Silicon nitride-based ceramic chip with compact surface and preparation method thereof
By using the use of suppressing powder mixing during the sintering of silicon nitride ceramic sheets to control the volatility of the glass phase, the problem of holes on the surface of silicon nitride ceramic sheets is solved, the density and pressure resistance value are improved, and the product performance and life are improved.
Patent Information
- Application Number
- CN202411264613.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-10
AI Technical Summary
During the sintering process, holes form on the surface of the ceramic sheet due to volatilization of the glass phase, which affects the density and pressure resistance value and reduces the life and yield of the ceramic sheet.
Using a preparation method, by mixing boron nitride and α-phase silicon nitride powder, anhydrous ethanol and slab 85 are added for emulsification and dispersion, forming a sintered powder, and adding anhydrous ethanol and slab to the ball mill 85 The ball mill dispersion is carried out to prevent the mixing of powder, combine the solvent and the organic carrier to form a slurry, coat it on the surface of the silicon nitride green body, and sintered under a nitrogen atmosphere to control the volatility of the glass phase and avoid the formation of holes.
Effectively suppresses the volatility of the glass phase on the surface of the silicon nitride ceramic sheet, improves the density and pressure resistance of the ceramic sheet, and reaches 25kv, improves product performance and life, and reduces the surface roughness and copper plating. Peeling force.
Smart Images

Figure CN119039010A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic preparation, in particular to a silicon nitride-based ceramic sheet with a dense surface and a preparation method thereof. Background Art
[0002] Silicon nitride is a compound composed of silicon and nitrogen. It has the characteristics of high strength, high thermal conductivity, low density, and wear resistance. Therefore, it is widely used in the field of new energy. With the continuous development of new material technology, the application prospects of silicon nitride are becoming more and more broad. In the field of electronics, silicon nitride is used as a ceramic substrate material and packaging material to improve the reliability and performance of electronic equipment. In addition, silicon nitride materials can also be used to manufacture high-temperature semiconductor devices and optoelectronic devices.
[0003] As a strong covalent bond compound, silicon nitride has a very low diffusion coefficient. Therefore, pure silicon nitride cannot be sintered to a dense state. During sintering, a sintering aid must be added to form a liquid phase to help it densify. During the sintering process, the sintering aid is very easy to volatilize, resulting in the formation of more pores on the surface of the ceramic tile, thereby affecting the withstand voltage value of the ceramic tile, resulting in a decrease in the life and yield of the ceramic tile.
[0004] Therefore, it is an urgent problem to find a silicon nitride-based ceramic sheet with a dense surface and a preparation method thereof. Summary of the invention
[0005] The purpose of the present invention is to provide a silicon nitride-based ceramic with a dense surface and a preparation method thereof, and to provide a coating with an inhibitory effect, so as to uniformly control the volatilization of the glass phase on the surface of the ceramic to avoid the formation of holes, thereby improving the density and withstand voltage of the ceramic, so as to solve the problem that the glass phase of the ceramic is easy to volatilize during the existing conventional silicon nitride sintering process, resulting in the formation of holes on the surface of the ceramic.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a silicon nitride-based ceramic sheet with a dense surface comprises the following steps:
[0008] Step S1, preparation of intercalated mixed powder: mixing boron nitride and α-phase silicon nitride powder, adding anhydrous ethanol and Span 85 for emulsification and dispersion, and then drying at 80-100° C. to obtain intercalated mixed powder;
[0009] Step S2, preparation of mixed powder: adding the mixed powder to a ball mill, adding anhydrous ethanol and Span 85, ball milling dispersion, and then filter pressing and drying, placing in a muffle furnace, heating to 800-850° C. and calcining for 2-8 hours, calcining and grinding to obtain mixed powder;
[0010] Step S3, slurry preparation: weigh the intercalated mixed powder, the inhibited mixed powder, the solvent and the organic carrier, mix and stir, and grind them uniformly to obtain a slurry;
[0011] Step S4, powder coating and sintering: coating the prepared slurry on the surface of the silicon nitride green body, debinding and sintering in a nitrogen atmosphere, keeping the temperature for 2-8 hours to obtain a ceramic sheet.
[0012] The mass ratio of boron nitride to α-phase silicon nitride is (80-100):(1-20), the particle size D50 of the boron nitride powder is 2-10 μm, and the particle size D50 of the α-phase silicon nitride powder is 0.2-2 μm.
