High-thermal-shock-resistance rare earth composite high-strength heat storage refractory brick for hot blast stove and preparation method of refractory brick

By adding solid waste rare earth powder and thermally expandable volume stable fine powder to high alumina bricks for hot air furnaces, combined with reasonable particle size composition and firing process, the brick loss, deformation and crushing problems of high-heat vibration high alumina bricks are solved. The compressive strength and heat storage rate are improved, and efficient use of hot air furnaces and resource utilization are achieved.

CN119038970AActive Publication Date: 2024-11-29BAOTOU ANDESHANAI NEW MATERIAL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411329287.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-29
Estimated Expiration
2044-09-24

AI Technical Summary

Technical Problem

The existing high-heat vibration high-aluminum bricks for hot air furnaces have problems such as brick drop, deformation, and crushing during use. The raw material cost is high, the firing temperature is high, the production energy consumption is high, the strength, the thermal shock resistance and the heat storage rate are high. Quality indicators still need to be improved.

Method used

A high-thermal shock resistance rare earth composite high-strength heat-retaining refractory brick is adopted, including aggregate high-alumina bauxite clinker, solid waste rare earth powder, thermal expansion volume stable fine powder and combined slurry, and the composition and firing are carried out through reasonable particle size. The process enhances the compressive strength and thermal shock stability of the material, and reduces costs by using solid waste and rare earth tailings.

Benefits of technology

It improves the thermal shock, compressive strength and heat storage rate of high-aluminum refractory bricks, extends the service life, reduces production costs and energy consumption, and achieves high density, high pressure resistance and high heat storage performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038970A_ABST
    Figure CN119038970A_ABST
Patent Text Reader

Abstract

The invention provides a high thermal shock resistance rare earth composite high-strength heat storage refractory brick for a hot blast stove and a preparation method thereof, and relates to the technical field of refractory bricks, the refractory brick comprises the following raw materials by weight: 15-25 parts of 5-3mm aggregate high bauxite clinker, 15-25 parts of 3-1mm high bauxite clinker, 10-25 parts of 1-0mm high bauxite clinker, 5-17 parts of 200 mesh high bauxite clinker fine powder, and 10-20 parts of secondary aluminum ash powder, the solid waste rare earth material powder accounts for 5-10 parts, the soft clay accounts for 0-4 parts, the thermal expansion volume stable fine powder accounts for 3-11 parts, and the binding slurry accounts for 3-5 parts. The preparation method comprises the following steps: weighing ingredients, carrying out wet ball milling, sintering and crushing, grading the raw materials, proportioning, mixing and stirring, carrying out compression molding, baking, and calcining to obtain a finished product. The prepared rare earth composite high-strength heat storage refractory brick with high thermal shock resistance is wide in raw material distribution and low in cost; the firing temperature in the preparation process is low, and energy is saved; the prepared product has the characteristics of high compression strength, good thermal shock resistance, high volume density, high heat storage rate, high refractoriness under load and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of refractory bricks, and in particular relates to a rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for a hot blast furnace and a preparation method thereof. Background Art

[0002] According to statistics, the energy consumption of the domestic industrial sector accounts for 70% of the total national energy consumption. Among them, industrial kilns are the largest energy consumers in my country, accounting for about 25% of the total national energy consumption. Low energy utilization is one of the main reasons for the high energy consumption of industrial kilns. Compared with industrial kilns in developed countries, the average thermal efficiency of domestic industrial kilns is about 20% lower, and the energy wasted is equivalent to 200 million tons of standard coal. The hot blast furnace is used as a blast furnace heating and blowing device. The high-temperature flue gas after combustion passes through the holes of the hot blast furnace checker bricks and transfers heat to the checker bricks; during the "air supply period", the cold air is heated into hot air through convection heat exchange and radiation heat exchange. The selection of refractory materials for hot blast furnaces is mainly determined by the hot air temperature. When the wind temperature is between 900 and 1100°C, high-aluminum bricks, mullite bricks or sillimanite bricks are used for the lining and checker bricks of the high-temperature part; when the wind temperature is higher than 1100°C, high-aluminum bricks, mullite bricks and silica bricks are generally used as furnace linings or checker bricks.

[0003] The commonly used heat storage body for hot blast furnaces is checker bricks. Existing technical research is mostly to improve the thermal performance of checker bricks, improve heat exchange efficiency and extend service life by reducing the size of the grid holes, reducing the equivalent thickness of the checker bricks and increasing the heat exchange surface area per unit volume. Checker bricks are present in the heat storage chamber of the hot blast furnace as heat storage bodies. Their materials are mainly divided into three types: high silicon material, high aluminum material and clay material. Among them, high aluminum checker bricks have an aluminum content of about 70%, low creep, and an operating temperature of 800~1000℃. They are located in the middle part of the heat storage chamber of the hot blast furnace and account for 25~30% of the usage.

[0004] The hot blast furnace uses a series of low creep bricks containing "three stones" and high thermal shock resistance bricks. The thermal shock resistance of high-alumina refractory bricks refers to the ability of refractory bricks to resist rapid temperature changes without being destroyed. Coal gangue is solid waste generated during coal mining, washing and processing. At present, there are more than 1,500 coal mining stone mountains, covering an area of ​​13,500 hm2. 2 More than 100 million tons per year, forming an additional area of ​​more than 400 hm 2. Coal gangue has become the industrial waste with the largest cumulative stock and the largest occupied site in my country. Andalusite is a natural aluminum-silica refractory mineral raw material with high-temperature reaction activity. The phase transformation and microstructural changes of andalusite at high temperature give it special properties such as excellent thermal shock resistance, high thermal mechanical strength, good corrosion resistance, etc. When producing refractory castables, a certain amount of andalusite is added to improve the load softening and creep properties of the refractory castables; andalusite of different particle sizes plays different roles in improving material properties. Coarse-grained andalusite can improve the high-temperature strength of the material, while fine-grained andalusite can improve the thermal shock resistance of the material, which is effective in solving the cracking problem during the use of castables. The "three-stone" minerals have good thermal shock resistance because they can be irreversibly transformed into mullite and SiO2 melt under high temperature conditions, and the expansion rate of mullite is relatively small, α=5.3*10 -6 / ℃, which is beneficial to resist thermal shock.

[0005] High-alumina and clay refractory materials are usually used for the checker bricks in the middle and lower parts of the regenerator of the hot blast furnace. As the height of the regenerator of a large hot blast furnace increases, the pressure of the upper checker bricks on the lower refractory materials increases. According to a foreign investigation on the damage of checker bricks in large high-temperature hot blast furnaces, it was found that the cracking and breaking of the checker bricks in the lower part are increasing due to the influence of periodic temperature fluctuations. Therefore, in addition to continuing to control its creep characteristics, higher requirements must be placed on the room temperature compressive strength and thermal shock stability of the products.

[0006] High-alumina refractory products have the main characteristics of high refractoriness, excellent impact resistance, high compressive strength and high refractoriness under load. They are used to build various large blast furnaces, such as high-temperature parts of thermal equipment such as steelmaking furnaces. High-alumina bricks are widely used in metallurgy, chemical industry, construction and other industries. However, there are still many problems in the use of high-thermal shock-resistant high-alumina bricks for hot blast furnaces, such as brick falling, deformation, and breakage. The existing problems include: high raw material cost, high firing temperature, high production energy consumption, and quality indicators such as strength, thermal shock resistance, and heat storage rate still need to be improved.

[0007] Based on this, a rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace and a preparation method thereof are proposed. Summary of the invention

[0008] In view of the above-mentioned deficiencies in the prior art, the present invention provides a rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for a hot blast furnace and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is: In a first aspect, the present invention provides a high thermal shock resistance rare earth composite high-strength heat storage refractory brick for a hot blast furnace, comprising the following raw materials in parts by weight: 65-80 parts of aggregate high-alumina bauxite clinker, 10-20 parts of secondary aluminum ash powder, 5-10 parts of solid waste rare earth powder, 0-4 parts of soft clay, 3-11 parts of thermal expansion volume stable fine powder, and 3-5 parts of bonding slurry; The binding slurry is prepared by mixing a lignin binder and water.

[0010] As a further illustration of the present invention, the aggregate high alumina clinker includes the following raw materials in parts by weight: 15 to 25 parts of 5 to 3 mm high alumina clinker, 15 to 25 parts of 3 to 1 mm high alumina clinker, 10 to 25 parts of 1 to 0 mm high alumina clinker, and 5 to 17 parts of 200 mesh high alumina clinker fine powder.

