Zirconium-free flow control refractory material and manufacturing method thereof
Through the formulation and firing process of zirconium-free component flow-controlled refractory materials, the problems of shortage of zirconium ore resources and high import average price are solved, and efficient and low-cost corrosion-resistant and anti-shock-resistant refractory materials are provided, which is suitable for the metallurgical industry. It extends its service life and promotes resource recycling.
Patent Information
- Application Number
- CN202411152264.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
China's zirconium ore resources are insufficient, resulting in the upstream of the zirconium industry chain relying on imports. The existing current-controlled refractory materials all contain zirconium components and cannot meet the demand under high average import prices. There is a lack of alternative materials that are zirconium-free but have the same functions.
Adopt zirconium-free flow-controlled refractory formula, including recycled corundum kiln tools, electromelted magnesium-aluminum spinel, 95 ceramic parts, silicon carbide silo bowls for recycled new energy lithium batteries, steel mill recycling waste bricks, cooked alumina, plates Corundum, active α-Al2O3 micro powder, industrial aluminum sheet, silicon carbide powder, graphite electrode powder, Yixing white mud and magnesium silicon chelating agent, combined with thermosetting liquid bonding agent, it is prepared with good quality through specific particle grading and firing processes. Resistant material that is resistant to corrosion and flush.
It has achieved a service life of more than 50%, low cost, saving non-renewable resources, and has significant market competitiveness. It is suitable for the metallurgical industry, reducing the consumption of non-renewable resources, and promoting the recycling of waste resources.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of inorganic non-metallic materials for steel mills in the metallurgical field, and more specifically to a zirconium-free flow-control refractory and a manufacturing method thereof. Background Art
[0003] Zirconium is a rare metal, but its abundance in the earth is greater than that of copper, nickel, lead and zinc. It is called a rare metal because there are few independent zircon deposits. At present, there are 38 independent zircon minerals known, which can be divided into three categories. One is zircon in the form of zircon silicate, the other is baddeleyite in the form of oxide, and there are also heterogeneous stone, sodium zircon and zircon-tantalum ore in the form of zircon silicate containing titanium, niobium, tantalum and other elements. The taste of zirconium dioxide in these minerals varies greatly, ranging from 4% to 99%. Zirconium products mainly include zirconium silicate, zirconium oxychloride, zirconium dioxide, composite zirconium oxide and ceramic structural parts, which are used in strategic emerging industries such as modern ceramics, special glass, atomic energy industry, as well as various industrial fields such as chemical industry, precision casting and medical treatment.
[0004] In terms of the development background of zirconium ore in my country, the overall zirconium industry in my country is mainly based on midstream refining and downstream processing. At present, the technology and patents of China's zirconium industry are concentrated in the fields of refining and processing. In the next ten years, China's demand for zirconium ore resources will remain large, and the domestic zirconium ore resource consumption structure will also undergo a major change, from the traditional zirconium silicate ceramic industry to the high-quality zirconium chemical products and precision casting industries. However, China's recoverable reserves of zirconium ore resources are insufficient, and the output of zircon sand mined and produced domestically is far from meeting domestic demand. China's zircon sand supply relies heavily on imports.
[0005] The upstream link of the zirconium industry chain is ore dressing and refining. The product after preliminary ore washing is zircon sand. Since zirconium ore is non-renewable, irreplaceable and non-reusable, and more than 70% of China's zirconium ore resources are primary zirconium ore resources, they have not yet been fully mined and utilized due to the difficulty of ore dressing and high mining costs. The actual recoverable reserves are seriously insufficient, and the mined coastal sand ore deposits can only meet part of the production and processing needs of the domestic zircon industry, resulting in the upstream zircon ore basically relying on imports; zircon sand is prepared through related processes to obtain midstream products, mainly zirconium oxychloride, chemical zirconium dioxide, fused zirconium oxide, zirconium silicate, composite zirconium oxide, etc.
[0006] In terms of the current status and scale of domestic zirconium ore supply and demand, the overall domestic supply and demand are greatly misaligned, and the degree of import dependence is extremely high. As the overall zirconium ore demand and price fluctuations increase, the overall zirconium ore market size fluctuates and rises. The overall supply decline has exacerbated the overall supply and demand situation, further leading to an increase in the overall average import price of zirconium concentrate. At the same time, the import volume fluctuated slightly and decreased, and due to the recovery of demand, it increased significantly in 2022, and the price rose sharply again in early 2024.
