Curing agent composition for epoxy resin and epoxy resin composition

The combination of oligomers formed by the polycondensation reaction of isomeric aromatic diamines and acid anhydrides and liquid aromatic diamines is solved, and the poor processability and solvent problems of traditional high-temperature resistant epoxy adhesives are achieved at high temperatures, achieving 250% High performance usage and high adhesion effect above ℃.

CN119039568APending Publication Date: 2024-11-29SHANGHAI HUAYI RESINS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411159525.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional high-temperature resistant epoxy adhesives have poor processability and solvent environmental problems when used at high temperatures, and generally can only withstand 200℃. Rarely, they can withstand 250℃, making it difficult to maintain high performance at higher temperatures.

Method used

By selecting different isomer aromatic diamines and polycondensation reactions with acid anhydrides, an amine-terminated oligomer is obtained, forming a new epoxy resin composition, combining liquid aromatic diamines and accelerators, forming a traditional high-temperature toughening agent without the need for traditional high-temperature resistant toughening agents epoxy resin curing agent composition for the preparation of epoxy resin composition.

Benefits of technology

The epoxy resin composition used at higher temperatures is realized, maintaining high performance and adhesion, avoiding solvent problems in traditional methods, and improving the flexibility and adhesion of the epoxy resin system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005006040230000111
    Figure BDA0005006040230000111
  • Figure BDA0005006040230000112
    Figure BDA0005006040230000112
  • Figure BDA0005006040230000131
    Figure BDA0005006040230000131
Patent Text Reader

Abstract

A curing agent composition for epoxy resin and an epoxy resin composition. The invention provides a curing agent composition for epoxy resin. The curing agent composition comprises: (1) an oligomer formed by anhydride and a first aromatic diamine; (2) an oligomer formed from an anhydride with a second aromatic diamine, wherein the second aromatic diamine is an isomer with the first aromatic diamine; (3) liquid aromatic diamine; and (4) an optional accelerator. The epoxy resin composition disclosed by the invention has excellent high temperature resistance, and can resist the high temperature of 250 DEG C for a long time especially when being applied to the field of adhesives. When the composition is used, a traditional high-temperature-resistant toughening agent does not need to be added, meanwhile, the composition can be used at a high temperature, and meanwhile high performance is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of polymers, and more specifically to a curing agent composition for epoxy resins, and an epoxy resin composition. Background Art

[0002] High-performance, high-temperature resistant epoxy adhesives are now increasingly used in high-end applications such as aerospace and pressed ceramics.

[0003] Traditional high temperature resistant epoxy adhesives use multifunctional epoxy resins, phenolic epoxy resins, etc. as high temperature resistant main resins, thermoplastics, CTBN, polyether, polyurethane, etc. as modified toughening agents, alicyclic amines, aromatic amines as curing agents, but the high temperature resistance is generally only 200°C, and rarely 250°C.

[0004] High temperature resistant epoxy system, especially the one that can withstand temperatures above 250℃, will inevitably choose high temperature resistant epoxy resin system. However, this type of resin, toughening agent, and curing agent are basically solid or semi-solid, and are generally dissolved by solvent or at high temperature (>170℃), which has poor processability or environmental problems with solvents.

[0005] Therefore, there is an urgent need in the art for a new epoxy resin composition that does not require a traditional high temperature resistant toughening agent and can be used at higher temperatures while achieving higher performance. Summary of the invention

[0006] After extensive research, the inventors of the present application discovered that the above-mentioned technical problems can be solved by selecting different isomeric aromatic diamines and acid anhydrides for polycondensation to obtain amino-terminated oligomers, that is, providing a new epoxy resin composition that does not require traditional high-temperature resistant toughening agents and can be used at higher temperatures while achieving higher performance.

[0007] On the one hand, the present application provides a curing agent composition for epoxy resin, the curing agent composition comprising:

[0008] (1) an oligomer formed by an acid anhydride and a first aromatic diamine;

[0009] (2) an oligomer formed by an acid anhydride and a second aromatic diamine, wherein the second aromatic diamine and the first aromatic diamine are isomers;

[0010] (3) liquid aromatic diamines; and

[0011] (4) Optional accelerator.

[0012] On the other hand, the present application provides an epoxy resin composition, which comprises:

[0013] (1) the epoxy resin curing agent composition described in the present application; and

[0014] (2) Epoxy resin

[0015] Another aspect of the present application provides an epoxy resin product, which is prepared using the epoxy resin composition described in the present application. DETAILED DESCRIPTION

[0016] "Scope" disclosed herein is defined in the form of lower limit and upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a particular range. The scope defined in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a particular parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0017] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.

[0018] In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.

[0019] In the present application, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0020] In this application, unless otherwise specified, the terms "include" and "comprising" mentioned herein may be open-ended or closed-ended. For example, the terms "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0021] In the description of this article, it should be noted that, unless otherwise specified, "above" and "below" are inclusive of the number itself, and "several" in "one or several" means two or more.

[0022] In the description herein, unless otherwise specified, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0023] Herein, unless otherwise specified, percentage (%) or part refers to percentage by weight or part by weight relative to the composition.

[0024] Herein, if there is no contrary description, the sum of the contents of the various components in the composition is 100%.

[0025] Herein, if there is no contrary description, the sum of the parts of each component in the composition may be 100 parts by weight.