[0011] The invention adopts reasonable clinker composition with different particle sizes to facilitate particle accumulation, and the surface structure is uniform and not rough.

[0012] As a further illustration of the present invention, the solid waste rare earth powder comprises the following raw materials in parts by weight: 40-65 parts of calcined coal gangue, 30-40 parts of rare earth tailings, and 5-20 parts of lanthanum carbonate or cerium carbonate powder.

[0013] As a further illustration of the present invention, the soft clay is specifically at least one of Su clay and Guangxi white mud; the thermal expansion volume stable fine powder is specifically a mixed powder of andalusite powder and sillimanite powder, and the mass ratio of the andalusite powder to the sillimanite powder is 4:3~9:2.

[0014] As a further illustration of the present invention, the binding slurry is specifically made of lignin and tap water in a mass ratio of 1:2.11~2.13.

[0015] The second aspect of the present invention provides a method for preparing the above-mentioned rare earth composite high-strength heat storage refractory bricks with high thermal shock resistance for hot blast furnaces, comprising the following steps: S1. Ingredient weighing: weigh the following raw materials in parts by weight: 40-65 parts of calcined coal gangue, 30-40 parts of rare earth tailings, and 5-20 parts of lanthanum carbonate or cerium carbonate powder; S2, wet ball milling: adding weighed calcined coal gangue powder, rare earth tailing powder, lanthanum carbonate or cerium carbonate powder into a ball mill, stirring and wet ball milling, and drying after discharging; S3, sintering and crushing: the dried material in S2 is sintered at high temperature, and then crushed and sieved to obtain solid waste rare earth powder; S4, fully and evenly stirring and mixing the lignin binder and water to obtain a binding slurry; S5. Ingredients: weigh the raw material ratio of the rare earth composite high-strength heat storage refractory bricks for hot blast furnaces according to any one of claims 1 to 5; S6, mixing and stirring: stir and mix the weighed aggregate high-alumina clinker; at the same time, add the secondary aluminum ash powder, solid waste rare earth powder, soft clay, thermal expansion volume stable fine powder, and binding slurry in sequence, stir and mix thoroughly, and let stand for use after stirring; S7, pressing and molding: pressing the mixed raw materials after standing with high-alumina refractory bricks to obtain a semi-finished product initial mold; S8, baking: putting the semi-finished product into an oven for baking, and taking it out after naturally cooling it in the oven after baking; S9, calcination system: evenly spread the alumina powder in an energy-saving box-type electric furnace, and then put the dried semi-finished product into the energy-saving box-type electric furnace for calcination; S10. Finished product: After the fired high-alumina refractory brick samples are naturally cooled to room temperature by the furnace temperature, they are taken out to obtain high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnaces made from solid waste and rare earth tailings.

[0016] As a further illustration of the present invention, the material-water ratio of wet ball milling in S2 is 1 / 6, and the stirring time is 15-20 min; The sintering temperature in S3 is 950~1300℃, and the temperature is kept for 1~3h. After cooling, the sintered steel is put into a crusher for crushing, and then passed through a 200-mesh sieve; In S4, the lignin binder and water are mixed in a mass ratio of 1:2.11-2.13.

[0017] As a further illustration of the present invention, before the batching of S5, raw material selection is required: aggregate high-alumina bauxite clinker, secondary aluminum ash powder, solid waste rare earth material powder, soft clay, thermal expansion volume stable fine powder, and combined slurry raw materials are graded to determine different particle sizes; Among them, the aggregate high alumina clinker is selected from 5~3mm high alumina clinker, 3~1mm high alumina clinker, 1~0mm high alumina clinker and 200 mesh high alumina clinker fine powder respectively; the solid waste rare earth material powder particle size is selected from 200 mesh; the secondary aluminum ash powder is selected from 200 mesh; the soft clay is selected from 200 mesh; the andalusite powder in the thermal expansion volume stable fine powder is selected from 200 mesh and the sillimanite powder is selected from 325 mesh.

[0018] In S5, the aggregate high-alumina bauxite clinker is prepared according to the following weight fractions: 15-25 parts of 5-3mm high-alumina bauxite clinker, 15-25 parts of 3-1mm high-alumina bauxite clinker, 10-25 parts of 1-0mm high-alumina bauxite clinker, and 5-17 parts of 200-mesh high-alumina bauxite clinker fine powder; the thermal expansion volume stable fine powder is prepared according to the mass ratio of garnet powder to sillimanite powder of 4:3-9:2.

[0019] As a further illustration of the present invention, in S6, the mixing time of the aggregate is 1 to 3 minutes, and the mixing time of the fine powder is 2 to 3 minutes, wherein the fine powder is composed of secondary aluminum ash powder, solid waste rare earth powder, soft clay, and thermal expansion volume stable fine powder; after the aggregate is evenly mixed, it is stirred together with the fine powder for 2 to 3 minutes, and finally the prepared binding slurry is added and stirred for 4 to 6 minutes; after stirring, it is packed into a bag and left to stand for 1 to 5 hours for use; The molding pressure of S7 is 137MPa, and the molding rate is ≥98%; In S8, the baking temperature is 110°C, the baking time is 24h~48h, and it needs to be baked until the moisture content is less than 2%.

[0020] As a further illustration of the present invention, the calcination conditions in S9 are specifically set as: heating between room temperature and 80°C for 0.5h, and keeping warm for 0.5~1h; heating between 80~500°C for 1~1.5h, and keeping warm for 1~2h; heating between 800~1100°C for 1~1.5h, and keeping warm for 1~2h; heating between 1100°C and the highest temperature for 1~1.5h, and keeping warm for 5~6h at the highest temperature of 1450°C~1520°C.

[0021] The present invention enhances the compressive strength of high-alumina materials while utilizing solid waste, further improving the thermal shock resistance and heat storage rate of high-alumina refractory bricks. The functional additive solid waste rare earth material has the effect of fluxing and sintering, which not only reduces energy consumption but also helps to improve the compressive strength of high-alumina refractory bricks.

[0022] The thermal expansion volume stabilizing fine powder added in the present invention, andalusite and sillimanite materials have the characteristics of small thermal expansion coefficient, improved room temperature pressure resistance and the like. When andalusite is decomposed at high temperature, a certain amount of mullite and liquid phase are generated. The produced mullite is helpful to improve the thermal shock stability and load softening temperature of high-alumina refractory bricks, and the liquid phase promotes the sintering and densification of the matrix and aggregate in the material.

[0023] The main raw materials of the present invention are widely distributed, easily available and low in cost; the solid waste rare earth material in the present invention is prepared by using coal gangue, rare earth tailings and rare earth compounds, and a physical and chemical reaction occurs during the calcination of coal gangue, rare earth tailings and rare earth compounds: the volatile matter changes, impurities in the raw materials are removed, and at the same time, the chemical reaction produced by calcination makes the product purer, and the obtained solid waste rare earth material powder is more uniform and has good performance stability; the sintering temperature of the present invention is sintered at 1450°C-1520°C, which saves energy consumption to a certain extent.

[0024] The high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnaces made from solid waste and rare earth tailings of the present invention have excellent properties such as high density, high compressive strength, high thermal shock stability, high heat storage and the like.

[0025] The high-alumina refractory brick doped with rare earth oxides of the present invention has rare earth powder concentrated in the pores around fine particles, thereby enhancing the bonding effect between particles inside the material; the rare earth oxides have an extremely high melting point and can resist high temperature effects, and are used at high temperatures.

[0026] Solid waste rare earth powder can react with acidic compounds at sintering temperature to generate substances with higher refractoriness, which promotes the low-temperature sintering of high-aluminum refractory materials and improves the mechanical properties of refractory bricks to a certain extent. Doping with solid waste rare earth powder promotes the nucleation and growth of high-aluminum refractory grains, improving the refractoriness and thermal shock stability of the material. Doping with solid waste rare earth powder can promote the development of crystal phases in refractory materials and enhance the bonding force between particles in refractory materials. Doping with solid waste rare earth powder can promote the thermal storage and thermal conductivity of high-aluminum refractory materials. After doping with sillimanite and andalusite powder at the same time, the present invention reduces the content of impurities and converts them into mullite after heating to form a dense network structure. Doping with solid waste rare earth powder, thermal expansion volume stabilizing powder, etc., begins to jointly promote the sintering of refractory materials at around 1300°C, and uses the volume effect to compensate for the sintering shrinkage of refractory materials under high temperature. By doping with thermal expansion volume stabilizing powder, under a suitable calcination process, and utilizing its different decomposition temperatures and expansion properties, high-alumina refractory products will have expansion caused by the decomposition of unconverted crystals at industrial use temperatures, which will generate certain stress inside the refractory material, resisting the load and enhancing creep resistance and thermal shock resistance.

