agent, and 0.2 parts by mass of dry powder defoaming agent.

2. The cement-based polymer waterproof mortar according to claim 1, characterized in that: The mass ratio of the first liquid material, the second liquid material and the powder material is 1:0.5:4.

2.

3. The cement-based polymer waterproof mortar according to claim 1, characterized in that: The polymerizable monomers include bis(glycerol carbonate) octenedicarboxylate, 2,4,6-triallyloxy-1,3,5-triazine, sodium p-styrene sulfonate, and hydroxyethyl methacrylate.

4. The cement-based polymer waterproof mortar according to claim 1, characterized in that: The hydrophobic modified zeolite is obtained by immersing zeolite in silane emulsion, filtering, drying and grinding.

5. The cement-based polymer waterproof mortar according to claim 4, characterized in that: The silane emulsion is obtained by mixing gamma-aminopropyl triethoxysilane, polyvinyl alcohol, isobutyl triethoxysilane, a composite emulsifying system of Span 80 and OP-10, and water.

6. A method for preparing a cement-based polymer waterproof mortar according to any one of claims 1 to 5, characterized in that: The method comprises the following preparation steps: (1) 100 parts by mass of cement, 300 parts by mass of sand, 0.25 parts by mass of fly ash, 1 part by mass of cellulose ether, 0.2 parts by mass of dry powder water reducing agent, and 0.2 parts by mass of dry powder defoaming agent were stirred and mixed to obtain a premixed powder; (2) 50 to 70 parts by weight of styrene butadiene emulsion and 15 to 25 parts by weight of water are stirred and mixed at 300 r / min for 1 to 3 minutes, and then 0.2 to 0.5 parts by weight of a defoamer is added, and the stirring and mixing is continued for 1 to 3 minutes to obtain a first liquid material; (3) Under light-proof conditions, 25 to 35 parts by weight of polymerizable monomer, 6 to 11 parts by weight of emulsifier, and 5 to 15 parts by weight of water were stirred and mixed at 300 r / min for 1 to 3 minutes, and then 0.5 to 4 parts by weight of aqueous photoinitiator were added, and the stirring and mixing was continued for 1 to 3 minutes to obtain a second liquid material; (4) 32 to 40 parts by weight of the hydrophobically modified zeolite and the second liquid material are stirred at 1500 to 1800 r / min for 10 to 20 minutes, and then 0.03 times of 1,5,7-triazabicyclo[4,4,0]dec-5-ene in the second liquid material is added, the temperature is raised to 140° C., and the reaction is stirred for 18 to 24 hours. During this period, water is continuously added to ensure that the mass of the water is 3.8 times that of the hydrophobically modified zeolite. After naturally cooling to room temperature, a premix is ​​obtained; (5) The premixed powder and the first liquid material are mixed, stirred at 100 to 300 r / min for 5 to 7 minutes, and then the premix is ​​added, stirred at 500 to 800 r / min for 10 to 30 minutes, poured, vibrated, and light-cured, and standard curing is performed for 10 to 15 days to obtain a cement-based polymer waterproof mortar.

7. The method for preparing cement-based polymer waterproof mortar according to claim 6, characterized in that: The preparation method of the hydrophobically modified zeolite is as follows: immersing zeolite particles with a particle size of 6 to 10 mm in a silane emulsion of 50 to 100 times their mass for 12 hours, followed by filtering, drying, and grinding. During grinding, the zeolite particles of each particle size are first crushed to 2 mm, and then placed in a ball mill for ball milling for 40 minutes to obtain a hydrophobically modified zeolite with a particle size of 0.1 to 2000 μm; the silane emulsion is obtained by mixing γ-aminopropyltriethoxysilane, polyvinyl alcohol, isobutyltriethoxysilane, a composite emulsification system of Span 80 and OP-10, and water in a volume ratio of 13 to 15:18 to 20:12 to 15:9 to 11:50 to 60; the mass ratio of Span 80 to OP-10 in the composite emulsification system of Span 80 and OP-10 is 4:

1.

8. The method for preparing cement-based polymer waterproof mortar according to claim 6, characterized in that: The polymerization monomer is obtained by mixing bis(glycerol carbonate) octenedicarboxylate, 2,4,6-triallyloxy-1,3,5-triazine, sodium p-styrene sulfonate and hydroxyethyl methacrylate in a mass ratio of 2:1:1:

3.

9. The method for preparing cement-based polymer waterproof mortar according to claim 8, characterized in that: The preparation method of the bis(carbonate glyceryl) octenedicarboxylate is as follows: under nitrogen protection, a catalyst 4-dimethylaminopyridine and octenedicarboxylic acid are mixed in a mass ratio of 1:3.3-3.4, then dichloromethane with a mass of 20 times that of the octenedicarboxylic acid is added and stirred to dissolve, then glycerol carbonate with a mass of 1.2-1.6 times that of the octenedicarboxylic acid and dichloromethane with a mass of 8-10 times that of the octenedicarboxylic acid are added, stirring and dissolving is continued, and then a dichloromethane solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide with a mass of 7-9 times that of the octenedicarboxylic acid is added at a rate of 5s / drop at -4-4°C to dissolve. The mixture was heated to 25°C and reacted for 15 to 17 hours, and then filtered. The filtrate was washed twice with 0.5N dilute hydrochloric acid and saturated sodium carbonate solution, respectively, which was 8 to 10 times the mass of octenedicarboxylic acid. The mixture was then dried with magnesium sulfate and concentrated in a vacuum drying oven at 50°C for 5 hours. The residue of glycerol carbonate was then washed with water and finally washed and dried with n-hexane to obtain bis(glycerol carbonate) octenedicarboxylate. The mass ratio of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide to dichloromethane in the dichloromethane solution of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide was 0.65:

1.

10. The method for preparing cement-based polymer waterproof mortar according to claim 6, characterized in that: The radiation light source for the photocuring is OmniCure S1000 UV, the radiation energy density is 6.5 mW / cm2, and the radiation curing time is 600 s.

Citation Information

Patent Citations

  • Flame-retardant polymer cement waterproof mortar

    CN102503304A

  • High-adhesion waterproof ceramic tile joint filling mortar and preparation method thereof

    CN114907079A

  • Method for producing aqueous synthetic resin emulsion, method for producing reemulsifiable synthetic resin powder, method for producing polymer cement mortar, aqueous synthetic resin emulsion, and reemulsifiable synthetic resin powder

    WO2017104671A1