[0007] The flow control refractory materials used in the prior art contain zirconium components in order to achieve physical and chemical properties. With the overall average price of imported zirconium concentrate rising, there is a lack of flow control refractory materials that do not use zirconium but can meet the usage standards. Summary of the invention
[0008] In order to solve the above problems, the present invention provides a zirconium-free flow-control refractory material and its manufacturing method which has good corrosion resistance and erosion resistance, a service life increased by more than 50% compared with the original zirconium oxide component, low cost, and saves non-renewable resources.
[0009] According to one aspect of the present invention, a zirconium-free flow-control refractory material comprises the following components in percentage by weight: 6% to 10% of recycled corundum kiln furniture, 22% to 24% of fused magnesium aluminum spinel, 7% to 11% of 95 ceramic parts, 4% to 6% of silicon carbide saggers for lithium batteries for renewable energy, 4% to 8% of recycled waste bricks from steel mills, 4% to 9% of slaked alumina, 13% to 19% of plate-shaped corundum, 5% to 8% of active α-Al2O3 micropowder, 2% to 4% of industrial aluminum sheets, 2% to 4% of silicon carbide powder, 2% to 4% of graphite electrode powder, 3% to 5% of Yixing white mud, and 4% to 6% of magnesium silicon chelating agent. The sum of the weights of all the components in the above formula is 100%, and 4% to 5% of thermosetting liquid binder is added.
[0010] In some embodiments, the particle grading of each component is as follows: the particle diameter of regenerated corundum kiln furniture is 5-3 mm, the particle diameter of fused magnesium aluminum spinel is 3-2, 2-1, 1-0 mm, the particle diameter of 95 ceramic parts is 3-1 mm, the particle diameter of silicon carbide sagger for lithium batteries for renewable energy is 3-1 mm, the particle diameter of waste bricks recycled from steel mills is 1-0 mm, the particle diameter of slaked alumina is 1-0 mm, the particle diameter of plate-like corundum is 325 mesh, the active α-Al2O3 powder is 5 um, the industrial aluminum sheet is 250 mesh, the silicon carbide powder is 240 mesh, the graphite electrode powder is 180 mesh, the Yixing white mud is 200 mesh, and the magnesium silicon chelating agent is 200 mesh; the thermosetting binder is liquid.
[0011] In some embodiments, the fused magnesia-alumina spinel particle size distribution is as follows:
[0012] 3~2㎜ 9%~12%
[0013] 2~1㎜ 5%~8%
[0014] 1~0㎜ 6%~10%.
[0015] In some embodiments, the total weight percentage of the particle grading of the fused magnesia-alumina spinel is 21% to 30%.
[0016] In some embodiments, the regenerated corundum kiln furniture has: Al2O3 content ≥ 85%, SiO2 content ≤ 10%;
[0017] The fused magnesium-aluminum spinel has an Al2O3 content of 71-75%, a MgO content of 22-27%, a SiO2 content of <0.4%, a Fe2O3 content of ≤0.4%, and a CaO content of ≤0.6%;
[0018] The 95 ceramic parts: Al2O3 content ≥ 95%, Fe2O3 content ≤ 0.8%;
[0019] The silicon carbide sagger for lithium battery used for renewable energy: SiC content ≥ 80%, SiO2 content ≤ 15%;
[0020] The steel mill recycled waste bricks: Al2O3 content ≥ 80%, Fe2O3 content < 1%, SiO2 content ≤ 15%;
[0021] The calcined alumina has an Al2O3 content of ≥85% and a Fe2O3 content of ≤0.4%;
[0022] The plate-shaped corundum has an Al2O3 content of ≥99.5% and a Fe2O3 content of ≤0.4%;
[0023] The active α-Al2O3 micro powder has Al2O3 content ≥ 99% and Fe2O3 content ≤ 0.3%;
[0024] The industrial aluminum sheet: active aluminum Al≥96%;
[0025] The silicon carbide powder: SiC content ≥ 98%;
[0026] The graphite electrode powder: C content ≥ 97%;
[0027] The Yixing white mud: Al2O3 content ≥ 33%, Fe2O3 content ≤ 1.5%;
[0028] The magnesium-silicon chelating agent has a MgO content of 52-60% and a SiO2 content of 40-48%;
[0029] The thermosetting binder has a residual carbon content of 43±5%, a solid content of 70-83%, and a viscosity of 16000-18000 MPa.