[0027] In summary, the present invention has the following advantages compared with the prior art: The invention enhances the thermal shock resistance and compressive strength of high-alumina refractory bricks, synthesizes solid waste coal gangue and rare earth compounds into a functional additive solid waste rare earth material, and scientifically selects the chemical components of raw materials from different factories, reasonably controls the ingredients, mixes and stirs them until the high-alumina refractory bricks are pressed and formed, and a suitable firing process system is used to prepare a high thermal shock resistance rare earth composite high-strength heat storage refractory brick for hot blast furnaces made of solid waste and rare earth tailings. The raw materials used are widely distributed and low in cost; the firing temperature is low in the preparation process, which saves energy; the prepared product has the characteristics of high compressive strength, good thermal shock resistance, high bulk density, high heat storage rate, high softening temperature under load and the like.

[0028] The main raw materials of the present invention are high-alumina granular high-alumina bauxite clinker as aggregate, and solid waste rare earth raw materials, thermal expansion volume stable fine powder, secondary aluminum ash powder, soft clay, and bonding slurry as auxiliary materials. It is a new technical application approach for solid waste and rare earth oxides. It can obtain a high thermal shock resistance rare earth composite high-strength heat storage refractory brick for hot blast furnaces prepared by using solid waste and rare earth tailings, thereby increasing the service life of high-alumina refractory bricks for hot blast furnaces.

[0029] The main raw materials of the refractory bricks in the present invention are high-alumina bauxite clinker, secondary aluminum ash powder, solid waste rare earth material powder, thermal expansion volume stable fine powder, etc. The raw materials are widely distributed, easy to obtain, and low in cost; the firing temperature in the preparation process is low, which saves energy; the prepared high-alumina refractory brick products have high body density, high strength, high thermal shock stability, and high heat storage; the service life of high-temperature kiln hot blast furnaces is extended, and the repair and maintenance costs are reduced. Compared with traditional high-alumina refractory bricks for high-temperature kilns, the material products doped with rare earth components have the characteristics of high-temperature thermal shock stability, high density, excellent resistance to rapid cooling and heating, high compressive strength, and high heat storage. It is used in high-temperature hot blast furnace linings, checker bricks for hot blast furnaces, etc. While comprehensively utilizing solid waste, the application field of rare earth products is broadened. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a flow chart of the preparation method of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] The following is explained in conjunction with specific embodiments. Table 1 Raw material information table in the following examples Reagents Main Ingredients 88 high alumina bauxite clinker 5~3 / 3~1 / 1~0mm <![CDATA[Weight content: Al2O3: 88%, SiO2: 2%, CaO + MgO: 1%, Fe2O3: 1.5%, R2O: 0.5%, the oxides of the remaining components account for 7%]]> 85 high alumina clinker 5~3 / 3~1 / 1~0mm <![CDATA[Weight content: Al2O3: 85%, SiO2: 5%, CaO + MgO: 1%, Fe2O3: 1.5%, R2O: 0.5%, the oxides of the remaining components account for 7%]]> 80 high alumina clinker 5~3 / 3~1 / 1~0mm <![CDATA[Weight content: Al2O3: 80%, SiO2: 10%, CaO + MgO: 1%, Fe2O3: 1.5%, R2O: 0.5%, the oxides of the remaining components account for 7%]]> Andalusite <![CDATA[Weight content: Al2O3: 58%, Fe2O3: 0.8%, K2O + Na2O: 0.5%, the remainder being oxides of the remaining components]]> Sillimanite <![CDATA[Weight content: Al2O3: 57%, SiO2: 41%, Fe2O3: 0.5%, K2O + Na2O: 0.1%, the remainder being oxides of the remaining components]]> Secondary aluminum ash <![CDATA[Weight content: Al2O3: 80%, SiO2: 12%, oxides of the remaining components account for 8%]]> Calcined coal gangue <![CDATA[Weight content: Al2O3: 30%, Fe2O3: 0.5%, SiO2: 45%, MgO + CaO: 15%, the oxides of the remaining components account for 10%]]> Rare earth tailings <![CDATA[Weight content: Al2O3: 19%, SiO2: 65%, REO: 5%, the balance being oxides of the remaining components]]> Guangxi white clay <![CDATA[Weight content: Al2O3: 33%, SiO2: 41%, CaO: 3%, Fe2O3: 3%, MgO: 4%, the oxides of the remaining components account for 16%]]> Table 2 Equipment information table in the following embodiments name factory model Vertical mortar mixer Shaoxing Yina Instrument Manufacturing Co., Ltd. UJZ-15 Electric program-controlled screw press Shandong Mingren Heavy Machinery Co., Ltd. EPK-630 Electric blast drying oven Beijing Yongguangming Medical Instrument Co., Ltd. 101-1ABS Energy-saving box-type electric furnace Tianjin Zhonghuan Experimental Electric Furnace Co., Ltd. SX-G64163

[0033] Example 1

[0034] like Figure 1 As shown, this embodiment provides a high thermal shock resistance rare earth composite high-strength heat storage refractory brick for a hot blast furnace, comprising the following raw materials in parts by weight: 25 parts of 5~3mm aggregate high alumina bauxite clinker, 20 parts of 3~1mm high alumina bauxite clinker, 10 parts of 1~0mm high alumina bauxite clinker, 12 parts of 200 mesh high alumina bauxite clinker fine powder, 20 parts of secondary aluminum ash powder, 10 parts of solid waste rare earth material powder, 7 parts of thermal expansion volume stable fine powder, and 3.5 parts of lignin binding slurry; wherein the thermal expansion volume stable fine powder is prepared according to the mass ratio of garnet powder and sillimanite powder of 4:3.

[0035] The preparation method of the above-mentioned rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace comprises the following steps: S1. Ingredient weighing: weigh the raw materials according to the following weight proportions: 60 parts of calcined coal gangue, 35 parts of rare earth tailings, and 5 parts of cerium carbonate powder.

[0036] S2. Wet ball milling: Add weighed calcined coal gangue powder, rare earth tailings powder and cerium carbonate powder into the ball mill; the material-water ratio is 1 / 6, stir and mix thoroughly for 15 minutes; dry the material after discharge.

[0037] S3, sintering: sintering at a high temperature of 1200°C, keeping warm for 1 hour, and after cooling, putting the material into a crusher for crushing, sieving through 200 meshes, and obtaining solid waste rare earth powder.

[0038] S4. The lignin binder and tap water are stirred and mixed thoroughly and evenly using a high-speed separation stirrer in a mass ratio of 1:2.11 to obtain a binding slurry.

[0039] S5. Raw material selection: The aggregate high-alumina clinker is selected from 5~3mm high-alumina clinker, 3~1mm high-alumina clinker, 1~0mm high-alumina clinker and 200-mesh high-alumina clinker fine powder; the solid waste rare earth powder is selected from 200-mesh; the secondary aluminum ash powder is selected from 200-mesh; among the thermal expansion volume stable fine powder, the andalusite powder is selected from 200-mesh and the sillimanite powder is selected from 325-mesh; package and set aside.

[0040] S6. Batching: weigh the materials according to the raw material composition ratio of the above-mentioned high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnace.

[0041] S7. Mixing and stirring: Mix the weighed aggregates of different particle sizes; at the same time, fully mix the fine powder composed of secondary aluminum ash, solid waste rare earth powder, and thermal expansion volume stable fine powder; wherein, the mixing time of the aggregate is 2 minutes, and the mixing time of the fine powder is 3 minutes. After the aggregate is mixed, the fine powder is added and stirred for 2 minutes, and finally the prepared binding slurry is added and stirred for 5 minutes; after stirring, the mixture is packed into bags and left to stand for 1 hour for use.

[0042] S8. Pressing and molding: The static mixture is pressed into high-alumina refractory bricks by an electric programmable screw brick press. The size of the high-alumina bricks is pressed according to user requirements, such as standard bricks and others; the molding pressure is 137MPa, and the molding rate is ≥98%; the semi-finished product prototype is obtained.

[0043] S9, baking: put the pressed semi-finished product into an oven and bake it at 110°C for 24 hours. After baking, cool it naturally in the oven and then take it out; the moisture after baking is less than 2%.

