High-damping oil-resistant rubber vibration damping material with closed-cell foaming structure and preparation method of high-damping oil-resistant rubber vibration damping material

By introducing polymer microspheres and sheet fillers into the rubber material, and performing surface modification and dual vulcanization treatment, forming a closed-cell foam structure, the shortcomings of existing rubber materials in oil resistance and stability are solved, and the Better damping performance and oil resistance.

CN119039676APending Publication Date: 2024-11-29GLOBAL ENERGY INTERCONNECTION RES INST CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411092610.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing rubber vibration damping materials have shortcomings in oil resistance and material structural stability, especially in insulating oil environments, resulting in unsatisfactory vibration damping effects and unstable material performance.

Method used

Rubber materials with closed-cell foam structure are used to introduce polymer microspheres and sheet fillers and undergo surface modification treatment, combined with the dual vulcanization reaction in the vulcanization system to form a polysulfide bond and a carbon-carbon single-bonded vulcanization structure, which enhances the The damping properties and oil resistance of the material.

Benefits of technology

It significantly improves the damping and oil resistance of rubber materials, enhances the material's resistance to high temperature and aging, and improves its stability and service life in an insulating oil environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004986995500000061
    Figure BDA0004986995500000061
  • Figure BDA0004986995500000071
    Figure BDA0004986995500000071
  • Figure BDA0004986995500000091
    Figure BDA0004986995500000091
Patent Text Reader

Abstract

The invention provides a high-damping oil-resistant rubber vibration-damping material with a closed-cell foaming structure and a preparation method of the high-damping oil-resistant rubber vibration-damping material. The material is composed of a rubber matrix, a spherical filler, a lamellar filler, a surface modifier, a plasticizer, an anti-aging agent, a polymer microsphere pre-dispersed rubber master batch, sulfur, zinc oxide, stearic acid, a vulcanization accelerator, a peroxide vulcanizing agent and an auxiliary vulcanizing agent. The preparation method comprises the following steps: preparing polymer microsphere pre-dispersed masterbatch, organically modifying the surface of the lamellar filler, and preparing a rubber blended rubber material. Through modification and uniform dispersion of the lamellar filler, the oil resistance and damping performance of the rubber material are improved; the polymer microspheres form a closed-pore structure, so that the vibration absorption capacity is enhanced; the sulfur and peroxide dual vulcanization system improves the high temperature resistance, oil resistance and aging resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber damping materials, and in particular to a high-damping oil-resistant rubber vibration-damping material with a closed-cell foaming structure and a preparation method thereof. Background Art

[0002] With the rapid development of industry and technology, my country's power industry has made significant progress, and the voltage level and capacity of power equipment have been continuously improved. However, these equipment inevitably generate mechanical vibration and noise pollution during operation, which has caused great trouble to the surrounding residents. Therefore, the power industry has an increasingly urgent need to suppress vibration and noise.

[0003] Due to its unique viscoelastic properties, rubber materials have excellent vibration reduction and isolation capabilities, and have important application potential in the field of vibration reduction and noise reduction of power transmission and transformation equipment. The application locations of rubber vibration reduction materials in power transmission and transformation equipment include the outside and inside of the device body. Compared with the relatively simple design of externally applied rubber materials, internally applied rubber materials face more complex challenges, especially the rubber materials inside the device body need to be immersed in insulating oil for a long time, which puts higher requirements on the material's oil resistance and damping performance. This has always been the focus and difficulty of research in this field.

[0004] Specifically, the rubber material on the outside of the device body is mainly used to isolate the transmission of external mechanical vibration and noise. The design requirements are relatively simple, and usually only the vibration reduction performance and durability of the material need to be considered. As for the rubber material inside the device body, in addition to having good vibration reduction and noise reduction effects, it must also maintain the stability of its physical and chemical properties in an environment where it is immersed in insulating oil for a long time. Insulating oil places strict requirements on the oil resistance of rubber materials. At the same time, the damping performance of rubber materials must also maintain excellent performance under harsh conditions such as high temperature and high pressure.