[0030] According to one aspect of the present invention, a method for manufacturing a zirconium-free flow control refractory is characterized by comprising the following steps:
[0031] S1: Ingredients, weighed in proportion: recycled corundum kiln furniture, fused magnesium aluminum spinel, 95 ceramic parts, lithium battery silicon carbide sagger for renewable energy, recycled waste bricks from steel mills, slaked alumina, plate-shaped corundum, active α-Al2O3 powder, industrial aluminum sheet, silicon carbide powder, graphite electrode powder, Yixing white mud and magnesium silicon chelating agent;
[0032] S2: mixing, mixing the raw materials in S1 with the liquid binder;
[0033] S3: molding, using a mold to mold the uniformly mixed raw materials;
[0034] S4: Natural drying: place the formed refractory body in a natural environment to dry for 12-24 hours;
[0035] S5: Heating and drying, placing the formed refractory body into a drying kiln and slowly heating and drying for 32 to 51 hours;
[0036] S6: Firing: Push the dried green body into a medium-high temperature tunnel kiln and evenly heat it to 580℃±30℃, keep it warm for 15 to 20 hours, and finally cool it down to room temperature at a uniform speed before taking it out of the kiln;
[0037] S7: Inspection and warehousing: inspect the refractory materials and pack and store qualified products.
[0038] In some embodiments, the drying process is as follows: the drying kiln temperature is uniformly increased to 80°C within 1 hour, and kept at 80°C for 15 hours, and then the temperature is uniformly increased from 80°C to 180°C within 20 hours, and kept at 180°C for 15 hours.
[0039] In some embodiments, during the firing process, the temperature is uniformly raised to 580° C.±30° C. within 15 to 20 hours, and then uniformly lowered to room temperature.
[0040] Compared with the prior art, the beneficial effects of the present invention are: good corrosion resistance and erosion resistance, service life increased by more than 50% compared with the original zirconium oxide component, low cost, and saving of non-renewable resources. In the present invention, because the flow control refractory does not contain high zirconium oxide components, the cost is very low, which is conducive to market price competition and has obvious advantages in market competitiveness; the service life of the flow control refractory is increased by more than 50% compared with the original zirconium oxide component; the flow control refractory can achieve energy saving and consumption reduction for the steel industry, smelt fine steel and high-quality steel, and increase benefits, playing an irreplaceable role; using renewable resources, optimizing production process flow, carrying out energy-saving transformation, selecting high-efficiency energy-saving technology and equipment, recycling, giving full play to the synergistic carbon reduction effect of comprehensive utilization of large solid waste to replace natural resources, forming a carbon reduction demonstration effect of waste refractory industry; causing the industry to pay attention to waste refractory resources, strengthen the recycling of waste resources, and locally adopt a large amount of recycled waste recycling refractory with an amount greater than 50%, which greatly reduces costs while saving non-renewable resources. DETAILED DESCRIPTION
[0041] The present invention is described in detail below in conjunction with various embodiments, but it should be noted that these embodiments are not limitations of the present invention, and equivalent changes or substitutions in functions, methods or structures made by ordinary technicians in the field based on these embodiments are all within the scope of protection of the present invention.
[0042] In the description of the present invention, it should be noted that, unless otherwise specified and limited, the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a mechanical connection or an electrical connection, or it can be the internal connection of two components. It can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meaning of the terms can be understood according to the specific circumstances.
[0043] The zirconium-free flow-control refractory material described in the present invention comprises the following components in percentage by weight: 6% to 10% of recycled corundum kiln furniture, 22% to 24% of fused magnesium aluminum spinel, 7% to 11% of 95 ceramic parts, 4% to 6% of silicon carbide saggers for lithium batteries for renewable energy, 4% to 8% of recycled waste bricks from steel mills, 4% to 9% of slaked alumina, 13% to 19% of plate-shaped corundum, 5% to 8% of active α-Al2O3 micropowder, 2% to 4% of industrial aluminum sheets, 2% to 4% of silicon carbide powder, 2% to 4% of graphite electrode powder, 3% to 5% of Yixing white mud, and 4% to 6% of magnesium silicon chelating agent. The sum of the weights of all the components in the above formula is 100%, and 4% to 5% of thermosetting liquid binder is added.