[0044] S10, calcination system: the alumina powder is evenly spread in an energy-saving box-type electric furnace, and then the dried semi-finished product is placed in the energy-saving box-type electric furnace for calcination; wherein the calcination conditions are set as follows: heating between room temperature and 80°C for 0.5h, and keeping warm for 0.5h; heating between 80 and 500°C for 1.5h, and keeping warm for 2h; heating between 800 and 1100°C for 1.5h, and keeping warm for 2h; heating between 1100°C and 1450°C for 1h, and keeping warm at a high temperature of 1450°C for 6h.

[0045] S11. Finished product: After the fired high-alumina brick samples are naturally cooled to room temperature by the furnace temperature, they are taken out to obtain finished products of high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnaces made of solid waste and rare earth tailings.

[0046] The above-mentioned test of using solid waste and rare earth tailings to prepare high thermal shock resistance rare earth composite high strength heat storage refractory bricks for hot blast furnaces is as follows: The bulk density is 2.58g / cm 3 The apparent porosity is 23.22%, the water absorption is 8.5%, the compressive strength is 72.09MPa, the heat storage rate is increased by 13.60%, and the thermal shock resistance: thermal shock stability 1100℃ water cooling ≥115 times.

[0047] Example 2

[0048] The present embodiment provides a high thermal shock resistance rare earth composite high-strength heat storage refractory brick for a hot blast furnace, comprising the following raw materials in parts by weight: 25 parts of 5-3mm aggregate high alumina bauxite clinker, 15 parts of 3-1mm high alumina bauxite clinker, 25 parts of 1-0mm high alumina bauxite clinker, 5 parts of 200 mesh high alumina bauxite clinker fine powder, 10 parts of secondary aluminum ash powder, 6 parts of solid waste rare earth material powder, 1 part of soft clay, 11 parts of thermal expansion volume stable fine powder, and 4.5 parts of lignin binding slurry; wherein the thermal expansion volume stable fine powder is prepared according to a mass ratio of garnet powder to sillimanite powder of 2:1.

[0049] The preparation method of the above-mentioned rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace comprises the following steps: S1. Ingredient weighing: weigh the raw materials according to the following weight proportions: 65 parts of calcined coal gangue, 30 parts of rare earth tailings, and 10 parts of lanthanum carbonate powder.

[0050] S2. Wet ball milling: Add weighed calcined gangue powder, rare earth tailings powder and lanthanum carbonate powder into the ball mill; the material-water ratio is 1 / 6, stir and mix thoroughly for 20 minutes; dry after discharge.

[0051] S3, sintering: sintering at a high temperature of 950°C, keeping warm for 2 hours, and after cooling, putting the material into a crusher for crushing, sieving through 200 meshes, and obtaining solid waste rare earth powder.

[0052] S4. The lignin binder and tap water are stirred and mixed thoroughly and evenly using a high-speed separation stirrer in a mass ratio of 1:2.12 to obtain a binding slurry.

[0053] S5. Raw material selection: The aggregate high-alumina clinker is selected from 5~3mm high-alumina clinker, 3~1mm high-alumina clinker, 1~0mm high-alumina clinker and 200-mesh high-alumina clinker fine powder; the solid waste rare earth powder is selected from 200 mesh; the secondary aluminum ash powder is selected from 200 mesh; the soft clay is selected from 200 mesh; the andalusite powder and sillimanite powder in the thermal expansion volume stable fine powder are selected from 200 mesh and 325 mesh, respectively; package and set aside.

[0054] S6. Batching: weigh the materials according to the raw material composition ratio of the above-mentioned high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnace.

[0055] S7. Mixing and stirring: Mix the weighed aggregates of different particle sizes; at the same time, fully mix the fine powder composed of secondary aluminum ash, solid waste rare earth powder, soft clay, and thermal expansion volume stable fine powder; wherein, the mixing time of the aggregate is 1 min, and the mixing time of the fine powder is 2 min. After the aggregate is mixed, the fine powder is added and stirred for 2 min, and finally the prepared binding slurry is added and stirred for 4 min; after stirring, the mixture is packed into bags and left to stand for 2 h for use.

[0056] S8. Pressing and molding: The static mixture is pressed into high-alumina refractory bricks by an electric programmable screw brick press. The size of the high-alumina bricks is pressed according to user requirements, such as standard bricks and others; the molding pressure is 137MPa, and the molding rate is ≥98%; the semi-finished product prototype is obtained.

[0057] S9. Baking: Place the pressed semi-finished product into an oven and bake it at 110°C for 48 hours. After baking, cool it naturally in the oven and then take it out. The moisture content after baking is less than 1%.

[0058] S10, calcination system: the alumina powder is evenly spread in an energy-saving box-type electric furnace, and then the semi-finished product after drying is placed in the energy-saving box-type electric furnace for calcination; wherein the calcination conditions are set as follows: heating between room temperature and 80°C for 0.5h, and keeping warm for 0.5h; heating between 80 and 500°C for 1h, and keeping warm for 2h; heating between 800 and 1100°C for 1h, and keeping warm for 2h; heating between 1100°C and 1450°C for 1h, and keeping warm at a high temperature of 1460°C for 5h.

[0059] S11. Finished product: After the fired high-alumina brick samples are naturally cooled to room temperature by the furnace temperature, they are taken out to obtain the finished product of high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnaces made of solid waste and rare earth tailings.

[0060] The above-mentioned high thermal shock resistance rare earth composite high strength heat storage refractory bricks for hot blast furnaces using solid waste and rare earth tailings are tested as follows: The bulk density is 2.90g / cm 3 The apparent porosity is 18.69%, the water absorption is 6.45%, the compressive strength is 76.58MPa, the heat storage rate is increased by 10.11%, and the thermal shock resistance: thermal shock stability 1100℃ water cooling ≥120 times.

[0061] Example 3

[0062] The present embodiment provides a high thermal shock resistance rare earth composite high-strength heat storage refractory brick for a hot blast furnace, comprising the following raw materials in parts by weight: 20 parts of 5-3mm aggregate high alumina bauxite clinker, 25 parts of 3-1mm high alumina bauxite clinker, 15 parts of 1-0mm high alumina bauxite clinker, 17 parts of 200 mesh high alumina bauxite clinker fine powder, 15 parts of secondary aluminum ash powder, 5 parts of solid waste rare earth material powder, 2 parts of soft clay, 10 parts of thermal expansion volume stable fine powder, and 3 parts of lignin binding slurry; wherein the thermal expansion volume stable fine powder is prepared according to the mass ratio of garnet powder to sillimanite powder of 7:3.

[0063] The preparation method of the above-mentioned rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace comprises the following steps: S1. Ingredient weighing: weigh the raw materials according to the following weight proportions: 60 parts of calcined coal gangue, 35 parts of rare earth tailings, and 10 parts of cerium carbonate powder.

[0064] S2. Wet ball milling: Add weighed calcined coal gangue powder, rare earth tailings powder and cerium carbonate powder into the ball mill; the material-water ratio is 1 / 6, stir and mix thoroughly for 20 minutes; dry the material after discharge.

[0065] S3, sintering: sintering at a high temperature of 1100°C, keeping warm for 2 hours, and after cooling, putting the material into a crusher for crushing, sieving through 200 meshes, and obtaining solid waste rare earth powder.

[0066] S4. The lignin binder and tap water are stirred and mixed thoroughly and evenly using a high-speed separation stirrer in a mass ratio of 1:2.13 to obtain a binding slurry.

[0067] S5. Raw material selection: The aggregate high-alumina clinker is selected from 5~3mm high-alumina clinker, 3~1mm high-alumina clinker, 1~0mm high-alumina clinker and 200-mesh high-alumina clinker fine powder; the solid waste rare earth powder is selected from 200 mesh; the secondary aluminum ash powder is selected from 200 mesh; the soft clay is selected from 200 mesh; the andalusite powder and sillimanite powder in the thermal expansion volume stable fine powder are selected from 200 mesh and 325 mesh, respectively; package and set aside.

[0068] S6. Batching: weigh the materials according to the raw material composition ratio of the above-mentioned high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnace.

[0069] S7. Mixing and stirring: Mix the weighed aggregates of different particle sizes; at the same time, fully mix the fine powder composed of secondary aluminum ash, solid waste rare earth powder, soft clay, and thermal expansion volume stable fine powder; wherein, the mixing time of the aggregate is 3 minutes, and the mixing time of the fine powder is 2 minutes. After the aggregate is mixed, the fine powder is added and stirred for 3 minutes, and finally the prepared binding slurry is added and stirred for 6 minutes; after stirring, the mixture is packed into bags and left to stand for 5 hours for use.