[0005] In recent years, the number of patent applications in the field of rubber vibration damping materials has increased significantly. Patent No. ZL

[0006] 202010562305.7 discloses a high-performance rubber damping material and its preparation method. The patent grafts hydroxyethyl methacrylate and lignin onto the rubber molecular chain of natural latex through graft copolymerization to prepare a high-performance rubber damping material. However, the natural rubber matrix has poor transformer oil resistance and cannot be used in the internal environment of power transmission and transformation equipment such as transformers.

[0007] Patent No. ZL 201810486284.8 discloses a wide temperature range high damping oil-resistant shock-absorbing rubber composite material and its preparation method. The composite material is mainly made by mixing nitrile / polyamide blended elastomer and butyl rubber with other additives, and then vulcanizing and finalizing. The patent adopts the addition of non-polar nitrile rubber to increase the damping effect, but the non-polar butyl rubber and the polar nitrile / polyamide blended elastomer cannot achieve good compatibility at the microscopic level, resulting in poor material performance. In addition, the non-polar butyl rubber has poor oil resistance. When the filling amount is large, it will introduce defective structures in the rubber material, affecting the stability of the material.

[0008] Introducing a foaming structure into a rubber material is one of the methods to improve vibration damping performance. Rubber vibration damping pads can rely on the foaming structure in the rubber material to absorb external vibration energy, thereby playing a role in reducing vibration and noise. Patent No. ZL201010142415.4 discloses a low-hysteresis microporous rubber material for high-speed railway fastener vibration reduction and its preparation method, which mainly introduces a chemical foaming agent into the rubber matrix to prepare a vibration damping pad with a pore structure. However, due to the instability of the chemical foaming agent, an interpenetrating structure of pores is easily formed during the foaming process, resulting in a decrease in the vibration reduction effect. At the same time, the oil resistance of the interpenetrating structure is poor. Once the insulating oil is immersed, the rubber material will swell severely, affecting its performance.

[0009] In summary, the rubber vibration damping materials in the prior art still have many deficiencies in practical applications, especially in terms of oil resistance and material structure stability, which need further improvement and optimization. Therefore, the development of high-performance rubber vibration damping materials suitable for power transmission and transformation equipment, especially oil-resistant rubber materials, is of great significance for improving the operating stability of power transmission and transformation equipment and reducing noise pollution. This not only helps to improve the quality of life of residents, but also promotes the sustainable development of the power industry. Future research should focus on the improvement of material formulations and the application of new foaming technologies to improve the comprehensive performance of rubber vibration damping materials in power transmission and transformation equipment. The rubber material with a closed-cell foaming structure has a large number of independent bubble structures inside, which not only has a low density, but also can effectively absorb and isolate vibration energy, thereby significantly improving the vibration damping performance. At the same time, the closed-cell structure can also prevent the penetration of oil substances, thereby enhancing the oil resistance of the material. Therefore, it is of great practical significance to develop a high-damping oil-resistant rubber vibration damping material with a closed-cell foaming structure.

[0010] The purpose of the present invention is to provide a high-damping oil-resistant rubber vibration-damping material with a closed-cell foam structure and a preparation method thereof, so as to solve the problems of poor oil resistance, poor vibration reduction effect and complex preparation process existing in the prior art, thereby meeting the needs of various types of mechanical equipment for high-performance vibration-damping materials. Summary of the invention

[0011] In order to solve the above problems in the prior art, the present invention proposes a rubber vibration damping material with a closed-cell foam structure, and the material composition is as follows:

[0012] Rubber matrix: 100 parts by mass;

[0013] Spherical filler: 30-60 parts by mass;

[0014] Lamellar filler: 1 to 10 parts by mass;

[0015] Surface modifier: 1 to 10 parts by mass;

[0016] Plasticizer: 5-20 parts by weight;

[0017] Antiaging agent: 2 to 6 parts by weight;

[0018] Polymer microsphere pre-dispersed masterbatch: 2-10 parts by weight;

[0019] Sulfur: 1 to 5 parts by mass;

[0020] Zinc oxide: 1 to 5 parts by mass;

[0021] Stearic acid: 1 to 5 parts by mass;

[0022] Vulcanization accelerator: 0.5-5 parts by mass;

[0023] Peroxide curing agent: 1 to 5 parts by mass;

[0024] Vulcanizing agent: 1 to 5 parts by weight.