[0044] The particle grading of each component is as follows: the particle diameter of recycled corundum kiln furniture is 5-3mm, the particle diameter of fused magnesium aluminum spinel is 3-2, 2-1, 1-0mm, the particle diameter of 95 ceramic parts is 3-1mm, the particle diameter of silicon carbide sagger for lithium batteries for renewable energy is 3-1mm, the particle diameter of waste bricks recycled from steel mills is 1-0mm, the particle diameter of slaked alumina is 1-0mm, the particle diameter of plate-like corundum is 325 mesh, the active α-Al2O3 powder is 5um, the industrial aluminum sheet is 250 mesh, the silicon carbide powder is 240 mesh, the graphite electrode powder is 180 mesh, the Yixing white mud is 200 mesh, and the magnesium silicon chelating agent is 200 mesh; the thermosetting binder is liquid.
[0045] The particle size distribution of fused magnesia-alumina spinel is as follows:
[0046] 3~2㎜ 9%~12%
[0047] 2~1㎜ 5%~8%
[0048] 1~0㎜ 6%~10%.
[0049] The sum of the weight percentages of the particle grading of the fused magnesia-alumina spinel is 21% to 30%.
[0050] Regenerated corundum kiln furniture: Al2O3 content ≥85%, SiO2 content ≤10%;
[0051] Fused magnesium aluminate spinel: Al2O3 content 71-75%, MgO content 22-27%, SiO2 content <0.4%, Fe2O3 content ≤0.4%, CaO content ≤0.6%;
[0052] 95 Ceramic parts: Al2O3 content ≥95%, Fe2O3 content ≤0.8%;
[0053] Silicon carbide sagger for lithium battery for renewable energy: SiC content ≥ 80%, SiO2 content ≤ 15%;
[0054] Steel plant recycled waste bricks: Al2O3 content ≥80%, Fe2O3 content <1%, SiO2 content ≤15%;
[0055] Burnt alumina: Al2O3 content ≥85%, Fe2O3 content ≤0.4%;
[0056] Tabular corundum: Al2O3 content ≥ 99.5%, Fe2O3 ≤ 0.4%;
[0057] Active α-Al2O3 powder: Al2O3 content ≥99%, Fe2O3 ≤0.3%;
[0058] Industrial aluminum sheet: active aluminum Al ≥ 96%;
[0059] Silicon carbide powder: SiC content ≥98%;
[0060] Graphite electrode powder: C content ≥ 97%;
[0061] Yixing white mud: Al2O3 content ≥33%, Fe2O3 content ≤1.5%;
[0062] Magnesium-silicon chelating agent: MgO content 52-60%, SiO2 content 40-48%;
[0063] Thermosetting binder: residual carbon content 43±5%, solid content 70-83%, viscosity 16000-18000mpa.
[0064] Magnesium-silicon chelating agent:
[0065] The performance of refractory binders is not only related to the construction and dispersion performance of refractory materials, but also its existence form at high temperature will have an important impact on the service life of refractory materials. Compared with conventional binders such as cement and aluminum gel powder, SiO2 powder is an important binder for magnesium castables and machine pressing. It forms a MgO-SiO2-H2O network binding system with magnesium oxide, thereby generating strength.
[0066] There are mainly the following problems in the hydration process:
[0067] 1. After hydration, MgO powder can form magnesium hydroxide covering the surface of magnesium oxide particles, which hinders the further development of hydration and is not conducive to improving strength;
[0068] 2. The fineness of silicon micropowder is usually below 1um, and there are problems such as uneven dispersion and low hydration efficiency. Introduction to the role of magnesium silicon chelating agent:
[0069] Chelating agents can make multiple metal atoms or ions form a complex with a ring structure, which is called a chelate. Magnesium-silicon chelating agents can effectively prevent magnesium and calcium metal ions from forming precipitates during chemical reactions. This promotes the continuous hydration of magnesium oxide and silicon oxide, improves the strength of the MgO-SiO2-H2O network-like bonding system, and significantly improves the various indicators of mechanically pressed products after high temperature.