[0026] In this context, unless otherwise specified, "a combination thereof" means a multi-component mixture of the elements described, for example a mixture of two, three, four and up to the maximum possible multi-component mixture.

[0027] If not specifically stated, the terms "a" or "an" used in the present specification means "at least one".

[0028] Herein, unless otherwise stated, all reactions are carried out at normal temperature and pressure.

[0029] In the present application, unless otherwise specified, all terms "parts" refer to parts by weight.

[0030] On the one hand, the present application provides a curing agent composition for epoxy resin, the curing agent composition comprising:

[0031] (1) an oligomer formed by an acid anhydride and a first aromatic diamine;

[0032] (2) an oligomer formed by an acid anhydride and a second aromatic diamine, wherein the second aromatic diamine and the first aromatic diamine are isomers;

[0033] (3) liquid aromatic diamines; and

[0034] (4) Optional accelerator.

[0035] In the above components (1) and (2) of the present application, the acid anhydride may be the same or different, preferably the same. The acid anhydride may be a common acid anhydride used as a curing agent in an epoxy resin composition, including but not limited to phthalic anhydride, phthalic anhydride, maleic anhydride, trimellitic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnorbornene dicarboxylic anhydride, methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, methyl humic anhydride, pyromellitic dianhydride, benzophenone tetracarboxylic anhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, cyclohexanetricarboxylic anhydride, etc., preferably an acid anhydride having 1 or 2 aliphatic rings or aromatic rings in the molecule, and 1 or 2 acid anhydride groups, and having 4-25 carbon atoms, preferably 8-20.

[0036] In one example of the present application, the first or second aromatic diamine can be represented by the following structure: H2N-R 10 -NH2, where R 10 is an aryl group containing 6 to 16 carbon atoms in the ring and, optionally, up to one heteroatom containing -N-, -O-, or -S-. Also included herein are those R 10 Group, where R 10 is a diphenylene group or a diphenylmethane group. Representatives of such diamines are 2,6-diaminopyridine, 3,5-diaminopyridine, m-phenylenediamine, p-phenylenediamine, p,p'-methylenedianiline, 2,6-diaminotoluene, and 2,4-diaminotoluene.

[0037] Other examples of the first or second aromatic diamines (merely illustrative) include phenylenediamines, such as 1,4-diaminobenzene, 1,3-diaminobenzene, and 1,2-diaminobenzene; diphenyl(thio)ether diamines, such as 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, and 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide; benzophenone diamines, such as 3,3'-diaminobenzophenone and 4,4'-diaminobenzophenone; diphenylphosphine diamines, such as 3,3 diphenyl alkylene diamines, such as 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylpropane, and 4,4'-diaminodiphenylpropane; diphenyl sulfide diamines, such as 3,3'-diaminodiphenyl sulfide and 4,4'-diaminodiphenyl sulfide; diphenyl sulfone diamines, such as 3,3'-diaminodiphenyl sulfone and 4,4'-diaminodiphenyl sulfone; and benzidines, such as benzidine and 3,3'-dimethylbenzidine.

[0038] In the present application, the first aromatic diamine and the second aromatic diamine are different and are isomers. For example, among the aromatic diamines exemplified above, 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether and 3,3'-diaminodiphenyl ether; 1,4-diaminobenzene, 1,3-diaminobenzene and 1,2-diaminobenzene; 3,3'-diaminodiphenyl phosphine and 4,4'-diaminodiphenyl phosphine, etc. are all isomers. In the present application, the first aromatic diamine can be any one of the above aromatic diamines, and the second aromatic diamine is an isomer of the first aromatic diamine. For example, if the first aromatic diamine is 4,4'-diaminodiphenyl ether, then the second aromatic diamine can be 3,4'-diaminodiphenyl ether or 3,3'-diaminodiphenyl ether, and so on. The inventors have found that the oligomers (oligomers formed by anhydride and aromatic diamine) of the present application contain different isomers, and therefore have good miscibility with liquid aromatic amines. Mixing oligomers of different isomers with liquid aromatic amines can obtain a rigid structure such as an aromatic ring to maintain a high Tg, and can also improve the flexibility of the resin system by introducing an oligomer curing agent, thereby improving the adhesion of the high temperature resistant epoxy resin composition.

[0039] In one example of the present application, the molar ratio of the aromatic diamine (the first aromatic diamine or the second aromatic diamine) to the acid anhydride may be, for example, (0.5-10):1, (1-8):1, (2-6):1, or 3:1.

[0040] The method for preparing the oligomer described in the present application (i.e., the oligomer formed by anhydride and the first or second aromatic diamine, in this article, sometimes oligomer 1 is used to represent the oligomer formed by anhydride and the first aromatic diamine, and oligomer 2 is used to represent the oligomer formed by anhydride and the second aromatic diamine) is a commonly used method in the art, including but not limited to mixing anhydride and aromatic diamine (heating or room temperature). In one example of the present application, the method for preparing the oligomer includes reacting anhydride and diamine in a solvent (e.g., an organic polar solvent, such as DMF, DMSO, DMAC or a combination thereof). The amount of all monomers in the solvent may be in the range of about 5 to about 40 weight percent, more preferably in the range of about 6 to about 35 weight percent, and most preferably in the range of about 8 to about 30 weight percent. The temperature of the reaction is usually not higher than about 100°C, preferably in the range of about 10°C to 80°C. The reaction time is usually in the range of about 0.2 to 60 hours.