[0013] The mixed powder is at least one of magnesium fluoride, magnesium nitride, yttrium fluoride, yttrium nitride and silicon oxide;
[0014] The mixed powder particle size D50 is suppressed to 0.2-2μm.
[0015] In step S3, the mass ratio of the intercalated mixed powder to the suppressed mixed powder is (85-100):(2-16). The solvent is at least one of methyl isobutyl ether, diethylene glycol monobutyl ether, pinene alcohol, and N-methylpyrrole.
[0016] In step S3, the organic carrier includes methyl isobutyl ether, ethyl cellulose, butyl benzyl phthalate and Span 85; the mass ratio of methyl isobutyl ether, ethyl cellulose, butyl benzyl phthalate and Span 85 is 9:0.75:0.15:0.1.
[0017] In step S3, the sum of the sintered mixed powder and the suppressed mixed powder accounts for (30-50) wt% of the slurry, the solvent accounts for (25-35) wt% of the slurry, and the organic carrier accounts for (25-35) wt% of the slurry.
[0018] In step S3, grinding is performed using a three-roller grinder, with the roller spacing set to 80 μm and then adjusted to 5 μm, the roller speed being 100-300 r / min, and grinding being performed 3-6 times.
[0019] The slurry is coated on the surface of the silicon nitride green body by using one of the processes of spraying, coating, printing and casting, and the coating thickness is 5-35 μm.
[0020] In step S4, the debinding temperature is set to 500-700°C and kept warm for 2-8h; the sintering temperature is set to 1750-1900°C and the nitrogen pressure is 0.5MPa-2MPa.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The silicon nitride-based ceramic with a dense surface and the preparation method thereof described in the present invention can form a uniform glass phase vapor pressure on the ceramic surface by adding the anti-mixing powder, which can effectively inhibit the volatilization of the glass phase of the ceramic when sintering, and avoid the formation of pores on the ceramic surface due to the volatilization of the glass phase, thereby improving the density and withstand voltage value of the ceramic, and the withstand voltage value can reach 25kv, thereby improving product performance and life;
[0023] The present invention discloses a silicon nitride-based ceramic sheet with a dense surface and a preparation method thereof. The added anti-mixing powder can inhibit the volatilization of silicon nitride at high sintering temperatures and can effectively inhibit the growth of grains on the surface of silicon nitride, thereby reducing the surface roughness of the ceramic sheet and improving the peeling force after copper plating, so that the 0.4 mm copper coating peeling force reaches 13.5 N / mm. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a microscope photograph of the silicon nitride ink imprint of Example 1;
[0025] Figure 2 This is a microscope photograph of the silicon nitride ink imprint of Example 2;
[0026] Figure 3 This is a microscope photograph of the silicon nitride ink imprint of Example 3;
[0027] Figure 4 This is a microscope photograph of the silicon nitride ink imprint of Example 4;
[0028] Figure 5 A microscopic photograph of a silicon nitride ink imprint of a comparative example;
[0029] Figure 6 This is a metallographic microscope photo of silicon nitride of the comparative example (magnified 500 times);
[0030] Figure 7 This is a metallographic microscope photo of silicon nitride of Example 3 (magnified 500 times);
[0031] Figure 8 This is an electron microscope photo of silicon nitride of a comparative example (magnified 2000 times);
[0032] Fig. 9 This is an electron microscope photograph of silicon nitride of Example 3 (magnified 2000 times). DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Reference Figure 1-9 , the present invention provides the following technical solutions:
[0035] In the experiment, the particle size D50 of boron nitride powder is 2-10μm, and the morphology is a flaky structure, and the particle size D50 of α-phase silicon nitride powder is 0.2-2μm.
[0036] The preparation steps of silicon nitride green body are as follows:
[0037] 1. Powder ratio: Silicon nitride powder with a particle size of D50 = 0.8um, magnesium oxide and yttrium oxide are mixed in a mass ratio of 92:4:4 to form a mixed powder;
[0038] 2. Slurry preparation: Take 100g of the mixed powder prepared in step 1, 62.5g of anhydrous ethanol, 62.5g of toluene, 15g of polyvinyl butyral, 5g of dibutyl phthalate, and 2.5g of lecithin and add them to a drum ball mill for ball milling at a speed of 35r / min for 18h, and then degas the material;
[0039] 3. Tape casting: After degassing, the slurry is cast using a tape casting machine. The casting temperature range is 30℃, 40℃, 50℃, 60℃, and 50℃. The thickness of the green body is 0.45mm.
