High-strength ceramsite prepared from machine-made sand sludge filter cake and method
High-strength ceramsite is prepared by combining manufactured sand sludge filter cake with aluminous and calcareous raw materials, followed by drying, granulation, and calcination. This solves the problems of low compressive strength and low admixture of ceramsite in existing technologies, and achieves efficient utilization and environmentally friendly ceramsite preparation.
Patent Information
- Application Number
- CN202411175222.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
In existing technologies, the compressive strength of ceramsite prepared from manufactured sand sludge filter cake is low, the amount of manufactured sand sludge filter cake is low, the comprehensive utilization rate is low, and the traditional preparation method has potential environmental hazards.
High-strength ceramsite is prepared by using manufactured sand sludge filter cake as the main raw material, combined with aluminous and calcareous raw materials, through drying, granulation and calcination. The manufactured sand sludge filter cake serves as the main ceramsite matrix, and a small amount of calcareous raw material is added as a pore-forming agent to form uniform pores and improve strength.
The prepared high-strength ceramsite has a compressive strength of 18.9–23.1 MPa, high content of manufactured sand sludge filter cake, high comprehensive utilization rate, saving natural shale resources and reducing environmental hazards.
Smart Images

Figure CN119038956A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of light aggregate preparation, and in particular to high-strength ceramsite and a method for preparing machine-made sand sludge filter cake. Background Art
[0002] In the process of industrial wet sand production, the stone powder produced by crushing stones is discharged after washing, sedimentation, and filtration, forming sludge filter cake waste. At present, most of this filter cake waste is directly stored in the open air, which not only occupies a large amount of land, but also creates obstacles to the subsequent production of machine-made sand. In addition, the open-air storage of filter cake waste is also prone to disasters such as dust and landslides, and there are extremely high safety hazards. Therefore, it has become an important issue to be solved urgently to recycle the waste of machine-made sand filter cake and alleviate its storage status.
[0003] Aggregate is the main raw material of concrete and plays an indispensable role in the skeleton and support of buildings. However, natural aggregate is a non-renewable resource, and artificial sand and gravel aggregate has gradually been widely used. On the other hand, ceramsite is a man-made lightweight aggregate with low density, high strength, and good frost resistance. Its application in the construction field can effectively alleviate the shortage of natural aggregate. However, the preparation of ceramsite requires resources such as silicon, aluminum, iron, and calcium.
[0004] At present, there are few technologies related to the preparation of high-strength ceramsite from machine-made sand sludge filter cakes, and the theoretical and practical development is still imperfect. In the existing technology, the patent "A method for firing ceramsite using machine-made sand sludge cakes" (publication number: CN114031416A) uses machine-made sand sludge cakes and dredging sludge as raw materials, and prepares ceramsite through drying, crushing, screening, mixing, granulation, drying, firing and other processes, and finally obtains sintered ceramsite with the best cylinder pressure strength of 7.52 MPa, but the machine-made sand sludge cake dosage of the patent is low, and the optimal condition is machine-made sand sludge cake: dredging sludge = 1:2, and the cylinder pressure strength is low.
[0005] The patent "A low-sintering temperature, lightweight, high-strength shale ceramsite and its preparation method" (publication number: CN117820013A) uses shale powder as raw material, adds sawdust, straw powder, etc. as pore-forming agents, glass powder, fluorite, etc. as sintering aids, and is homogenized, formed, dried, and fired in a reducing or inert atmosphere. The prepared high-strength ceramsite has a cylinder compressive strength of 12.5MPa. However, the main raw material used in this patent is natural shale, and the mining of natural shale will cause certain harm to the environment.
[0006] In summary, the existing methods for preparing building materials from machine-made sand sludge filter cakes have the following problems: ① There are few studies on high-strength expanded clay, and the prepared expanded clay has low cylinder compressive strength; ② The dosage of machine-made sand sludge filter cakes is low, and the comprehensive utilization rate is low. Summary of the invention
[0007] The purpose of the present invention is to overcome the above-mentioned technical deficiencies, provide a high-strength ceramsite and method for preparing machine-made sand sludge filter cake, and solve the technical problems in the prior art that the ceramsite prepared from machine-made sand sludge filter cake has low cylinder pressure strength and low dosage of machine-made sand sludge filter cake.