[0041] While not being limited by theory, it is believed that the oligomer formed by the acid anhydride and the aromatic diamine (herein, the aromatic diamine is a collective term for the first aromatic diamine and the second aromatic diamine) has amine-terminated groups.

[0042] In one example of the present application, the molar ratio of oligomer 1 to oligomer 2 is (0.5-2):1, preferably (0.8-1.5):1, more preferably (0.9-1.2):1, and even better (0.95-1.05):1.

[0043] In the present application, the liquid aromatic diamine may be a liquid aromatic diamine used as an epoxy resin curing agent in the art. In one example of the present application, the liquid aromatic diamine is selected from at least one of the following: dimethylthiotoluenediamine (DMTDA), diethyltoluenediamine (DETDA), 4,4'-bis-sec-butylaminodiphenylmethane (MDBA), metaphenylenediamine (MXDA), paraphenylenediamine and o-phenylenediamine.

[0044] In one example of the present application, the amount of the liquid aromatic diamine is 100-1000 parts by weight, preferably 100-800 parts by weight, more preferably 150-600 parts by weight, and even more preferably 200-400 parts by weight, based on the total weight of oligomer 1 and oligomer 2 as 100 parts by weight.

[0045] In the present application, the curing agent composition may optionally include a curing accelerator (sometimes also referred to as an accelerator). In the context of the present application, the term "curing accelerator" or "accelerator" means a substance added to accelerate the reaction rate of epoxy resin and curing agent to reduce the curing reaction temperature and shorten the curing time, which is a component capable of accelerating the curing reaction of epoxy resin.

[0046] The curing accelerator is not particularly limited. In an exemplary embodiment, the curing accelerator can be selected from: imidazole and its derivatives, and amine adducts. For example, the curing accelerator can be imidazole, 1-methylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 2-methylimidazole and butyl glycidyl ether adduct, or 2-methylimidazole and 2-ethylhexyl glycidyl ether adduct. The curing accelerator can be, for example, available with the brand name Dyhard (e.g., DyhardUR500, DyhardUR300), or available with the brand name PN (e.g., PN-23) from Ajinomoto Co., Ltd., or available with the brand name MY (e.g., MY-24), but is not limited thereto.

[0047] The amount of the curing accelerator may depend on the desired properties of the final product. For example, the amount of the curing accelerator may be 1 to 30 parts by weight, preferably 2 to 25 parts by weight, preferably 3 to 20 parts by weight, preferably 5 to 18 parts by weight, preferably 8 to 16 parts by weight, based on the total weight of oligomer 1 and oligomer 2 being 100 parts by weight.

[0048] The curing agent composition described in the present application can be prepared using a common method. For example, the oligomer 1, oligomer 2, liquid aromatic diamine and optional accelerator can be mixed together by a physical method without using a solvent. The mixing can be carried out under heating (e.g., 30-100° C.).

[0049] In one example of the present application, the viscosity of the curing agent composition at 25° C. is 1000-10000 mPa.S, preferably 2000-8000 mPa.S, more preferably 3000-6000 mPa.S. The amine value of the curing agent composition is 100-1000 mgKOH / g, preferably 200-800 mgKOH / g, more preferably 300-600 mgKOH / g.

[0050] On the other hand, the present application provides an epoxy resin composition, which comprises:

[0051] (1) the epoxy resin curing agent composition described in the present application; and

[0052] (2) Epoxy resin.

[0053] According to one embodiment of the present application, the epoxy resin may be, for example, a liquid epoxy resin, a solid epoxy resin or a combination thereof.

[0054] In the context of the present application, "liquid epoxy resin" means an epoxy resin that is liquid at normal temperature.

[0055] According to one embodiment, the liquid epoxy resin can be selected from: bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, brominated bisphenol A epoxy resin, aliphatic glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, linear aliphatic epoxy resin, alicyclic epoxy resin, or a mixture thereof.

[0056] According to a preferred embodiment, the liquid epoxy resin is selected from bisphenol A epoxy resin, bisphenol F epoxy resin, aliphatic glycidyl ether epoxy resin and glycidyl ester epoxy resin or a mixture thereof.

[0057] According to a preferred embodiment, the epoxide equivalent of the liquid epoxy resin is 156 to 2500 g / eq, or 170 to 2200 g / eq, or 200 to 2000 g / eq, or 300 to 1800 g / eq, or 400 to 1700 g / eq, or 500 to 1600 g / eq, or 600 to 1500 g / eq, or 700 to 1200 g / eq, or 800 to 1100 g / eq, or 900 to 1000 g / eq.

[0058] According to a preferred embodiment, the number average molar mass of the liquid epoxy resin is 300 to 500 g / mol, preferably 350 to 500 g / mol, more preferably 400 to 500 g / mol. For example, the molecular weight of the liquid epoxy resin may be 310 g / mol, or 320 g / mol, or 330 g / mol, or 340 g / mol, or 350 g / mol, or 360 g / mol, or 370 g / mol, or 380 g / mol, or 390 g / mol, or 400 g / mol, or 410 g / mol, or 420 g / mol, or 430 g / mol, or 440 g / mol, or 450 g / mol, or 460 g / mol, or 470 g / mol, or 480 g / mol, or 490 g / mol, or 500 g / mol.