[0040] 4. Green billet die cutting: Use a die cutting machine to cut the green billet roll into 260×190mm green billets for later use.
[0041] Among them, the MW of polyvinyl butyral is 120,000-150,000.
[0042] Embodiment 1: This embodiment provides a method for preparing a silicon nitride-based ceramic sheet with a dense surface, and the specific steps are as follows:
[0043] A method for preparing a silicon nitride-based ceramic sheet with a dense surface comprises the following steps:
[0044] Step S1, preparation of intercalated mixed powder: 90g of boron nitride and 10g of α-phase silicon nitride powder are mixed and placed in an emulsifier, and then 300g of anhydrous ethanol and 0.5g of Span 85 are added for emulsification and dispersion, and then dried at 80°C to obtain intercalated mixed powder;
[0045] Step S2, preparation of mixed powder: 1 g of magnesium nitride, 0.5 g of yttrium fluoride and 0.5 g of silicon oxide are put into a ball mill, and then 6 g of anhydrous ethanol and 0.05 g of Span 85 are added for ball milling dispersion, followed by filter pressing and drying, and then placed in a muffle furnace, heated to 850° C. and calcined for 4 h. After calcination, the powder is finely ground using a jet mill to obtain a mixed powder having a particle size of D50=500 nm;
[0046] Step S3, slurry preparation: weigh raw materials according to 100g of intercalated mixed powder, 2g of inhibited mixed powder, 80.5g of solvent and 86g of organic carrier, mix and stir evenly, grind with a three-roll grinder, set the roller pitch to 80μm, 40μm, 20μm, 10μm, 5μm, roll in this roller pitch sequence, and the roller speed is 200r / min to prepare slurry;
[0047] Step S4, powder coating and sintering: the slurry prepared in step S3 is coated on the surface of the silicon nitride green body by a printing machine, with a wet film thickness of 10 μm, and the binder is debonded at 550°C. After keeping the temperature for 2 hours, the ceramic tile is sintered under a nitrogen pressure of 1.2 MPa at a sintering temperature of 1860°C and kept for 2 hours.
[0048] The solvent is methyl isobutyl ether; the ratio of the organic carrier is: methyl isobutyl ether: ethyl cellulose: butyl benzyl phthalate: Span 85 = 9:0.75:0.15:0.1.
[0049] Embodiment 2: This embodiment provides a method for preparing a silicon nitride-based ceramic sheet with a dense surface, and the specific steps are as follows:
[0050] A method for preparing a silicon nitride-based ceramic sheet with a dense surface comprises the following steps:
[0051] Step S1, preparation of intercalated mixed powder: 90g of boron nitride and 10g of α-phase silicon nitride powder are mixed and placed in an emulsifier, and then 300g of anhydrous ethanol and 0.5g of Span 85 are added for emulsification and dispersion, and then dried at 80°C to obtain intercalated mixed powder;
[0052] Step S2, preparation of mixed powder: 2 g of magnesium nitride, 1 g of yttrium fluoride and 1 g of silicon oxide are put into a ball mill, and then 12 g of anhydrous ethanol and 0.05 g of Span 85 are added for ball milling dispersion, followed by filter pressing and drying, and then placed in a muffle furnace, heated to 850° C. and calcined for 4 h. After calcination, the powder is ground with a jet mill to obtain a mixed powder with a particle size of D50=500 nm;
[0053] Step S3, slurry preparation: weigh raw materials according to 100g of intercalated mixed powder, 4g of inhibited mixed powder, 80.5g of solvent and 86g of organic carrier, mix and stir evenly, grind with a three-roll grinder, set the roller pitch to 80μm, 40μm, 20μm, 10μm, 5μm, roll in this roller pitch sequence, and the roller speed is 200r / min to prepare slurry;
[0054] Step S4, powder coating and sintering: the slurry prepared in step S3 is coated on the surface of the silicon nitride green body by a printing machine, with a wet film thickness of 10 μm, and the binder is debonded at 550°C. After keeping the temperature for 2 hours, the ceramic tile is sintered under a nitrogen pressure of 1.2 MPa at a sintering temperature of 1860°C and kept for 2 hours.
[0055] The solvent is methyl isobutyl ether; the ratio of the organic carrier is: methyl isobutyl ether: ethyl cellulose: butyl benzyl phthalate: Span 85 = 9:0.75:0.15:0.1.