[0008] In order to achieve the above technical purpose, the technical solution provided by the present invention is: In a first aspect, the present invention provides a method for preparing high-strength ceramsite from machine-made sand sludge filter cake, comprising the following steps: mixing dry machine-made sand sludge filter cake, aluminum raw material and calcium raw material to obtain raw material; the dry machine-made sand sludge filter cake accounts for more than 50% of the raw material; adding water to the raw material to moisten it and then granulating it to obtain ceramsite blank; the ceramsite blank is dried and calcined to obtain high-strength ceramsite.
[0009] In a second aspect, the present invention provides a high-strength ceramsite prepared by the above method.
[0010] Compared with the prior art, the beneficial effects of the present invention include: The present invention uses machine-made sand sludge filter cake as the main raw material, combined with external aluminum raw materials and calcium raw materials, and obtains high-strength ceramsite through batching, granulation, drying and calcination. The machine-made sand sludge filter cake and aluminum raw materials are the main ceramic matrix, which improves the strength of the ceramsite; the machine-made sand sludge filter cake has a strong bonding ability and contains a large amount of Fe, Ca, K, Mg, Na and other components, and no additional binder and flux are needed. During the sintering process, it will make it easier for strong mineral phases such as mullite and liquid phases to form, so that the ceramsite can have higher strength; by adding a small amount of calcium raw materials as pore-forming agents, uniform pores are formed inside the ceramsite to meet relevant standards. In the high-strength ceramsite of the present invention, the machine-made sand sludge filter cake has a high dosage and a high comprehensive utilization rate, and the obtained ceramsite has a cylinder pressure strength of 18.9 to 23.1 MPa. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 It is a process flow chart of the method for preparing high-strength ceramsite from machine-made sand sludge filter cake of the present invention; Figure 2 These are product pictures of high-strength ceramsite obtained in Examples 1 to 3 of the present invention, wherein (a) is Example 1, (b) is Example 2, and (c) is Example 3. DETAILED DESCRIPTION
[0012] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0013] In view of the problems that the existing prepared ceramsite has low cylinder pressure strength, low dosage of machine-made sand sludge filter cake, and low comprehensive utilization rate, the present invention adopts machine-made sand sludge filter cake as the main raw material to prepare high-strength ceramsite, thereby realizing efficient and high value-added utilization of machine-made sand sludge filter cake, saving traditional shale raw materials, saving resources, and effectively solving the problems existing in the above-mentioned technology.
[0014] The main chemical composition of the machine-made sand sludge filter cake waste material used in the present invention is SiO 2 、Al 2 O 3 , Fe 2 O 3 , after adding an appropriate amount of calcium raw materials, it can be used as a raw material for preparing ceramsite. In addition, the main chemical components of machine-made sand filter cake waste are MgO, K 2 O and the like have a fluxing effect, which can reduce the difficulty of firing ceramsite. Therefore, the present invention uses the solid waste generated in the production of machine-made sand - machine-made sand sludge filter cake as the main raw material, saves the consumption of natural shale resources, combines external raw materials and preparation technology, can produce high-strength ceramsite, and at the same time uses the machine-made sand sludge filter cake in a high dosage to relieve the pressure on the storage yard.
[0015] First, see Figure 1 The present invention provides a method for preparing high-strength ceramsite from machine-made sand sludge filter cake, comprising the following steps: The dried machine-made sand sludge filter cake, the aluminum raw material and the calcium raw material are mixed and stirred to obtain a raw meal; the dried machine-made sand sludge filter cake accounts for more than 50% of the raw meal; Add water to the raw material to moisten it and then granulate it to obtain ceramsite blank; The ceramsite blank is dried and calcined to obtain high-strength ceramsite.
[0016] Preferably, the dried machine-made sand sludge filter cake is obtained by drying the machine-made sand sludge filter cake at 95°C to 105°C to constant weight. The machine-made sand sludge filter cake can be dried to effectively reduce the moisture content in the sludge, reduce its volume, improve stability and uniformity, and facilitate subsequent mixing with other powders; at the same time, the drying process can also eliminate pathogens and achieve harmless treatment of the sludge.
[0017] Preferably, the aluminum raw material comprises bauxite, and the calcium raw material comprises limestone.
[0018] Further preferably, the mass ratio of the dried machine-made sand sludge filter cake, bauxite and limestone is (10-14): (4-6): (1-3), and more preferably (10-14): (4-6): 1; wherein, if the amount of dried machine-made sand sludge filter cake increases and the amount of bauxite decreases, the strength of the ceramsite decreases; if the amount of dried machine-made sand sludge filter cake decreases and the amount of bauxite increases, the utilization rate of solid waste is low. If the amount of limestone decreases, the internal pores of the obtained ceramsite decrease and the density increases; if the amount of limestone is too high, the internal pores of the ceramsite are too many, the strength decreases, and the water absorption rate is too high, which will cause the finished ceramsite to fail to meet the requirements of the standard GB / T 17431.1-2010 "Light Aggregate and Its Test Methods".