[0070] S8. Pressing and molding: The uniformly mixed materials are pressed into high-alumina refractory bricks using an electric programmable screw brick press. The size of the produced high-alumina bricks is pressed according to user requirements, such as standard bricks and others; the molding pressure is 137MPa, and the molding rate is ≥98%; the semi-finished product prototype is obtained.

[0071] S9. Baking: Place the pressed semi-finished product into an oven and bake it at 110°C for 48 hours. After baking, cool it naturally in the oven and take it out. The moisture content after baking is less than 2%.

[0072] S10, calcination system: evenly spread the alumina powder in an energy-saving box-type electric furnace, and then put the dried semi-finished product into the energy-saving box-type electric furnace for calcination; the calcination conditions are set as follows: heating between room temperature and 80°C for 0.5h, and keeping warm for 1h; heating between 80 and 500°C for 1.5h, and keeping warm for 1h; heating between 800 and 1100°C for 1.5h, and keeping warm for 1h; heating between 1100°C and 1520°C for 1.5h, and keeping warm at a high temperature of 1520°C for 5h.

[0073] S11. Finished product: After the fired high-alumina brick sample is naturally cooled to room temperature by the furnace temperature, it is taken out to obtain the finished product of the high thermal shock resistance rare earth composite high-strength heat storage refractory brick for hot blast furnace made of solid waste and rare earth tailings.

[0074] The above-mentioned high thermal shock resistance rare earth composite high strength heat storage refractory bricks for hot blast furnaces using solid waste and rare earth tailings are tested as follows: The bulk density is 2.920g / cm 3 The apparent porosity is 18.50%, the water absorption is 6.34%, the compressive strength is 80.63MPa, the heat storage rate is increased by 11.12%, and the thermal shock resistance: thermal shock stability 1100℃ water cooling ≥125 times.

[0075] Example 4

[0076] The present embodiment provides a high thermal shock resistance rare earth composite high-strength heat storage refractory brick for a hot blast furnace, comprising the following raw materials in parts by weight: 15 parts of 5-3mm aggregate high alumina bauxite clinker, 25 parts of 3-1mm high alumina bauxite clinker, 20 parts of 1-0mm high alumina bauxite clinker, 15 parts of 200 mesh high alumina bauxite clinker fine powder, 17 parts of secondary aluminum ash powder, 7 parts of solid waste rare earth material powder, 4 parts of soft clay, 3 parts of thermal expansion volume stabilizing fine powder, and 5 parts of lignin binding slurry; wherein the thermal expansion volume stabilizing fine powder is prepared according to a mass ratio of 9:2 between andalusite powder and sillimanite powder.

[0077] The preparation method of the above-mentioned rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace comprises the following steps: S1. Ingredient weighing: weigh the raw materials according to the following weight proportions: 40 parts of calcined coal gangue, 40 parts of rare earth tailings, and 20 parts of cerium carbonate powder.

[0078] S2. Wet ball milling: Add weighed calcined coal gangue powder, rare earth tailings powder and cerium carbonate powder into the ball mill; the material-water ratio is 1 / 6, stir and mix thoroughly for 15 minutes; dry the material after discharge.

[0079] S3, sintering: sintering at a high temperature of 1300°C, keeping warm for 3 hours, and after cooling, putting the material into a crusher for crushing, sieving through 200 meshes, and obtaining solid waste rare earth powder.

[0080] S4. The lignin binder and tap water are stirred and mixed thoroughly and evenly using a high-speed separation stirrer in a mass ratio of 1:2.13 to obtain a binding slurry.

[0081] S5. Raw material selection: The aggregate high-alumina clinker is selected from 5~3mm high-alumina clinker, 3~1mm high-alumina clinker, 1~0mm high-alumina clinker and 200-mesh high-alumina clinker fine powder; the solid waste rare earth powder is selected from 200 mesh; the secondary aluminum ash powder is selected from 200 mesh; the soft clay is selected from 200 mesh; the andalusite powder and sillimanite powder in the thermal expansion volume stable fine powder are selected from 200 mesh and 325 mesh, respectively; package and set aside.

[0082] S6. Batching: weigh the materials according to the raw material composition ratio of the above-mentioned high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnace.

[0083] S7. Mixing and stirring: Mix the weighed aggregates of different particle sizes; at the same time, fully mix the fine powders consisting of secondary aluminum ash, solid waste rare earth powder, soft clay, and thermal expansion volume stable fine powder; wherein, the mixing time of the aggregate is 2 minutes, and the mixing time of the fine powder is 2 minutes. After the aggregates are mixed, the fine powder is added and stirred for 3 minutes, and finally the prepared binder is added and stirred for 5 minutes; after stirring, the mixture is packed into bags and left to stand for 3 hours for use.

[0084] S8. Pressing and molding: The static mixture is pressed into high-alumina refractory bricks by an electric programmable screw brick press. The size of the high-alumina bricks is pressed according to user requirements, such as standard bricks and others; the molding pressure is 137MPa, and the molding rate is ≥98%; the semi-finished product prototype is obtained.

[0085] S9, baking: put the pressed semi-finished product into an oven and bake it at 110°C for 24 hours. After baking, cool it naturally in the oven and then take it out; the moisture after baking is less than 2%.

[0086] S10, calcination system: evenly spread the alumina powder in an energy-saving box-type electric furnace, and then put the dried semi-finished product into the energy-saving box-type electric furnace for calcination; the calcination conditions are set as follows: heating between room temperature and 80°C for 0.5h, and keeping warm for 0.5h; heating between 80 and 500°C for 1.5h, and keeping warm for 2h; heating between 800 and 1100°C for 1.5h, and keeping warm for 2h; heating between 1100°C and 1480°C for 1.5h, and keeping warm at a high temperature of 1480°C for 5h.

[0087] S11. Finished product: After the fired high-alumina brick samples are naturally cooled to room temperature by the furnace temperature, they are taken out to obtain the finished product of high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnaces made of solid waste and rare earth tailings.

[0088] The above-mentioned high thermal shock resistance rare earth composite high strength heat storage refractory bricks for hot blast furnaces using solid waste and rare earth tailings are tested as follows: The bulk density is 2.66 g / cm 3 The apparent porosity is 24.44%, the water absorption is 9.33%, the compressive strength is 65MPa, the heat storage rate is increased by 12.55%, and the thermal shock resistance: thermal shock stability 1100℃ water cooling ≥102 times.

[0089] Comparative Example 1 The comparative example provides a refractory brick for a hot blast furnace, comprising the following raw materials in parts by weight: 25 parts of 5-3 mm aggregate high alumina clinker, 20 parts of 3-1 mm high alumina clinker, 10 parts of 1-0 mm high alumina clinker, 16 parts of 200 mesh high alumina clinker fine powder, 23 parts of secondary aluminum ash powder, 10 parts of solid waste rare earth material powder, 0 parts of thermal expansion volume stabilizing fine powder, and 3.5 parts of lignin binding slurry.

[0090] The preparation method of the above-mentioned rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace comprises the following steps: S1. Ingredient weighing: weigh the raw materials according to the following weight proportions: 60 parts of calcined coal gangue, 35 parts of rare earth tailings, and 5 parts of cerium carbonate powder.

[0091] S2. Wet ball milling: Add weighed calcined coal gangue powder, rare earth tailings powder and cerium carbonate powder into the ball mill; the material-water ratio is 1 / 6, stir and mix thoroughly for 15 minutes; dry the material after discharge.

[0092] S3, sintering: sintering at a high temperature of 1200°C, keeping warm for 1 hour, and after cooling, putting the material into a crusher for crushing, sieving through 200 meshes, and obtaining solid waste rare earth powder.

[0093] S4. The lignin binder and tap water are stirred and mixed thoroughly and evenly using a high-speed separation stirrer in a mass ratio of 1:2.11 to obtain a binding slurry.

[0094] S5. Raw material selection: The aggregate high-alumina clinker is selected from 5~3mm high-alumina clinker, 3~1mm high-alumina clinker, 1~0mm high-alumina clinker and 200-mesh high-alumina clinker fine powder; the solid waste rare earth powder particle size is selected from 200 mesh; the secondary aluminum ash powder is selected from 200 mesh; package and set aside.