[0070] According to one aspect of the present invention, a method for manufacturing a zirconium-free flow control refractory is characterized by comprising the following steps:
[0071] S1: Ingredients, weighed in proportion: recycled corundum kiln furniture, fused magnesium aluminum spinel, 95 ceramic parts, lithium battery silicon carbide sagger for renewable energy, recycled waste bricks from steel mills, slaked alumina, plate-shaped corundum, active α-Al2O3 powder, industrial aluminum sheet, silicon carbide powder, graphite electrode powder, Yixing white mud and magnesium silicon chelating agent;
[0072] S2: mixing, mixing the raw materials in S1 with the liquid binder;
[0073] S3: molding, using a mold to mold the uniformly mixed raw materials;
[0074] S4: Natural drying: place the formed refractory body in a natural environment to dry for 12-24 hours;
[0075] S5: Heating and drying, placing the formed refractory body into a drying kiln and slowly heating and drying for 32 to 51 hours;
[0076] S6: Firing: Push the dried green body into a medium-high temperature tunnel kiln and evenly heat it to 580℃±30℃, keep it warm for 15 to 20 hours, and finally cool it down to room temperature at a uniform speed before taking it out of the kiln;
[0077] S7: Inspection and warehousing: inspect the refractory materials and pack and store qualified products.
[0078] The process of heating and drying is as follows: the temperature of the drying kiln is uniformly raised to 80°C within 1 hour, and kept at 80°C for 15 hours, and then the temperature is uniformly raised from 80°C to 180°C within 20 hours, and kept at 180°C for 15 hours.
[0079] During the firing process, the temperature is evenly raised to 580°C ± 30°C within 15 to 20 hours, and finally lowered to room temperature at a uniform rate.
[0080] The production process requirements of zirconium-free flow control refractory materials are as follows:
[0081] (1) The ingredients should be weighed strictly according to the proportion, the fine powder should be mixed evenly, and when mixing the powder, the additives should be added between the materials. The mixed powder stirred by the mixer should be checked for uniform chemical composition;
[0082] (2) The temperature of the materials mixed by the wet mill or high-speed mixer should be controlled to prevent the material temperature from being too high or too low, which will affect the plasticity and molding adhesion of the mixed materials. In winter, insulation measures should be taken, and in summer, the temperature of the storage room should be lowered as much as possible, preferably around 25°C, with a humidity of about 50%;
[0083] (3) During molding, the pressure should be light first and then heavy, and the mold cavity should be vented to avoid layer cracking; check the curvature of the bottom cover of the mold frequently to prevent the deformation of the flow control refractory material without zirconium component and cause waste;
[0084] (4) Strictly control the temperature rise curve during the firing process. The temperature must be lowered slowly and evenly to prevent cracks.
[0085] (5) When grinding flow-control refractory materials without zirconium components, the parallelism and flatness must be strictly controlled;
[0086] (6) Zirconium-free flow control refractory materials should be handled with care during processing, transportation or shot blasting. When fixing or hooping, they should be gently tapped with a wooden hammer or rubber hammer. Iron hammers are prohibited.
[0087] Embodiment 1:
[0088] The raw material specifications are as follows:
[0089] Regenerated corundum kiln furniture: Al2O3 content ≥85%, SiO2 content ≤10%;
[0090] Fused magnesium aluminate spinel: Al2O3 content 71-75%, MgO content 22-27%, SiO2 content <0.4%, Fe2O3 content ≤0.4%, CaO content ≤0.6%;
[0091] 95 Ceramic parts: Al2O3 content ≥95%, Fe2O3 content ≤0.8%;
[0092] Silicon carbide sagger for lithium battery for renewable energy: SiC content ≥ 80%; SiO2 content ≤ 15%;
[0093] Steel plant recycled waste bricks: Al2O3 content ≥80%, Fe2O3 content <1%, SiO2 content ≤15%;
[0094] Burnt alumina: Al2O3 content ≥85%, Fe2O3 content ≤0.4%;
[0095] Tabular corundum: Al2O3 content ≥ 99.5%, Fe2O3 ≤ 0.4%;
[0096] Active α-Al2O3 powder: Al2O3 content ≥99%, Fe2O3 ≤0.3%;
[0097] Industrial aluminum sheet: active aluminum Al ≥ 96%;
[0098] Silicon carbide powder: SiC content ≥98%;
[0099] Graphite electrode powder: C content ≥ 97%;
[0100] Yixing white mud: Al2O3 content ≥33%, Fe2O3 content ≤1.5%;
[0101] Magnesium-silicon chelating agent: MgO content 52-60%, SiO2 content 40-48%,
[0102] Thermosetting binder: residual carbon content 43±5%, solid content 70-83%, viscosity 16000-18000mpa.