[0019] Preferably, the amount of water added to the raw meal is 23-27% of the raw meal mass.
[0020] Preferably, the ceramsite blank is dried at 95°C to 105°C to constant weight. The surface of the ceramsite blank prepared in the present invention is relatively moist and easy to stick. If it is not dried and directly placed in a muffle furnace for calcination in large quantities, the prepared ceramsite is very easy to stick and the shape is incomplete. The surface of the ceramsite after drying in the present invention is smooth, there is no adhesion phenomenon, and it can be fired in large quantities, which is conducive to industrialization.
[0021] Preferably, the calcination treatment is to first raise the temperature to 390°C to 400°C and keep it at that temperature for 20 min to 30 min; then continue to raise the temperature to the firing temperature and keep it at that temperature, and then cool down to room temperature after the firing is completed.
[0022] More preferably, the sintering temperature is 1050° C. to 1200° C., and the sintering time is 15 min to 60 min.
[0023] More preferably, the heating rate is 3-6°C / min; after the sintering is completed, the temperature is lowered to room temperature along with the furnace.
[0024] In a second aspect, the present invention provides a high-strength ceramsite prepared by the above method.
[0025] The main mechanism of action and advantages of the present invention are: (1) The strength of ceramsite mainly comes from the silicon-aluminum components in the raw materials, that is, the ceramsite matrix. In addition, the traditional process also requires the addition of a certain amount of binders, fluxes, pore-forming agents, etc. to improve the performance and preparation conditions of ceramsite. The present invention uses machine-made sand sludge filter cake and bauxite as the main ceramsite matrix. The machine-made sand sludge filter cake has a high silicon content, and the aluminum source is provided by bauxite. The machine-made sand sludge filter cake has a strong bonding ability and contains a large amount of Fe, Ca, K, Mg, Na and other components, so there is no need to add additional binders and fluxes.
[0026] (2) The ignition loss of machine-made sand sludge filter cake and bauxite is small, so a small amount of limestone is added as a pore-forming agent. In addition, the components such as Fe, Ca, K, Mg, and Na in the filter cake will make it easier to form strong mineral phases such as mullite and liquid phases during the sintering process, making the ceramsite have higher strength.
[0027] (3) The machine-made sand sludge filter cake of the present invention has a high dosage and a high comprehensive utilization rate; the high-strength ceramsite prepared by the preparation process proposed in the present invention has high cylinder compressive strength and better performance.
[0028] The present invention is further described in detail below through specific examples and comparative examples. Among them, the main chemical composition of the machine-made sand sludge filter cake used in the present invention is 52.32wt% SiO 2 、15.02wt%Al 2 O 3 , 9.92wt%Fe 2 O 3 , 5.99wt% CaO, 6.59wt% MgO, 3.10wt% K 2 O, 2.08wt% Na 2 O and small amounts of other elements.
[0029] Example 1 This embodiment provides a method for preparing high-strength ceramsite from machine-made sand sludge filter cake, comprising the following steps: S1. Drying: Place the machine-made sand sludge filter cake in a 105°C oven and dry it for 60 min until constant weight is obtained to obtain a dry machine-made sand sludge filter cake; S2. Batching: Mix the dried machine-made sand sludge filter cake, bauxite and limestone in a mass ratio of 12:5:1 to prepare raw meal; S3, granulation: weigh an appropriate amount of the raw material obtained in step S2, add 25% of the mass of the raw material of municipal water and form into a mass, rub and granulate by hand to obtain ceramsite blank; S4, drying: drying the ceramsite blank obtained in step S3 in an oven at 105°C for 60 min until constant weight is obtained to obtain a dried ceramsite blank; S5, firing: the dried ceramsite blank obtained in step S4 is placed in a muffle furnace, the room temperature is raised to 400°C, the heating rate is 5°C / min, and the temperature is kept for 30 min; the temperature is raised from 400°C to 1125°C, the heating rate is 5°C / min; the ceramsite is fired for 30 min, and after the firing is completed, the temperature is lowered to room temperature with the furnace to obtain high-strength ceramsite.