[0095] S6. Batching: weigh the materials according to the raw material composition ratio of the above-mentioned high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnace.

[0096] S7. Mixing and stirring: Mix the weighed aggregates of different particle sizes; at the same time, fully mix the fine powder composed of secondary aluminum ash and solid waste rare earth powder; the mixing time of the aggregate is 2 minutes, and the mixing time of the fine powder is 3 minutes. After the aggregate is mixed, the fine powder is added and stirred for 2 minutes, and finally the prepared binding slurry is added and stirred for 5 minutes; after stirring, the mixture is packed into bags and left to stand for 1 hour for use.

[0097] S8. Pressing and molding: The static mixture is pressed into high-alumina refractory bricks by an electric programmable screw brick press. The size of the high-alumina bricks is pressed according to user requirements, such as standard bricks and others; the molding pressure is 137MPa, and the molding rate is ≥98%; the semi-finished product prototype is obtained.

[0098] S9, baking: put the pressed semi-finished product into an oven and bake it at 110°C for 24 hours. After baking, cool it naturally in the oven and then take it out; the moisture after baking is less than 2%.

[0099] S10, calcination system: the alumina powder is evenly spread in an energy-saving box-type electric furnace, and then the dried semi-finished product is placed in the energy-saving box-type electric furnace for calcination; wherein the calcination conditions are set as follows: heating between room temperature and 80°C for 0.5h, and keeping warm for 0.5h; heating between 80 and 500°C for 1.5h, and keeping warm for 2h; heating between 800 and 1100°C for 1.5h, and keeping warm for 2h; heating between 1100°C and 1450°C for 1h, and keeping warm at a high temperature of 1450°C for 6h.

[0100] S11. Finished product: After the fired high-alumina brick sample is naturally cooled to room temperature by the furnace temperature, the finished refractory brick is obtained by taking it out.

[0101] The above-mentioned refractory brick products for hot blast stoves are tested as follows: The bulk density is 2.59 g / cm 3 The apparent porosity is 23.01%, the water absorption is 8.7%, the compressive strength is 73.96MPa, the heat storage rate is increased by 13.82%, and the thermal shock resistance: thermal shock stability 1100℃ water cooling: 76 times.

[0102] It can be seen from the above performance test results that no thermal expansion volume stabilizing fine powder was added in Comparative Example 1, so the high temperature performance thermal shock stability was poor and the number of 1100°C water cooling times was low.

[0103] Comparative Example 2 The present embodiment provides a refractory brick for a hot blast furnace, comprising the following raw materials in parts by weight: 25 parts of 5-3 mm aggregate high alumina clinker, 20 parts of 3-1 mm high alumina clinker, 10 parts of 1-0 mm high alumina clinker, 12 parts of 200 mesh high alumina clinker fine powder, 24 parts of secondary aluminum ash powder, 0 parts of solid waste rare earth material powder, 7 parts of thermal expansion volume stable fine powder, 6 parts of soft clay, and 3.5 parts of lignin binding slurry; wherein the thermal expansion volume stable fine powder is prepared according to a mass ratio of 4:3 between andalusite powder and sillimanite powder.

[0104] The method for preparing the refractory bricks for the hot blast stove comprises the following steps: S1. The lignin binder and tap water are stirred and mixed uniformly in a mass ratio of 1:2.11 using a high-speed separation stirrer to obtain a binding slurry.

[0105] S2. Raw material selection: Aggregate high alumina clinker is selected from 5~3mm high alumina clinker, 3~1mm high alumina clinker, 1~0mm high alumina clinker and 200 mesh high alumina clinker fine powder; secondary aluminum ash powder is selected from 200 mesh; soft clay is selected from 200 mesh; andalusite powder and sillimanite powder in thermal expansion volume stable fine powder are selected from 200 mesh and 325 mesh respectively; package and set aside.

[0106] S3. Batching: weigh the materials according to the raw material composition ratio of the refractory bricks for the hot blast furnace mentioned above.

[0107] S4. Mixing and stirring: Mix the weighed aggregates of different particle sizes; at the same time, fully mix the fine powder composed of secondary aluminum ash, thermal expansion volume stable fine powder and soft clay; wherein, the mixing time of the aggregate is 2 minutes, and the mixing time of the fine powder is 3 minutes. After the aggregate is mixed, the fine powder is added and stirred for 2 minutes, and finally the prepared binding slurry is added and stirred for 5 minutes; after stirring, the mixture is packed into bags and left to stand for 1 hour for use.

[0108] S4. Pressing and molding: The static mixture is pressed into high-alumina refractory bricks by an electric programmable screw brick press. The size of the high-alumina bricks is pressed according to user requirements, such as standard bricks and others; the molding pressure is 137MPa, and the molding rate is ≥98%; the semi-finished product prototype is obtained.

[0109] S5. Baking: Place the pressed semi-finished product into an oven and bake it at 110°C for 24 hours. After baking, cool it naturally in the oven and then take it out. The moisture content after baking is less than 2%.

[0110] S5. Calcination system: evenly spread the alumina powder in an energy-saving box-type electric furnace, and then place the dried semi-finished product into the energy-saving box-type electric furnace for calcination; the calcination conditions are set as follows: heating between room temperature and 80°C for 0.5h, and keeping warm for 0.5h; heating between 80 and 500°C for 1.5h, and keeping warm for 2h; heating between 800 and 1100°C for 1.5h, and keeping warm for 2h; heating between 1100°C and 1450°C for 1h, and keeping warm at a high temperature of 1450°C for 6h.

[0111] S11. Finished product: After the fired high-alumina brick sample is naturally cooled to room temperature by the furnace temperature, the finished refractory brick is obtained by taking it out.

[0112] The above refractory brick products are tested as follows: The bulk density is 2.52g / cm 3 The apparent porosity is 24.35%, the water absorption is 8.62%, the compressive strength is 56.83MPa, and the thermal shock resistance: thermal shock stability 1100℃ water cooling ≥118 times.

[0113] It can be seen from the above performance test results that no solid waste rare earth powder was added in Comparative Example 2, so the compressive strength of the product is poorer than that of Example 1, and the bulk density is lower.

[0114] Comparative Example 3 The present embodiment provides a refractory brick for a hot blast furnace, comprising the following raw materials in parts by weight: 25 parts of 5-3 mm aggregate high alumina clinker, 20 parts of 3-1 mm high alumina clinker, 10 parts of 1-0 mm high alumina clinker, 19 parts of 200 mesh high alumina clinker fine powder, 20 parts of secondary aluminum ash powder, 0 parts of solid waste rare earth material powder, 0 parts of thermal expansion volume stable fine powder, 6 parts of calcined coal gangue, and 3.5 parts of lignin binding slurry.

[0115] The method for preparing the refractory bricks for the hot blast stove comprises the following steps: S1. The lignin binder and tap water are stirred and mixed uniformly in a mass ratio of 1:2.11 using a high-speed separation stirrer to obtain a binding slurry.

[0116] S2. Raw material selection: Aggregate high alumina clinker is selected from 5~3mm high alumina clinker, 3~1mm high alumina clinker, 1~0mm high alumina clinker and 200 mesh high alumina clinker fine powder; secondary aluminum ash powder is selected from 200 mesh; calcined coal gangue is selected from 200 mesh; package and set aside.

[0117] S3. Batching: weigh the materials according to the raw material composition ratio of the refractory bricks for the hot blast furnace mentioned above.

[0118] S4. Mixing and stirring: Mix the weighed aggregates of different particle sizes; at the same time, fully mix the high-alumina clinker fine powder, secondary aluminum ash, and calcined coal gangue fine powder; the mixing time of the aggregate is 2 minutes, and the mixing time of the fine powder is 3 minutes. After the aggregate is mixed, the fine powder is added and stirred for 2 minutes, and finally the prepared binding slurry is added and stirred for 5 minutes; after stirring, the mixture is packed into bags and left to stand for 1 hour for use.

[0119] S4. Pressing and molding: The static mixture is pressed into high-alumina refractory bricks by an electric programmable screw brick press. The size of the high-alumina bricks is pressed according to user requirements, such as standard bricks and others; the molding pressure is 137MPa, and the molding rate is ≥98%; the semi-finished product prototype is obtained.

[0120] S5. Baking: Place the pressed semi-finished product into an oven and bake it at 110°C for 24 hours. After baking, cool it naturally in the oven and then take it out. The moisture content after baking is less than 2%.