[0103] The basic production process of the zirconium-free flow control refractory product of the present invention is: according to the formula in Table 1 below, regenerated corundum kiln furniture, fused magnesium aluminum spinel, 95 ceramic parts, lithium battery silicon carbide sagger for renewable energy, slaked alumina, and waste bricks recycled from steel mills are crushed and screened and mixed according to the formula in Table 1, added to a wet mill or a high-speed mixer and mixed for 3 to 6 minutes, a binder is added, and after mixing, the following fine powders are added: plate-shaped corundum, active α-Al2O3 micropowder, magnesium silicon chelating agent, silicon carbide powder, graphite electrode powder, Yixing white mud, and industrial aluminum flakes are mixed for 10 to 30 minutes and discharged. The molding adopts a screw brick press of more than 1,000 tons, and the materials are accurately weighed according to the shape and size of the bricks. The weighed materials are added to the mold and molded to the specified size. The overall dimensions, flatness, and diagonal dimensions of each brick are measured, and 50% of the unit weight is sampled in each shift. The porosity and volume density of each car of bricks are tested. Any unqualified phenomenon must be scrapped and the cause is found. The formed bricks generally need to be naturally dried before entering the drying kiln. The bricks are placed in the dryer, then formed and dried naturally, and then placed in the drying kiln for slow heating and drying for 32 to 51 hours. The temperature of the drying kiln should not exceed 180°C. Then, they are pushed into the medium-high temperature tunnel kiln and evenly heated to 580°C ± 30°C, kept warm for 15 to 20 hours, and finally cooled to room temperature at a uniform rate. The slow heating and drying process is preferably: the temperature of the drying kiln is evenly raised to 80°C within 1 hour, and kept at 80°C for 15 hours, and then the temperature is evenly raised from 80°C to 180°C within 20 hours, and kept at 180°C for 15 hours. The temperature is evenly raised to 580°C ± 30°C within 15 to 20 hours, and finally cooled to room temperature at a uniform rate. In order to improve the performance of zirconium-free flow-control refractory materials and prevent the generation and expansion of cracks, it is necessary to use steel strips to tie the periphery of the flow-control refractory materials and wrap them with thin iron sheets. This can prevent the flow-control refractory materials from breaking during use, and because the metal hoop is wrapped very tightly, it limits the expansion of cracks in the flow-control refractory materials, especially preventing the cracks from opening and expanding. In order to improve the flexibility of the flow-control refractory materials during the opening and drawing process and prevent steel leakage from between the working surfaces of the flow-control refractory materials, the working surfaces of the flow-control refractory materials must be processed on a grinding machine, and the flatness must be less than 0.03mm. After the ground flow-control refractory materials pass the inspection, asbestos pads and tinplate or iron shells must be pasted on the back. Their main function is to reduce the heat transferred to the hydraulic mechanism through the flow-control refractory materials and prevent the mechanism from deforming at high temperatures and affecting its service life.
[0104] The above are only some embodiments of the present invention. It should be pointed out that for ordinary technicians in this field, other modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. Zirconium-free flow control refractory, characterized in that: The invention comprises the following components in percentage by weight: 6% to 10% of recycled corundum kiln furniture, 22% to 24% of fused magnesium aluminum spinel, 7% to 11% of 95 ceramic parts, 4% to 6% of silicon carbide sagger for lithium battery used for renewable energy, 4% to 8% of recycled waste bricks from steel mills, 4% to 9% of slaked alumina, 13% to 19% of plate-shaped corundum, 5% to 8% of active α-Al2O3 micropowder, 2% to 4% of industrial aluminum sheet, 2% to 4% of silicon carbide powder, 2% to 4% of graphite electrode powder, 3% to 5% of Yixing white mud, and 4% to 6% of magnesium silicon chelating agent. The sum of the weights of all the components in the above formula is 100%, and 4% to 5% of thermosetting liquid binder is added.
2. The zirconium-free flow control refractory according to claim 1, characterized in that: The particle grading of each component is as follows: the particle diameter of recycled corundum kiln furniture is 5-3mm, the particle diameter of fused magnesium aluminum spinel is 3-2, 2-1, 1-0mm, the particle diameter of 95 ceramic parts is 3-1mm, the particle diameter of silicon carbide sagger for lithium batteries for renewable energy is 3-1mm, the particle diameter of waste bricks recycled from steel mills is 1-0mm, the particle diameter of slaked alumina is 1-0mm, the particle diameter of plate-like corundum is 325 mesh, the active α-Al2O3 powder is 5um, the industrial aluminum sheet is 250 mesh, the silicon carbide powder is 240 mesh, the graphite electrode powder is 180 mesh, the Yixing white mud is 200 mesh, and the magnesium silicon chelating agent is 200 mesh; the thermosetting binder is liquid.