[0056] Embodiment 3: This embodiment provides a method for preparing a silicon nitride-based ceramic sheet with a dense surface, and the specific steps are as follows:
[0057] A method for preparing a silicon nitride-based ceramic sheet with a dense surface comprises the following steps:
[0058] Step S1, preparation of intercalated mixed powder: 95g of boron nitride and 5g of α-phase silicon nitride powder are mixed and placed in an emulsifier, and then 300g of anhydrous ethanol and 0.5g of Span 85 are added for emulsification and dispersion, and then dried at 80°C to obtain intercalated mixed powder;
[0059] Step S2, preparation of mixed powder: 4 g of magnesium nitride, 2 g of yttrium fluoride and 2 g of silicon oxide are put into a ball mill, and then 24 g of anhydrous ethanol and 0.05 g of Span 85 are added for ball milling dispersion, followed by filter pressing and drying, and then placed in a muffle furnace, heated to 850° C. and calcined for 4 h. After calcination, the powder is ground with a jet mill to obtain a mixed powder with a particle size of D50=500 nm;
[0060] Step S3, slurry preparation: weigh raw materials according to 100g of intercalated mixed powder, 8g of inhibited mixed powder, 80.5g of solvent and 86g of organic carrier, mix and stir evenly, grind with a three-roll grinder, set the roller pitch to 80μm, 40μm, 20μm, 10μm, 5μm, roll in this roller pitch sequence, and the roller speed is 200r / min to prepare slurry;
[0061] Step S4, powder coating and sintering: the slurry prepared in step S3 is coated on the surface of the silicon nitride green body by a printing machine, with a wet film thickness of 10 μm, and the binder is debonded at 550°C. After keeping the temperature for 2 hours, the ceramic tile is sintered under a nitrogen pressure of 1.2 MPa at a sintering temperature of 1860°C and kept for 2 hours.
[0062] The solvent is methyl isobutyl ether; the ratio of the organic carrier is: methyl isobutyl ether: ethyl cellulose: butyl benzyl phthalate: Span 85 = 9:0.75:0.15:0.1.
[0063] Embodiment 4: This embodiment provides a method for preparing a silicon nitride-based ceramic sheet with a dense surface, and the specific steps are as follows:
[0064] A method for preparing a silicon nitride-based ceramic sheet with a dense surface comprises the following steps:
[0065] Step S1, preparation of intercalated mixed powder: 95g of boron nitride and 5g of α-phase silicon nitride powder are mixed and placed in an emulsifier, and then 300g of anhydrous ethanol and 0.5g of Span 85 are added for emulsification and dispersion, and then dried at 80°C to obtain intercalated mixed powder;
[0066] Step S2, preparation of mixed powder: 8 g of magnesium nitride, 4 g of yttrium fluoride and 4 g of silicon oxide are put into a ball mill, and then 48 g of anhydrous ethanol and 0.05 g of Span 85 are added for ball milling dispersion, followed by filter pressing and drying, and then placed in a muffle furnace, heated to 850° C. and calcined for 4 h. After calcination, the powder is ground with a jet mill to obtain a mixed powder with a particle size of D50=500 nm;
[0067] Step S3, slurry preparation: weigh raw materials according to 100g of intercalated mixed powder, 16g of inhibited mixed powder, 80.5g of solvent and 86g of organic carrier, mix and stir evenly, grind with a three-roll grinder, set the roller pitch to 80μm, 40μm, 20μm, 10μm, 5μm, roll in this roller pitch sequence, and the roller speed is 200r / min to prepare slurry;
[0068] Step S4, powder coating and sintering: the slurry prepared in step S3 is coated on the surface of the silicon nitride green body by a printing machine, with a wet film thickness of 10 μm, and the binder is debonded at 550°C. After keeping the temperature for 2 hours, the ceramic tile is sintered under a nitrogen pressure of 1.2 MPa at a sintering temperature of 1860°C and kept for 2 hours.
[0069] The solvent is methyl isobutyl ether; the ratio of the organic carrier is: methyl isobutyl ether: ethyl cellulose: butyl benzyl phthalate: Span 85 = 9:0.75:0.15:0.1.