[0121] S5. Calcination system: evenly spread the alumina powder in an energy-saving box-type electric furnace, and then place the dried semi-finished product into the energy-saving box-type electric furnace for calcination; the calcination conditions are set as follows: heating between room temperature and 80°C for 0.5h, and keeping warm for 0.5h; heating between 80 and 500°C for 1.5h, and keeping warm for 2h; heating between 800 and 1100°C for 1.5h, and keeping warm for 2h; heating between 1100°C and 1450°C for 1h, and keeping warm at a high temperature of 1450°C for 6h.

[0122] S11. Finished product: After the fired high-alumina brick sample is naturally cooled to room temperature by the furnace temperature, the finished refractory brick is obtained by taking it out.

[0123] The above refractory brick products are tested as follows: The bulk density is 2.51 g / cm 3 The apparent porosity is 24.96%, the water absorption is 9.2%, the compressive strength is 52.37MPa, and the thermal shock resistance: thermal shock stability 1100℃ water cooling ≥69 times.

[0124] It can be seen from the above performance test results that in Comparative Example 3, no thermal expansion volume stable fine powder was added, and the solid waste rare earth powder was replaced with a single calcined coal gangue fine powder. Therefore, compared with Example 1, the product has poor thermal shock resistance and compressive strength, and has a low bulk density.

[0125] Comparative Example 4 The present embodiment provides a refractory brick for a hot blast furnace, comprising the following raw materials in parts by weight: 25 parts of 5-3 mm aggregate high alumina clinker, 20 parts of 3-1 mm high alumina clinker, 10 parts of 1-0 mm high alumina clinker, 19 parts of 200 mesh high alumina clinker fine powder, 20 parts of secondary aluminum ash powder, 0 parts of solid waste rare earth material powder, 0 parts of thermal expansion volume stable fine powder, 6 parts of soft clay, 5 parts of rare earth compound lanthanum carbonate powder, and 3.5 parts of lignin binding slurry.

[0126] The method for preparing the refractory bricks for the hot blast stove comprises the following steps: S1. The lignin binder and tap water are stirred and mixed uniformly in a mass ratio of 1:2.11 using a high-speed separation stirrer to obtain a binding slurry.

[0127] S2. Raw material selection: Aggregate high alumina clinker is selected from 5~3mm high alumina clinker, 3~1mm high alumina clinker, 1~0mm high alumina clinker and 200 mesh high alumina clinker fine powder; secondary aluminum ash powder is selected from 200 mesh; soft clay is selected from 200 mesh; rare earth compound lanthanum carbonate powder is selected from 200 mesh; package and set aside.

[0128] S3. Batching: weigh the materials according to the raw material composition ratio of the refractory bricks for the hot blast furnace mentioned above.

[0129] S4. Mixing and stirring: Mix the weighed aggregates of different particle sizes; at the same time, fully mix the high-alumina clinker fine powder, secondary aluminum ash, soft clay fine powder, and rare earth compound lanthanum carbonate powder; the mixing time of the aggregate is 2 minutes, and the mixing time of the fine powder is 3 minutes. After the aggregate is mixed, the fine powder is added and stirred for 2 minutes, and finally the prepared binding slurry is added and stirred for 5 minutes; after stirring, the mixture is packed into bags and left to stand for 1 hour for use.

[0130] S4. Pressing and molding: The static mixture is pressed into high-alumina refractory bricks by an electric programmable screw brick press. The size of the high-alumina bricks is pressed according to user requirements, such as standard bricks and others; the molding pressure is 137MPa, and the molding rate is ≥98%; the semi-finished product prototype is obtained.

[0131] S5. Baking: Place the pressed semi-finished product into an oven and bake it at 110°C for 24 hours. After baking, cool it naturally in the oven and then take it out. The moisture content after baking is less than 2%.

[0132] S5. Calcination system: evenly spread the alumina powder in an energy-saving box-type electric furnace, and then place the dried semi-finished product into the energy-saving box-type electric furnace for calcination; the calcination conditions are set as follows: heating between room temperature and 80°C for 0.5h, and keeping warm for 0.5h; heating between 80 and 500°C for 1.5h, and keeping warm for 2h; heating between 800 and 1100°C for 1.5h, and keeping warm for 2h; heating between 1100°C and 1450°C for 1h, and keeping warm at a high temperature of 1450°C for 6h.

[0133] S11. Finished product: After the fired high-alumina brick sample is naturally cooled to room temperature by the furnace temperature, the finished refractory brick is obtained by taking it out.

[0134] The above refractory brick products are tested as follows: The bulk density is 2.57 g / cm 3 The apparent porosity is 23.47%, the water absorption is 8.67%, the compressive strength is 61.9MPa, and the thermal shock resistance: thermal shock stability 1100℃ water cooling ≥71 times.

[0135] It can be seen from the above performance test results that in Comparative Example 4, no thermal expansion volume stabilizing fine powder was added, and the solid waste rare earth powder was replaced with a single rare earth compound lanthanum carbonate powder. Therefore, compared with Example 1, the product has poorer thermal shock resistance and pressure resistance.

[0136] In summary, the main raw material aggregate high-alumina clinker in Examples 1-4 of the present invention is widely distributed and easily available. High-alumina clinker is prepared by high-temperature calcination of bauxite ore. The reserves of high-alumina bauxite in my country are about more than 1 billion tons, and its production areas are mainly in Shanxi, Henan and Guizhou. Secondary aluminum ash and calcined coal gangue are solid wastes, and there are many production companies. Rare earth tailings are mainly produced in Baotou, Inner Mongolia, Ganzhou, Jiangxi, Mianning, Sichuan and other places. my country's andalusite resources are mainly distributed in Henan, Xinjiang, Shaanxi, Jilin and other regions. The raw materials used are widely distributed and easily available.

[0137] The formula of the present invention contains solid waste rare earth powder, which enhances the bonding effect between particles inside the material, increases the density of high-alumina refractory materials, and improves the mechanical properties. Solid waste rare earth powder promotes the nucleation and growth of high-alumina refractory grains, and improves the refractoriness and thermal shock stability of the material. Sillimanite and andalusite powder are doped in the formula, and their different decomposition temperatures and expansibility are utilized under a suitable calcination process, so that the high-alumina refractory products have expansion caused by the decomposition of unconverted crystals at industrial use temperatures, so that a certain stress is generated inside the refractory material, which plays a role in resisting loads and enhancing creep resistance and thermal shock resistance.

[0138] The high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnaces prepared by using solid waste and rare earth compounds provided by the present invention have high pressure resistance, excellent thermal shock resistance, improved heat storage rate, extended service life of high-temperature kiln hot blast furnaces, and reduced repair and maintenance costs. The formula of the present invention utilizes solid waste secondary aluminum ash, calcined coal gangue, and rare earth tailings, saving production costs, making full use of resources, turning waste into treasure, and having good economic and social benefits.

[0139] The present invention provides a method for preparing high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnaces using solid waste and rare earth tailings, and preparing solid waste rare earth powder by wet ball milling and sintering. Combined with the unique formulation of the slurry, a high-speed separation stirrer is used to stir evenly, and then a hydrometer is used to test and add it after it meets the requirements. Strictly control the sequence and duration of the stirring process: the aggregate is stirred separately in the mixer for 1 to 2 minutes, the fine powder is stirred separately for 2 to 3 minutes, the aggregate is stirred evenly and then stirred together with the fine powder for 2 to 3 minutes, and finally the prepared binder is added for stirring, and the stirring time is 4 to 6 minutes; after stirring, it is packed into a bag, sealed and left to stand for 1 hour to 5 hours.

[0140] The pressing adopts EPK-630 electric program-controlled screw brick press with a pressing force of 137MPa. The calcination process adopts a unique multi-gradient heating and insulation system to promote the reaction and sintering of materials in different temperature zones: heating between room temperature and 80°C for 0.5h, insulation for 0.5~1h; heating between 80~500°C for 1~1.5h, insulation for 1~2h; heating between 800~1100°C for 1~1.5h, insulation for 1~2h; heating between 1100°C and the highest temperature for 1~1.5h, insulation for 5~6h at the highest temperature of 1450°C~1520°C. After the product of the present invention is prepared, the relevant performance test is carried out according to the national standard method.