3. The zirconium-free flow control refractory according to claim 1, characterized in that: The fused magnesia-alumina spinel particle size distribution is as follows: 3~2㎜9%~12% 2~1㎜5%~8% 1~0㎜6%~10%。 4. The zirconium-free flow control refractory according to claim 1, characterized in that: The total weight percentage of the particle grading of the fused magnesia-alumina spinel is 21% to 30%.
5. The zirconium-free flow control refractory according to claim 1, characterized in that: The regenerated corundum kiln furniture: Al2O3 content ≥ 85%, SiO2 content ≤ 10%; The fused magnesium-aluminum spinel has an Al2O3 content of 71-75%, a MgO content of 22-27%, a SiO2 content of <0.4%, a Fe2O3 content of ≤0.4%, and a CaO content of ≤0.6%; The 95 ceramic parts: Al2O3 content ≥ 95%, Fe2O3 content ≤ 0.8%; The silicon carbide sagger for lithium battery used for renewable energy: SiC content ≥ 80%, SiO2 content ≤ 15%; The steel mill recycled waste bricks: Al2O3 content ≥ 80%, Fe2O3 content < 1%, SiO2 content ≤ 15%; The calcined alumina has an Al2O3 content of ≥85% and a Fe2O3 content of ≤0.4%; The plate-shaped corundum has an Al2O3 content of ≥99.5% and a Fe2O3 content of ≤0.4%; The active α-Al2O3 micro powder has Al2O3 content ≥ 99% and Fe2O3 content ≤ 0.3%; The industrial aluminum sheet: active aluminum Al≥96%; The silicon carbide powder: SiC content ≥ 98%; The graphite electrode powder: C content ≥ 97%; The Yixing white mud: Al2O3 content ≥ 33%, Fe2O3 content ≤ 1.5%; The magnesium-silicon chelating agent has a MgO content of 52-60% and a SiO2 content of 40-48%; The thermosetting binder has a residual carbon content of 43±5%, a solid content of 70-83%, and a viscosity of 16000-18000 MPa.
6. A method for manufacturing a zirconium-free flow control refractory according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: Ingredients, weighed in proportion: recycled corundum kiln furniture, fused magnesium aluminum spinel, 95 ceramic parts, lithium battery silicon carbide sagger for renewable energy, recycled waste bricks from steel mills, slaked alumina, plate-shaped corundum, active α-Al2O3 powder, industrial aluminum sheet, silicon carbide powder, graphite electrode powder, Yixing white mud and magnesium silicon chelating agent; S2: mixing, mixing the raw materials in S1 with the liquid binder; S3: molding, using a mold to mold the uniformly mixed raw materials; S4: Natural drying: place the formed refractory body in a natural environment to dry for 12-24 hours; S5: Heating and drying, placing the formed refractory body into a drying kiln and slowly heating and drying for 32 to 51 hours; S6: Firing: Push the dried green body into a medium-high temperature tunnel kiln and evenly heat it to 580℃±30℃, keep it warm for 15 to 20 hours, and finally cool it down to room temperature at a uniform speed before taking it out of the kiln; S7: Inspection and warehousing: inspect the refractory materials and pack and store qualified products.
7. A method for manufacturing a zirconium-free flow control refractory material according to claim 6, characterized in that: The temperature-raising and drying process is as follows: the temperature of the drying kiln is uniformly raised to 80° C. within 1 hour, and kept at 80° C. for 15 hours; then, the temperature is uniformly raised from 80° C. to 180° C. within 20 hours, and kept at 180° C. for 15 hours.
8. The method for manufacturing a zirconium-free flow-control refractory according to claim 6, characterized in that: During the firing process, the temperature is uniformly raised to 580° C.±30° C. within 15 to 20 hours, and finally uniformly lowered to room temperature.
Citation Information
Patent Citations
Furnace lining of intermediate frequency furnace and preparation method thereof
CN106278304A
Zircon mullite brick for cement kiln and preparation method thereof
CN108516849A
Composite lining brick for torpedo ladle produced by recycling various waste refractory materials
CN114873997A
Environment-friendly plastic refractory for CFB (circulating fluid bed) furnace and preparation process of environment-friendly plastic refractory