[0070] Comparative Example: This embodiment provides a method for preparing a silicon nitride-based ceramic sheet with a dense surface, and the specific steps are as follows:
[0071] Step S1, preparation of intercalated mixed powder: 100 g of boron nitride is placed in an emulsifier, and then 300 g of anhydrous ethanol and 0.5 g of Span 85 are added for emulsification and dispersion, and then dried at 80° C. to obtain intercalated mixed powder;
[0072] Step S2, slurry preparation: weigh raw materials according to 100g of intercalated mixed powder, 80.5g of solvent and 86g of organic carrier, mix and stir evenly, grind with a three-roll grinder, set the roller pitch to 80μm, 40μm, 20μm, 10μm, 5μm, roll in this roller pitch sequence, and the roller speed is 200r / min to prepare slurry;
[0073] Step S3, powder coating and sintering: the slurry prepared in step S2 is coated on the surface of the silicon nitride green body by a printing machine, with a wet film thickness of 10 μm, and the binder is debonded at 550°C. After keeping the temperature for 2 hours, the ceramic tile is sintered under a nitrogen pressure of 1.2 MPa at a sintering temperature of 1860°C and kept for 2 hours.
[0074] The solvent is methyl isobutyl ether; the ratio of the organic carrier is: methyl isobutyl ether: ethyl cellulose: butyl benzyl phthalate: Span 85 = 9:0.75:0.15:0.1.
[0075] Table 1 Examples 1 to 4 and Comparative Examples Burnt Mixed Powder ,inhibition Mixed powder Ratio of raw materials
[0076]
[0077] Test method:
[0078] 1. Pore characterization
[0079] The ceramic pieces prepared in Examples 1-4 and Comparative Example were soaked in black ink for 5 min, then ultrasonically cleaned with pure water and anhydrous ethanol, and dried. The surface voids of the ceramic pieces were observed under a microscope at a magnification of 60 times. The test results are shown in Figure 1-5 .
[0080] 2. Density test
[0081] The density was tested by the displacement method using an analytical balance.
[0082] 3. Roughness test
[0083] The test was carried out using a roughness tester TR200.
[0084] 4. Withstand voltage test
[0085] Place the ceramic tile in a high-voltage test environment, and test the DC voltage from 15KV to 25KV, with an interval of 1kV each time and a test time of 10s each time. If there is a voltage breakdown, the test is suspended and the value at this time is the withstand voltage value.
[0086] 5. Peel force test
[0087] Take the ceramic sheets prepared in Examples 1-4 and the comparative example, and print a 15um thick layer of Ag-Cu-Ti active metal slurry on the surface thereof, wherein the mass ratio of Ag, Cu and Ti in the active metal slurry is 65:30:5; then use hot pressing technology to laminate a 0.4mm copper foil on the solder, and finally sinter, photolithograph and etch a test pattern, and use a peel strength tester to perform a peel force test.
[0088] Table 2 Experimental data of comparative test of Examples 1-4
[0089]
[0090] Through the above data and comparison Figure 1-5 The surface pores of the ceramic tile made in the comparative example are relatively large, resulting in a lower density and a withstand voltage value of only 17kv. The surface roughness is relatively large, and the bending strength of the ceramic tile is also relatively low, resulting in a low copper cladding peeling force; the ceramic tiles made in Examples 3 and 4 have no pores on the surface, a higher density, and a relatively high withstand voltage value. Inhibiting powder mixing can well inhibit the volatilization of silicon nitride on the surface of the ceramic tile at high temperature, and can effectively inhibit the growth of silicon nitride surface grains, thereby reducing the surface roughness of the ceramic tile and improving the copper cladding peeling force, especially the withstand voltage value of Example 3 reaches 25kv, and the peeling force can reach 13.5N / mm; it can be seen that adding inhibitory powder mixing can significantly reduce pores, improve density and withstand voltage value.
[0091] from Figure 6 , Figure 7 From the metallographic microscope photo magnified 500 times, it can be seen that the glass phase on the surface of the ceramic piece made in the comparative example evaporates unevenly, aggregates, and forms a larger glass state, resulting in a part of the surface without glass phase filling, such as Figure 6 As shown in the red circled area, pores are formed; no glass phase aggregation occurs on the surface of the ceramic tile prepared in Example 3, and the glass phase is uniformly suppressed inside the ceramic tile.
[0092] from Figure 8 , Fig. 9 It can be seen from the electron microscope photograph magnified 2000 times that the glass phase of the ceramic piece made in the comparative example is unevenly distributed. The marked red circled area has more pores due to the volatilization of the glass phase, and the grains grow abnormally, resulting in greater roughness. In Example 3, the volatilization of the glass phase of the ceramic piece is suppressed by suppressing the addition of mixed powder, so that the glass phase is evenly distributed. Due to the glass phase filling, no obvious pores are observed, the grains grow evenly, and no abnormal growth is observed. Therefore, the density of the ceramic piece in Example 3 is greater and the surface roughness is smaller.