[0059] According to a preferred embodiment, the liquid epoxy resin has an average of 2 to 5 epoxy functional groups per molecule, preferably 2.5 to 5 epoxy functional groups, preferably 3 to 5 epoxy functional groups, preferably 3.5 to 5 epoxy functional groups. For example, the liquid epoxy resin has an average of 2, 2.1, or 2.2, or 2.3, or 2.4, or 2.5, or 2.6, or 2.7, or 2.8, or 2.9, or 3.0, or 3.1, or 3.2, or 3.3, or 3.4, or 3.5, or 3.6, or 3.7, or 3.8, or 3.9, or 4.0, or 4.1, or 4.2, or 4.3, or 4.4, or 4.5, or 4.6, or 4.7, or 4.8, or 4.9, or 5 epoxy functional groups per molecule.

[0060] The liquid epoxy resin may be commercially available. As non-limiting examples, the following names or brands of liquid epoxy resins may be mentioned: AG-80, AFG-90H, bisphenol A type liquid epoxy resin NPEL-127E, bisphenol A type liquid epoxy resin 6101, bisphenol A type liquid epoxy resin 128, bisphenol A type liquid epoxy resin E44, ARALDITE GY250, ARALDITE GY9708-3, ARALDITE MY790-1, ARALDITE CY179-1, ARALDITE CY184, ARALDITE GY6010, ARALDITE GY2600, EPALLOY 5000, EPALLOY 5001LC, NPEF-1, NPEL-127, NPEL-127H, NPEL-127L, NPEL-128, NPEL-12BB, NPEL-128R, NPEL-128s, NPE-1286, NPEL-131, NPEL-144; DER-331 (liquid; epoxy equivalent weight 182 to 192; viscosity at 25°C 11,000 to 14,000 centipoise) and DER-332 (liquid; epoxy equivalent weight 171 to 175; viscosity at 25°C 4,000 to 6,000 centipoise) from Olin; available from Hexion Speciality Chemicals EPON828 (liquid; epoxy equivalent weight 185 to 192; viscosity at 25°C 11,000 to 15,000 centipoise), EPON830 (liquid; epoxy equivalent weight 190 to 198; viscosity at 25°C 17,000 to 22,500 centipoise), and EPON1001F (liquid; epoxy equivalent weight: 525 to 550; viscosity at 25°C 7,000 to 9,600 centipoise) from Dainippon Ink and Chemicals, Inc. 830 from Olin (liquid; epoxy equivalent weight 165 to 180; viscosity at 25°C 3000 to 4000 centipoise); DER-354 from Olin (liquid; epoxy equivalent weight 167 to 174; viscosity at 25°C 3400 to 4200 centipoise); EPIKOTE 828 from Hexion Speciality Chemicals (Rosbach, Germany) (liquid; epoxy equivalent weight 184 to 190; viscosity at 25°C 12000 to 14000 centipoise); EPILOX A 18-00 from Leuna Epilox GmbH (Leuna, Germany) (liquid; epoxy equivalent weight 175 to 185; viscosity at 25°C 8000 to 10000 centipoise).

[0061] In the context of the present application, the term "solid epoxy resin" means an epoxy resin that is solid at normal temperature.

[0062] According to a preferred embodiment, the epoxy equivalent of the solid epoxy resin is 450 to 2500 g / eq, or 450 to 1700 g / eq, or 500 to 1600 g / eq, or 600 to 1500 g / eq, or 700 to 1200 g / eq, or 800 to 1100 g / eq, or 900 to 1000 g / eq.

[0063] According to a preferred embodiment, the number average molecular weight of the solid epoxy resin is greater than 1000 g / mol, or greater than 1500 g / mol, or greater than 2000 g / mol, or greater than 2500 g / mol, or greater than 3000 g / mol.

[0064] According to one embodiment, the number average molecular weight of the solid epoxy resin is less than 10000 g / mol, or less than 9000 g / mol, or less than 8000 g / mol, or less than 7000 g / mol, or less than 6000 g / mol, or less than 5000 g / mol.

[0065] For example, the number average molecular weight of the solid epoxy resin may be 1000 g / mol, or 1200 g / mol, or 1400 g / mol, or 1600 g / mol, or 1800 g / mol, or 2000 g / mol, or 2200 g / mol, or 2400 g / mol, or 2600 g / mol, or 2800 g / mol, or 3000 g / mol, or 4000 g / mol.

[0066] According to a preferred embodiment, the solid epoxy resin has an average of 2 to 5 epoxy functional groups per molecule, preferably 2.5 to 5 epoxy functional groups, preferably 3 to 5 epoxy functional groups, preferably 3.5 to 5 epoxy functional groups. For example, the solid epoxy resin has an average of 2.1, or 2.2, or 2.3, or 2.4, or 2.5, or 2.6, or 2.7, or 2.8, or 2.9, or 3.0, or 3.1, or 3.2, or 3.3, or 3.4, or 3.5, or 3.6, or 3.7, or 3.8, or 3.9, or 4.0, or 4.1, or 4.2, or 4.3, or 4.4, or 4.5, or 4.6, or 4.7, or 4.8, or 4.9 epoxy functional groups per molecule.