[0141] The high thermal shock resistance rare earth composite high-strength heat storage refractory brick for blast furnace hot blast furnace provided by the present invention has a firing temperature range of 1450-1520°C, and the firing temperature of a high thermal shock resistance high-strength high-alumina brick for blast furnace hot blast furnace is low, and the energy consumption is small. Rare earth lanthanum oxide cerium has a certain fluxing and sintering effect, which reduces energy consumption and is beneficial to the improvement of the compressive strength of high-alumina bricks. Andalusite and sillimanite materials have the characteristics of small thermal expansion coefficient, improved room temperature pressure resistance, sintering densification, etc., which are helpful to improve the thermal shock resistance stability of high-alumina bricks.

[0142] The high thermal shock resistance rare earth composite high strength heat storage refractory brick for blast furnace hot blast furnace provided by the present invention has a volume density range of: 2.58~2.92g / cm 3 The compressive strength range is 65~80.63Mpa, the water absorption range is: 6.34%~10.71%, the heat storage rate is improved: 10.11%~13.60%, and the thermal shock resistance is: 1100℃ water cooling>102 times~125 times. The product has high volume density, high compressive strength, high thermal shock resistance and high heat storage.

[0143] High-alumina refractory bricks for hot blast furnaces have high strength and extend the service life of high-alumina refractory bricks for hot blast furnaces in rapid cooling and heating scenarios, with high heat storage rate; while comprehensively utilizing solid waste, it broadens the application field of rare earth products. It provides a new market path for high-alumina refractory bricks for hot blast furnaces.

[0144] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0145] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace, characterized in that: The raw materials include the following parts by weight: 65-80 parts of aggregate high-alumina clinker, 10-20 parts of secondary aluminum ash powder, 5-10 parts of solid waste rare earth powder, 0-4 parts of soft clay, 3-11 parts of thermal expansion volume stable fine powder, and 3-5 parts of binding slurry; The binding slurry is prepared by mixing a lignin binder and water.

2. The high thermal shock resistance rare earth composite high strength heat storage refractory brick for hot blast furnace according to claim 1, characterized in that: The aggregate high-alumina bauxite clinker includes the following raw materials in parts by weight: 15-25 parts of 5-3 mm high-alumina bauxite clinker, 15-25 parts of 3-1 mm high-alumina bauxite clinker, 10-25 parts of 1-0 mm high-alumina bauxite clinker, and 5-17 parts of 200 mesh high-alumina bauxite clinker fine powder.

3. The high thermal shock resistance rare earth composite high strength heat storage refractory brick for hot blast furnace according to claim 1, characterized in that: The solid waste rare earth powder comprises the following raw materials in parts by weight: 40-65 parts of calcined coal gangue, 30-40 parts of rare earth tailings, and 5-20 parts of lanthanum carbonate or cerium carbonate powder.

4. The high thermal shock resistance rare earth composite high strength heat storage refractory brick for hot blast furnace according to claim 1, characterized in that: The soft clay is specifically at least one of Su clay and Guangxi white mud; the thermal expansion volume stable fine powder is specifically a mixed powder of andalusite powder and sillimanite powder, and the mass ratio of the andalusite powder to the sillimanite powder is 4:3~9:

2.

5. The high thermal shock resistance rare earth composite high strength heat storage refractory brick for hot blast furnace according to claim 1, characterized in that: The binding slurry is specifically made of lignin and tap water in a mass ratio of 1:2.11-2.

13.

6. A method for preparing a rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for a hot blast stove according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Ingredient weighing: weigh the following raw materials in parts by weight: 40-65 parts of calcined coal gangue, 30-40 parts of rare earth tailings, and 5-20 parts of lanthanum carbonate or cerium carbonate powder; S2, wet ball milling: adding weighed calcined coal gangue powder, rare earth tailings powder, lanthanum carbonate or cerium carbonate powder into a ball mill, stirring and wet ball milling, and drying after discharging; S3, sintering and crushing: the dried material in S2 is sintered at high temperature, and then crushed and sieved to obtain solid waste rare earth powder; S4, fully and evenly stirring and mixing the lignin binder and water to obtain a binding slurry; S5. Ingredients: weigh the raw material ratio of the rare earth composite high-strength heat storage refractory bricks for hot blast furnaces according to any one of claims 1 to 5; S6, mixing and stirring: stir and mix the weighed aggregate high-alumina clinker; at the same time, add the secondary aluminum ash powder, solid waste rare earth powder, soft clay, thermal expansion volume stable fine powder, and binding slurry in sequence, stir and mix thoroughly, and let stand for use after stirring; S7, pressing and molding: pressing the mixed raw materials after standing with high-alumina refractory bricks to obtain a semi-finished product initial form; S8, baking: putting the semi-finished product into an oven for baking, and taking it out after naturally cooling it in the oven after baking; S9, calcination system: evenly spread the alumina powder in an energy-saving box-type electric furnace, and then put the dried semi-finished product into the energy-saving box-type electric furnace for calcination; S10. Finished product: After the fired high-alumina refractory brick samples are naturally cooled to room temperature by the furnace temperature, they are taken out to obtain high thermal shock resistance rare earth composite high-strength heat storage refractory bricks for hot blast furnaces made from solid waste and rare earth tailings.

7. The method for preparing a rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace according to claim 6, characterized in that: The material-water ratio in wet ball milling in S2 is 1 / 6, and the stirring time is 15-20 min; The sintering temperature in S3 is 950~1300℃, and the temperature is kept for 1~3h. After cooling, the sintered steel is put into a crusher for crushing, and then passed through a 200-mesh sieve; In S4, the lignin binder and water are mixed in a mass ratio of 1:2.11-2.

13.

8. The method for preparing a rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace according to claim 6, characterized in that: Before batching S5, raw material selection is required: aggregate high-alumina clinker, secondary aluminum ash powder, solid waste rare earth powder, soft clay, thermal expansion volume stable fine powder are graded to determine different particle sizes; Among them, the aggregate high-alumina bauxite clinker is selected from 5~3mm high-alumina bauxite clinker, 3~1mm high-alumina bauxite clinker, 1~0mm high-alumina bauxite clinker and 200-mesh high-alumina bauxite clinker fine powder; the solid waste rare earth material powder particle size is selected from 200 mesh; the secondary aluminum ash powder is selected from 200 mesh; the soft clay is selected from 200 mesh; the andalusite powder in the thermal expansion volume stable fine powder is selected from 200 mesh and the sillimanite powder is selected from 325 mesh; In S5, the aggregate high-alumina bauxite clinker is prepared according to the following weight fractions: 15-25 parts of 5-3mm high-alumina bauxite clinker, 15-25 parts of 3-1mm high-alumina bauxite clinker, 10-25 parts of 1-0mm high-alumina bauxite clinker, and 5-17 parts of 200-mesh high-alumina bauxite clinker fine powder; the thermal expansion volume stable fine powder is prepared according to the mass ratio of garnet powder to sillimanite powder of 4:3-9:

2.

9. The method for preparing a rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace according to claim 6, characterized in that: Aggregate mixing time in S6: 1~3min, fine powder mixing time: 2~3min, wherein the fine powder is composed of secondary aluminum ash powder, solid waste rare earth powder, soft clay, thermal expansion volume stable fine powder; after the aggregate is evenly mixed, it is mixed with the fine powder for 2~3min, and finally the prepared binding slurry is added for mixing, and the mixing time is 4min~6min; after mixing, it is packed into bags and left to stand for 1h~5h for use; The molding pressure of S7 is 137MPa, and the molding rate is ≥98%; In S8, the baking temperature is 110°C, the baking time is 24h~48h, and it needs to be baked until the moisture content is less than 2%.

10. The method for preparing a rare earth composite high-strength heat storage refractory brick with high thermal shock resistance for hot blast furnace according to claim 6, characterized in that: The specific calcination conditions in S9 are as follows: heating between room temperature and 80°C for 0.5 h, and keeping warm for 0.5~1 h; heating between 80~500°C for 1~1.5 h, and keeping warm for 1~2 h; heating between 800~1100°C for 1~1.5 h, and keeping warm for 1~2 h; heating between 1100°C and the highest temperature for 1~1.5 h, and keeping warm for 5~6 h at the highest temperature of 1450°C~1520°C.

Citation Information

Patent Citations

  • Bauxite composite refractory brick and preparation method and application thereof

    CN106187238A

  • A method for preparing a phosphorus removal agent based on rare earth modified coal gangue

    CN116809034A

  • Low-viscosity rare earth aluminosilicate as well as preparation method and application thereof

    CN117486225A

  • Lightweight high-strength aggregate prepared from rare earth coupled solid waste and preparation method thereof

    CN117623739A

  • Special acid resistant refractory brick and production method thereof

    WO2012119332A1