[0030] Example 2 This embodiment provides a method for preparing high-strength ceramsite from machine-made sand sludge filter cake, comprising the following steps: S1. Drying: Place the machine-made sand sludge filter cake in a 105°C oven and dry it for 60 min until constant weight is obtained to obtain a dry machine-made sand sludge filter cake; S2. Batching: Mix the dried machine-made sand sludge filter cake, bauxite and limestone in a mass ratio of 12:5:1 to prepare raw meal; S3, granulation: weigh an appropriate amount of the raw material obtained in step S2, add 25% of the mass of the raw material of municipal water and form into a mass, rub and granulate by hand to obtain ceramsite blank; S4, drying: drying the ceramsite blank obtained in step S3 in an oven at 105°C for 60 min until constant weight is obtained to obtain a dried ceramsite blank; S5, firing: the dried ceramsite blank obtained in step S4 is placed in a muffle furnace, the room temperature is raised to 400°C, the heating rate is 5°C / min, and the temperature is kept for 30 min; the temperature is raised from 400°C to 1125°C, the heating rate is 5°C / min; the ceramsite is fired for 40 min, and after the firing is completed, the temperature is lowered to room temperature with the furnace to obtain high-strength ceramsite.
[0031] Example 3 This embodiment provides a method for preparing high-strength ceramsite from machine-made sand sludge filter cake, comprising the following steps: S1. Drying: Place the machine-made sand sludge filter cake in a 105°C oven and dry it for 60 min until constant weight is obtained to obtain a dry machine-made sand sludge filter cake; S2. Batching: Mix the dried machine-made sand sludge filter cake, bauxite and limestone in a mass ratio of 12:5:1 to prepare raw meal; S3, granulation: weigh an appropriate amount of the raw material obtained in step S2, add 25% of the mass of the raw material of municipal water and form into a mass, rub and granulate by hand to obtain ceramsite blank; S4, drying: placing the ceramsite blank obtained in step S3 in an oven at 105° C. and drying to constant weight to obtain a dried ceramsite blank; S5, firing: the dried ceramsite blank obtained in step S4 is placed in a muffle furnace, the room temperature is raised to 400°C, the heating rate is 5°C / min, and the temperature is kept for 30 min; the temperature is raised from 400°C to 1150°C, the heating rate is 5°C / min; the ceramsite is fired for 30 min, and after the firing is completed, the temperature is lowered to room temperature with the furnace to obtain high-strength ceramsite.
[0032] Comparative Example 1: The only difference between this comparative example and Example 1 is that the sintering temperature is 1025° C., and the other steps and conditions are the same as those in Example 1.
[0033] Comparative Example 2: The only difference between this comparative example and Example 1 is that the sintering time is 70 min, and the other steps and conditions are the same as those in Example 1.
[0034] Comparative Example 3: The difference between this comparative example and Example 1 is that the mass ratio of raw materials is dried sludge filter cake: bauxite: limestone = 12:0:1, and the other steps and conditions are the same as those in Example 1.
[0035] Comparative Example 4: The only difference between this comparative example and Example 1 is that the mass ratio of raw materials is dried sludge filter cake: bauxite: limestone = 12:5:0, and the other steps and conditions are the same as those in Example 1.
[0036] Comparative Example 5: The only difference between this comparative example and Example 1 is that the sintering temperature is 1225° C., and the other steps and conditions are the same as those in Example 1.
[0037] Comparative Example 5 uses a higher firing temperature than Example 1. The prepared ceramsite sample melts obviously, the ceramsite melts and sticks together, and has serious appearance defects, making it impossible to perform performance testing.
[0038] The performance of the ceramsite obtained in the above Examples 1-3 and Comparative Examples 1-4 was tested in accordance with the requirements of GB / T17431.2-2010 "Lightweight Aggregates and Test Methods Thereof". The results are shown in Table 1 below.
[0039] Table 1 Test results of Examples 1-3 and Comparative Examples 1-4
[0040] It can be seen from Table 1 that the high-strength ceramsite samples prepared in Examples 1-3 of the present invention have a relatively high cylinder compressive strength, which is between 18.9 and 23.1 MPa. Figure 2 As shown, the high-strength ceramsite prepared in Examples 1-3 has no obvious defects in appearance.
[0041] Compared with Example 1, Comparative Example 1 adopted a lower firing temperature, and the cylinder compressive strength of the prepared expanded clay sample was significantly lower than that of Example 1, indicating that the higher firing temperature formed more strong mineral phases during the firing process, thereby improving the cylinder compressive strength of the expanded clay.