[0067] According to a preferred embodiment, the solid epoxy resin is selected from: solid bisphenol A epoxy resin, solid bisphenol A novolac epoxy resin, bisphenol S glycidyl ether epoxy resin, glycidyl ester epoxy resin.

[0068] The solid epoxy resin is commercially available. As non-limiting examples, the following solid epoxy resins may be mentioned: ARALDITE GT7071, ARALDITE GT7072, ARALDITE GT7004, ARALDITE GT6084-2, ARALDITE GT6097, ARALDITE GT6099, ARALDITE GT6610, ARALDITE GT7255, ARALDITE GT7013, ARALDITE GT7074, EBA-9000, bisphenol A type solid epoxy resin NPES-903, bisphenol A type solid epoxy resin NPES-905L, bisphenol A type solid epoxy resin NPES-904.

[0069] In a preferred embodiment, the solid epoxy resin is selected from isophthalic acid epoxy resin and trimesic acid epoxy resin.

[0070] In one example of the present application, the viscosity of the epoxy resin at 40°C is 500-15000 mP.s, such as 1000-12000 mP.s, 1500-10000 mP.s, 2000-8000 mP.s, 3000-5000 mP.s; the epoxy value is 0.5-1.5, such as 0.6-1.2, 0.7-1, 0.8-0.9.

[0071] In one example of the present application, based on 100 parts by weight of epoxy resin, the amount of the curing agent composition is 20-100 parts by weight, preferably 30-80 parts by weight, more preferably 35-70 parts by weight, and even more preferably 40-60 parts by weight.

[0072] According to a preferred embodiment, the epoxy resin composition of the present application further comprises an auxiliary agent.

[0073] In the context of the present application, the term "auxiliary agent" means an additive added to the above-mentioned curing agent composition and epoxy resin for improving the performance or processing technology of the epoxy resin composition, which helps to adjust the properties of the obtained epoxy resin composition.

[0074] As non-limiting examples, the auxiliary agents that may be mentioned include: inorganic fillers, pigments, system stabilizers, tackifiers, impact modifiers, defoamers, coupling agents, diluents, anti-aging agents.

[0075] According to one embodiment, the inorganic filler may be selected from aluminum hydroxide particles, silicon dioxide particles, calcium carbonate particles, aluminum oxide particles, and the like.

[0076] According to one embodiment, the pigment may be titanium dioxide, carbon black, or the like.

[0077] According to one embodiment, the system stabilizer may be selected from one or more of thiourea, hydroquinone, methoxyphenol and 2,6-di-tert-butyl-p-cresol.

[0078] According to one embodiment, the tackifier may be an acrylic copolymer tackifier, such as acResin DS 3532 from BASF; P-2M (2-hydroxyethyl methacrylate phosphate) from KYOEISHA CHEMICAL.

[0079] The impact modifier may be commercially available, for example, MBS (methacrylate-butadiene-styrene) core-shell copolymer impact modifier produced by Dow, with an average particle size of 100 to 400 microns; NBR (butadiene-acrylonitrile rubber) impact modifier produced by ARLANXEO HighPerformance, with an average particle size of 500 to 900 microns.

[0080] The auxiliary agent is not particularly limited. In an exemplary embodiment, the auxiliary agent is selected from a defoaming agent and a silane coupling agent.

[0081] As examples of defoamers, mention may be made of those available under the following trade names: BYK-W903, BYK-W909, BYK-W920, BYK-W935, BYK-W940, BYK-A535, BYK-052, BYK-052, BYK-088, BYK-077, BYK-071, BYK-070, BYK-065, BYK-A500, BYK-A525, BYK-055, BYK-141, BYK-A530, BYK-054, BYK-S 732 and BYK-A 506.

[0082] According to one embodiment, the coupling agent is a silane coupling agent. As examples of silane coupling agents, there can be mentioned KH550, KH 560, KH 570, SCA A10E, SCA A10M, SCA E87F, SCA E87T, etc.

[0083] The amount of the auxiliary agent may depend on the desired properties of the final product. In an exemplary embodiment, the content of the auxiliary agent in the epoxy resin composition of the present application may be 1 to 3 parts, such as 1.2 parts, or 1.4 parts, or 1.6 parts, or 1.8 parts, or 2.0 parts, or 2.2 parts, or 2.4 parts, or 2.6 parts, or 2.8 parts.

[0084] The epoxy resin composition described in the present application can be prepared using a common method. For example, the curing agent composition and the epoxy resin and the optional auxiliary agent can be mixed together by a physical method without using a solvent. The mixing can be carried out under heating (e.g., 30-100° C.).

[0085] According to one embodiment of the present application, no thermoplastic resin toughening agent is used in the epoxy resin composition and preparation method of the present application. For example, the thermoplastic resin toughening agent includes one or more of the following, or includes all of the following thermoplastic resin toughening agents: polysulfone, polyethersulfone, polyarylethersulfone, polyetherketone.

[0086] Another aspect of the present application provides an epoxy resin product, which is prepared using the epoxy resin composition described in the present application.

[0087] In one example of the present application, the epoxy resin product can use the epoxy resin composition as an adhesive to bond various elements (such as fibers, sheets, parts, etc.) together. For example, the epoxy resin product includes but is not limited to adhesive films and fiber-reinforced epoxy resin composite products.