[0093] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing a surface dense silicon nitride-based ceramic sheet, characterized in that: The specific steps are: Step S1, preparation of intercalated mixed powder: mixing boron nitride and α-phase silicon nitride powder, adding anhydrous ethanol and Span 85 for emulsification and dispersion, and then drying at 80-100° C. to obtain intercalated mixed powder; Step S2, preparing mixed powder: adding the mixed powder to a ball mill, adding anhydrous ethanol and Span 85, performing ball milling dispersion, then filtering and drying, placing in a muffle furnace, heating to 800-850° C. and calcining for 2-8 hours, grinding after calcination to obtain mixed powder; the mixed powder is at least one of magnesium fluoride, magnesium nitride, yttrium fluoride, yttrium nitride, and silicon oxide; Step S3, slurry preparation: weigh the intercalated mixed powder, the inhibited mixed powder, the solvent and the organic carrier, stir them evenly, grind them, and obtain slurry; Step S4, powder coating and sintering: coating the prepared slurry on the surface of the silicon nitride green body, debinding and sintering in a nitrogen atmosphere, keeping the temperature for 2-8 hours to obtain a ceramic sheet.
2. The method for preparing a surface dense silicon nitride-based ceramic sheet according to claim 1, characterized in that: The mass ratio of the boron nitride to the α-phase silicon nitride is (80-100):(1-20), the particle size D50 of the boron nitride powder is 2-10 μm, and the particle size D50 of the α-phase silicon nitride powder is 0.2-2 μm.
3. The method for preparing a surface dense silicon nitride-based ceramic sheet according to claim 1, characterized in that: The mixed powder particle size D50 is suppressed to 0.2-2μm.
4. The method for preparing a surface dense silicon nitride-based ceramic sheet according to claim 1, characterized in that: In step S3, the mass ratio of the inter-fired mixed powder and the suppressed mixed powder is (85-100):(2-16).
5. The method for preparing a surface dense silicon nitride-based ceramic sheet according to claim 1, characterized in that: In step S3, the solvent is at least one of methyl isobutyl ether, diethylene glycol monobutyl ether, terpineol, and N-methylpyrrole.
6. The method for preparing a silicon nitride-based ceramic sheet with a dense surface according to claim 1, characterized in that: In step S3, the organic carrier includes methyl isobutyl ether, ethyl cellulose, butyl benzyl phthalate and Span 85; the mass ratio of methyl isobutyl ether, ethyl cellulose, butyl benzyl phthalate and Span 85 is 9:0.75:0.15:0.
1.
7. The method for preparing a surface dense silicon nitride-based ceramic sheet according to claim 1, characterized in that: In step S3, the sum of the sintered mixed powder and the suppressed mixed powder accounts for (30-50) wt% of the slurry, the solvent accounts for (25-35) wt% of the slurry, and the organic carrier accounts for (25-35) wt% of the slurry.
8. The method for preparing a surface dense silicon nitride-based ceramic sheet according to claim 1, characterized in that: In step S3, grinding is performed using a three-roller grinder, with the roller spacing set to 80 μm and then adjusted to 5 μm, the roller speed being 100-300 r / min, and grinding being performed 3-6 times.
9. The method for preparing a surface dense silicon nitride-based ceramic sheet according to claim 1, characterized in that: The slurry is coated on the surface of the silicon nitride green body by using one of the processes of spraying, coating, printing and casting, and the coating thickness is 5-35 μm.
10. The method for preparing a silicon nitride-based ceramic sheet with a dense surface according to claim 1, characterized in that: In step S4, the debinding temperature is set to 500-700°C and kept warm for 2-8h; the sintering temperature is set to 1750-1900°C and the nitrogen pressure is 0.5-2MPa.
Citation Information
Patent Citations
Hexagonal boron nitride-glass composite material and preparation method thereof
CN108117395A
Y-Al-Si-O multi-element glass phase reinforced hexagonal boron nitride-based composite ceramic and preparation method thereof
CN111410539A
Structure and preparation method of porous silicon nitride ceramic surface coating
CN113816771A
Preparation method of boron nitride printing paste
CN116063084A
Boron nitride coated hard material
JP1992280972A
Cited By
Reactive sintering silicon nitride ceramic chip processing method
CN121135442A