[0042] Compared with Example 1, Comparative Example 2 used a longer firing time. There were no obvious defects in the appearance of the sample, but its cylinder compressive strength was reduced. The reason may be that the prolonged firing time caused a slight melting of the strength mineral phase in the high-strength expanded clay, resulting in a decrease in the cylinder compressive strength.
[0043] In Comparative Example 3, relative to Example 1, no bauxite was added, and the prepared expanded clay had a lower cylinder compressive strength. The reason may be that the aluminum content in the raw materials was reduced, which made it difficult to generate a strong mineral phase, resulting in a decrease in the cylinder compressive strength.
[0044] In Comparative Example 4, relative to Example 1, no limestone was added, and the bulk density of the prepared ceramsite was too high. The reason may be that the loss on ignition of the raw material was reduced, resulting in a decrease in the pores inside the ceramsite and an increase in density.
[0045] The present invention provides a high-strength ceramsite prepared from machine-made sand sludge filter cake and a method thereof. The machine-made sand sludge filter cake is used as the main raw material, and is combined with bauxite and limestone to prepare the high-strength ceramsite through processes such as drying, batching, granulation, drying, and sintering. The final ceramsite has a cylinder pressure strength of 18.9 to 23.1 MPa and a bulk density of 1023.47 to 1231.63 kg / m 3 , which complies with the relevant requirements of national standards. The method of the present invention can be used to utilize the machine-made sand sludge filter cake with high dosage and high added value. The dosage of the dry machine-made sand sludge filter cake can reach 66%, with high utilization rate, which can reduce the cost and environmental pressure of traditional disposal methods, and is conducive to achieving a high degree of unity of environmental benefits and social benefits. At the same time, it also has important practical significance for promoting the sustainable green development of the building materials industry.
[0046] The specific implementation of the present invention described above does not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing high-strength ceramsite from machine-made sand sludge filter cake, It is characterized in that The steps include: The dried machine-made sand sludge filter cake, the aluminum raw material and the calcium raw material are mixed and stirred to obtain a raw meal; the dried machine-made sand sludge filter cake accounts for more than 50% of the raw meal; adding water to the raw material to moisten it and then granulating it to obtain ceramsite blank; The ceramsite blank is dried and calcined to obtain high-strength ceramsite.
2. The method for preparing high-strength ceramsite from machine-made sand sludge filter cake according to claim 1, It is characterized in that The dried machine-made sand sludge filter cake is obtained by drying the machine-made sand sludge filter cake at 95° C. to 105° C. to a constant weight.
3. The method for preparing high-strength ceramsite from machine-made sand sludge filter cake according to claim 1, It is characterized in that The aluminum raw material includes bauxite, and the calcium raw material includes limestone.
4. The method for preparing high-strength ceramsite from machine-made sand sludge filter cake according to claim 3, It is characterized in that The mass ratio of the drying machine sand sludge filter cake, bauxite and limestone is (10-14): (4-6): (1-3).
5. The method for preparing high-strength ceramsite from machine-made sand sludge filter cake according to claim 1, It is characterized in that The amount of water added to the raw meal is 23-27% of the mass of the raw meal.
6. The method for preparing high-strength ceramsite from machine-made sand sludge filter cake according to claim 1, It is characterized in that The ceramsite blank is dried at 95°C to 105°C to a constant weight.
7. The method for preparing high-strength ceramsite from machine-made sand sludge filter cake according to claim 1, It is characterized in that The calcination treatment is to first raise the temperature to 390°C to 400°C and keep the temperature for 20 min to 30 min; then continue to raise the temperature to the firing temperature and keep the temperature, and then cool down to room temperature after the firing is completed.
8. The method for preparing high-strength ceramsite from machine-made sand sludge filter cake according to claim 7, It is characterized in that The sintering temperature is 1050°C to 1200°C, and the sintering time is 15 min to 60 min.
9. The method for preparing high-strength ceramsite from machine-made sand sludge filter cake according to claim 7, It is characterized in that During the calcination process, the heating rate is 3-6°C / min; after the calcination is completed, the temperature is lowered to room temperature along with the furnace.
10. The high-strength ceramsite prepared by the method as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Low-density and high-strength ceramic proppant and production method thereof
CN101831286A
Concrete lightweight aggregate and preparation method thereof
CN107601936A
Ceramsite prepared from sand washing sludge and municipal sludge and preparation method of ceramsite
CN110642637A
Method for firing light ceramsite by utilizing river sludge and machine-made sand tailing mud
CN113248276A
Method for preparing lightweight ceramsite by utilizing machine-made sand sludge
CN113831108A