[0088] The present application is described below in the form of specific examples, and its purpose is to better understand the content of the present application. It should be understood that these examples are merely illustrative and non-restrictive. The reagents used in the examples are conventionally purchased from the market unless otherwise specified. The methods and conditions used in the examples are conventional methods and conditions unless otherwise specified.

[0089] Example

[0090] Viscosity test method: ASTM D2196;

[0091] Amine value test method: ASTM D2074-2007;

[0092] Tensile shear strength test method: GB / T 7124-2008 Epoxy value test: GB / T 601-2002. The main raw material information used in the examples is as follows:

[0093]

[0094]

[0095]

[0096] Example 1

[0097] Preparation of curing agent composition:

[0098] 54.5g of pyromellitic anhydride was added to DMF, and after dissolving, 148.5g of 3,3'-diaminodiphenylmethane was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 1 containing amino terminal groups. 54.5g of pyromellitic anhydride was added to DMF, and after dissolving, 148.5g of 4,4'-diaminodiphenylmethane was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 2 containing amino terminal groups. 50g of oligomer 1, 50g of oligomer 2, and 12g of 1-methylimidazole were added to 300g of MXDA, heated at 80-100°C, dissolved, and stirred for 1-2h to obtain curing agent 1, and the viscosity was measured to be 4000-5000mPa.S at 25°C.

[0099] Curing agent 1 25℃ viscosity mPa.S 4000-5000 Amine value mgKOH / g 460

[0100] Preparation of epoxy resin:

[0101] AG-80, AFG-90H and EBA-9000 were mixed in a mass ratio of 5:2:3 and mixed at 80°C for 1 hour to obtain epoxy resin 1. The viscosity of epoxy resin 1 was measured to be 4000-6000 mP.s at 40°C, and the epoxy value was 0.81.

[0102] Preparation of epoxy resin composition:

[0103] The epoxy resin 1 and the curing agent 1 are mixed at a ratio of 100:50 to prepare an epoxy resin composition 1. The epoxy resin composition 1 is prepared into a specimen and subjected to a curing procedure of 2h@100°C+2h@150°C+2h@180°C and then tested for mechanical properties.

[0104] Composition 1 25℃ tensile shear strength MPa 18 250℃ tensile shear strength MPa 6

[0105] Comparative Example 1

[0106] Preparation of curing agent composition:

[0107] 54.5 g of pyromellitic anhydride was added to DMF, and after dissolving, 148.5 g of 4,4'-diaminodiphenylmethane was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 2 containing amino terminal groups. 100 g of oligomer 2 and 12 g of 1-methylimidazole were added to 300 g of MXDA, and heated at 80-120°C to dissolve and stir for 1-2 hours to obtain comparative curing agent 1.

[0108]

[0109] Since comparative curing agent 1 could not be completely dissolved to form a uniform liquid, it could not be mixed with epoxy resin to form an epoxy resin composition, and thus no further testing was performed.

[0110] Comparative Example 2

[0111] Preparation of curing agent composition:

[0112] 100g DDS and 12g 1-methylimidazole were added to 300g MXDA, heated at 80-100°C to dissolve and stirred for 1-2h to obtain comparative curing agent 2, and the viscosity was measured to be 200-500mPa.S at 25°C.

[0113] Comparison of curing agent 2 25℃ viscosity mPa.S 200-500 Amine value mgKOH / g 682

[0114] Preparation of epoxy resin:

[0115] AG-80, AFG-90H and EBA-9000 were mixed in a mass ratio of 5:2:3 and mixed at 80°C for 1 hour to obtain comparative epoxy resin 2. The comparative epoxy resin 2 was measured to have a viscosity of 4000-6000 mP.s at 40°C and an epoxy value of 0.81 mol / 100g.

[0116] Preparation of epoxy resin composition:

[0117] The comparative epoxy resin 2 and the comparative curing agent 2 were mixed at a ratio of 100:32 to prepare a comparative epoxy resin composition 2. The comparative epoxy resin composition 2 was prepared into a specimen, and subjected to a curing procedure of 2h@100°C+2h@150°C+2h@180°C, and then the mechanical properties were tested.

[0118] Comparative composition 2 25℃ tensile shear strength MPa 8 250℃ tensile shear strength MPa 2

[0119] Example 2

[0120] Preparation of curing agent composition:

[0121] 54.5g of pyromellitic anhydride was added to DMF, and after dissolving, 148.5g of 3,3'-diaminodiphenyl ether was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 1 containing amino terminal groups. 54.5g of pyromellitic anhydride was added to DMF, and after dissolving, 148.5g of 4,4'-diaminodiphenyl ether was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 2 containing amino terminal groups. 50g of oligomer 1, 50g of oligomer 2, and 12g of 1-methylimidazole were added to 300g of MXDA, heated at 80-100°C, dissolved, and stirred for 1-2h to obtain curing agent 2, and the viscosity was measured to be 3000-4000mPa.S at 25°C.

[0122] Curing agent 2 25℃ viscosity mPa.S 3000-4000 Amine value mgKOH / g 472

[0123] Preparation of epoxy resin:

[0124] AG-80, AFG-90H and EBA-9000 were mixed in a mass ratio of 5:2:3 and mixed at 80°C for 1 hour to obtain epoxy resin 2. The viscosity of epoxy resin 2 was measured to be 4000-6000 mP.s at 40°C, and the epoxy value was 0.81.

[0125] Preparation of epoxy resin composition:

[0126] The epoxy resin 2 and the curing agent 2 were mixed at a ratio of 100:50 to prepare an epoxy resin composition 2. The epoxy resin composition 2 was prepared into a specimen and subjected to a curing procedure of 2h@100°C+2h@150°C+2h@180°C and then tested for mechanical properties.

[0127] Composition 2 25℃ tensile shear strength MPa 20 250℃ tensile shear strength MPa 8

[0128] Example 3

[0129] Preparation of curing agent composition:

[0130] 54.5g of pyromellitic anhydride was added to DMF, and after dissolving, 99g of 3,3'-diaminodiphenylmethane was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 1 containing amino terminal groups. 54.5g of pyromellitic anhydride was added to DMF, and after dissolving, 99g of 4,4'-diaminodiphenylmethane was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 2 containing amino terminal groups. 50g of oligomer 1, 50g of oligomer 2, and 12g of 1-methylimidazole were added to 300g of MXDA, heated at 80-100°C, dissolved, and stirred for 1-2h to obtain curing agent 3, and the viscosity was measured to be 3000-4000mPa.S at 25°C.

[0131] Curing agent 3 25℃ viscosity mPa.S 3000-4000 Amine value mgKOH / g 466

[0132] Preparation of epoxy resin:

[0133] AG-80, AFG-90H and EBA-9000 were mixed in a mass ratio of 5:2:3 and mixed at 80°C for 1 hour to obtain epoxy resin 3. The viscosity of epoxy resin 3 was measured to be 4000-6000 mP.s at 40°C, and the epoxy value was 0.81.

[0134] Preparation of epoxy resin composition:

[0135] The epoxy resin 3 and the curing agent 3 were mixed at a ratio of 100:50 to prepare an epoxy resin composition 3. The epoxy resin composition 3 was prepared into a specimen and subjected to a curing procedure of 2h@100°C+2h@150°C+2h@180°C and then tested for mechanical properties.

[0136] Composition 3 25℃ tensile shear strength MPa 15 250℃ tensile shear strength MPa 5

[0137] Example 4

[0138] Preparation of curing agent composition:

[0139] 54.5g of pyromellitic anhydride was added to DMF, and after dissolving, 148.5g of 3,3'-diaminodiphenylmethane was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 1 containing amino terminal groups. 54.5g of pyromellitic anhydride was added to DMF, and after dissolving, 148.5g of 4,4'-diaminodiphenylmethane was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 2 containing amino terminal groups. 50g of oligomer 1, 50g of oligomer 2, and 12g of 1-methylimidazole were added to 300g of MXDA, heated at 80-100°C, dissolved, and stirred for 1-2h to obtain curing agent 4, and the viscosity was measured to be 4000-5000mPa.S at 25°C.

[0140] Curing agent 4 25℃ viscosity mPa.S 4000-5000 Amine value mgKOH / g 460

[0141] Preparation of epoxy resin:

[0142] AG-80, AFG-90H and EBA-9000 were mixed in a mass ratio of 5:3:2 and mixed at 80°C for 1 hour to obtain epoxy resin 4. The viscosity of epoxy resin 4 was measured to be 3000-5000 mP.s at 40°C, and the epoxy value was 0.85.

[0143] Preparation of epoxy resin composition:

[0144] The epoxy resin 4 and the curing agent 4 were mixed at a ratio of 100:52 to prepare an epoxy resin composition 4. The epoxy resin composition 4 was prepared into a specimen and subjected to a curing procedure of 2h@100°C+2h@150°C+2h@180°C and then tested for mechanical properties.

[0145]

[0146]

[0147] Example 5

[0148] Preparation of curing agent composition:

[0149] 54.5 g of pyromellitic anhydride was added to DMF, and after dissolving, 148.5 g of 3,3'-diaminodiphenylmethane was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 1 containing amino terminal groups. 54.5 g of pyromellitic anhydride was added to DMF, and after dissolving, 148.5 g of 4,4'-diaminodiphenylmethane was added, stirred at room temperature for 4-6 hours, washed with water, and dried at 110°C to obtain oligomer 2 containing amino terminal groups. 50 g of oligomer 1, 50 g of oligomer 2, and 12 g of 1-methylimidazole were added to 300 g of DETDA, heated at 80-100°C, dissolved, and stirred for 1-2 hours to obtain curing agent 5, and the viscosity was measured to be 7000-8000 mPa.S at 25°C.

[0150] Curing agent 5 25℃ viscosity mPa.S 7000-8000 Amine value mgKOH / g 410

[0151] Preparation of epoxy resin:

[0152] AG-80, AFG-90H and EBA-9000 were mixed in a mass ratio of 5:2:3 and mixed at 80°C for 1 hour to obtain epoxy resin 5. The viscosity of epoxy resin 5 was measured to be 4000-6000 mP.s at 40°C, and the epoxy value was 0.81.

[0153] Preparation of epoxy resin composition:

[0154] The epoxy resin 5 and the curing agent 5 were mixed at a ratio of 100:55 to prepare an epoxy resin composition 5. The epoxy resin composition 5 was prepared into a specimen and subjected to a curing procedure of 2h@100°C+2h@150°C+4h@180°C and then tested for mechanical properties.

[0155] Composition 5 25℃ tensile shear strength MPa 20 250℃ tensile shear strength MPa 5

Claims

1. A curing agent composition for epoxy resin, comprising: (1) an oligomer formed by an anhydride and a first aromatic diamine; (2) an oligomer formed by an acid anhydride and a second aromatic diamine, wherein the second aromatic diamine and the first aromatic diamine are isomers; (3) liquid aromatic diamines; and (4) Optional accelerator.

2. The curing agent composition according to claim 1, wherein In the components (1) and (2), the acid anhydrides may be the same or different, preferably the same; Preferably, the acid anhydride includes phthalic anhydride, phthalic anhydride, maleic anhydride, trimellitic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnorbornene dicarboxylic anhydride, methylhexahydrophthalic anhydride, hexahydrophthalic anhydride, methyl humic anhydride, pyromellitic dianhydride, benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, and cyclohexanetricarboxylic anhydride; Preferably, the acid anhydride has 1 or 2 aliphatic rings or aromatic rings in the molecule, 1 or 2 acid anhydride groups, and has 4-25 carbon atoms, preferably 8-20 carbon atoms.

3. The curing agent composition according to claim 1, wherein The first or second aromatic diamine is represented by the following structure: H2N-R 10 -NH2, where R 10 is an aryl group containing 6-16 carbon atoms in the ring and, optionally, up to one heteroatom comprising -N-, -O-, or -S-; Preferably R 10 is a diphenylene group or a diphenylmethane group; Preferably, the first or second aromatic diamine is 2,6-diaminopyridine, 3,5-diaminopyridine, m-phenylenediamine, p-phenylenediamine, p,p'-methylenedianiline, 2,6-diaminotoluene, and 2,4-diaminotoluene; Alternatively, the first or second aromatic diamine includes phenylenediamines such as 1,4-diaminobenzene, 1,3-diaminobenzene, and 1,2-diaminobenzene; diphenyl(thio)ether diamines such as 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl ether, and 3,3'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide; benzophenone diamines such as 3,3'-diaminobenzophenone and 4,4'-diaminobenzophenone; diphenylphosphine diamines such as 3,3'-diaminodiphenyl ether, diphenyl alkylene diamines, such as 3,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylpropane, and 4,4'-diaminodiphenylpropane; diphenyl sulfide diamines, such as 3,3'-diaminodiphenyl sulfide and 4,4'-diaminodiphenyl sulfide; diphenyl sulfone diamines, such as 3,3'-diaminodiphenyl sulfone and 4,4'-diaminodiphenyl sulfone; and benzidines, such as benzidine and 3,3'-dimethylbenzidine.

4. The curing agent composition according to claim 1, wherein The liquid aromatic diamine is selected from at least one of the following: dimethylthiotoluenediamine (DMTDA), diethyltoluenediamine (DETDA), 4,4'-bis-sec-butylaminodiphenylmethane (MDBA), m-phenylenediamine (MXDA), p-phenylenediamine and o-phenylenediamine; Preferably, the amount of the liquid aromatic diamine is 100-1000 parts by weight, preferably 100-800 parts by weight, more preferably 150-600 parts by weight, and even more preferably 200-400 parts by weight, based on 100 parts by weight of the total weight of oligomer (1) and oligomer (2).

5. The curing agent composition according to claim 1, wherein The accelerator is selected from the group consisting of imidazole and its derivatives, and amine adducts. For example, the curing accelerator may be imidazole, 1-methylimidazole, 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, an adduct of 2-methylimidazole and butyl glycidyl ether, or an adduct of 2-methylimidazole and 2-ethylhexyl glycidyl ether. Preferably, the amount of the accelerator is 1 to 30 parts by weight, preferably 2 to 25 parts by weight, preferably 3 to 20 parts by weight, preferably 5 to 18 parts by weight, preferably 8 to 16 parts by weight, based on 100 parts by weight of the total weight of oligomer (1) and oligomer (2).

6. An epoxy resin composition, comprising: (1) The epoxy resin curing agent composition according to any one of claims 1 to 5; as well as (2) Epoxy resin.

7. The epoxy resin composition according to claim 6, wherein The epoxy resin is a liquid epoxy resin, a solid epoxy resin or a combination thereof; Preferably, based on 100 parts by weight of the epoxy resin, the amount of the curing agent composition is 20-100 parts by weight, preferably 30-80 parts by weight, more preferably 35-70 parts by weight, and even more preferably 40-60 parts by weight.

8. The epoxy resin composition according to claim 6, wherein The epoxy resin composition further comprises an auxiliary agent; Preferably, the auxiliary agents include: inorganic fillers, pigments, system stabilizers, tackifiers, impact modifiers, defoamers, coupling agents, diluents and / or anti-aging agents.

9. An epoxy resin product, prepared using the epoxy resin composition according to any one of claims 6 to 8.

10. The epoxy resin product according to claim 9, wherein The epoxy resin product is prepared by bonding components together using the epoxy resin composition according to any one of claims 6 to 8 as an adhesive; preferably, the epoxy resin product comprises an adhesive film or a fiber-reinforced epoxy resin composite product.