[0025] The rubber matrix is ​​one or more of nitrile rubber, hydrogenated nitrile rubber and chloroprene rubber.

[0026] The spherical filler is one or more of carbon black, white carbon black, zinc oxide and aluminum oxide.

[0027] The lamellar filler is one or more of graphene, graphene oxide, kaolin and hydrotalcite.

[0028] The surface modifier is one or more of a glycidyl ether-terminated long-chain polyether silane coupling agent, dodecyl trimethoxy silane, and hexadecyl trimethoxy silane.

[0029] The plasticizer is one or more of liquid nitrile rubber, butyl benzyl phthalate, tricresyl phosphate and dinonyl phthalate.

[0030] The antioxidant is one or more of antioxidant RD, antioxidant D, antioxidant NBC, antioxidant 4010NA and antioxidant BLE.

[0031] The foaming agent is expandable polymer microspheres with a particle size of 1 to 100 μm.

[0032] The vulcanization accelerator is one or more of accelerator CZ, accelerator DM, accelerator TT, accelerator NS and accelerator ZDC.

[0033] The peroxide curing agent is one or more of diisopropylbenzene peroxide, 2,5-dimethyl-2,5-(di-tert-butylperoxy)hexane and diacyl peroxide.

[0034] The vulcanizing agent is one or more of the vulcanizing agent TAIC, the vulcanizing agent HVA-2 and the vulcanizing agent TMPT.

[0035] The preparation method of the rubber vibration damping material comprises the following steps:

[0036] preparing a polymer microsphere pre-dispersed masterbatch;

[0037] Organic modification of the surface of the lamellar filler;

[0038] Preparation of rubber blends.

[0039] The steps of preparing the polymer microsphere pre-dispersed masterbatch are as follows:

[0040] (1) dispersing a certain amount of polymer microspheres in deionized water, then adding a surfactant to the dispersion, wherein the mass ratio of polymer microspheres, surfactant, and deionized water is 1:(1-20):(50-1000), and emulsifying and mixing the mixture in a high shear homogenizer, wherein the emulsification speed is 1000-12000 rpm, the emulsification temperature is 30-80° C., and the emulsification time is 5-60 minutes to obtain a polymer microsphere dispersion;

[0041] (2) Mixing the polymer microsphere dispersion with the rubber latex in a solid mass ratio of 1:(5-20), placing the mixture in a stirring device for mixing, and then slowly adding the mixture into a flocculation reactor, stirring sufficiently until flocculation is complete, and washing and drying the flocculent gel.

[0042] The steps of organically modifying the surface of the flaky filler are as follows:

[0043] (1) placing a surface modifier in a mixture of ethanol and water, wherein the volume ratio of ethanol to water is 1:(0.1-0.5), and the volume concentration range of the surface modifier in the alcohol-water mixture is 1-10%, and stirring and hydrolyzing the prepared modifier dispersion at 20-40° C. for 10 hours;

[0044] (2) The prepared modifier is dispersed and sprayed evenly on the surface of the lamellar filler, and then the treated filler is heat-treated in an oven at 100-150° C. for 5-30 minutes to finally obtain a lamellar filler with surface modification.

[0045] The steps of preparing the rubber blend are as follows:

[0046] (1) Adding a rubber matrix into a rubber internal mixer, followed by adding zinc oxide, stearic acid, and an antioxidant, and then adding a foaming agent to pre-disperse the masterbatch, and mixing at 50° C. to 80° C. for 2 to 5 minutes; then adding a spherical filler, an organic modified lamellar filler, and a plasticizer, and mixing at 50° C. to 100° C. for 2 to 5 minutes; after the rubber materials are evenly mixed, discharging the mixed rubber and leaving it for 24 to 48 hours;

[0047] (2) Put the rubber mix back into the rubber internal mixer, add sulfur, vulcanization accelerator, peroxide vulcanizing agent, and co-vulcanizing agent in sequence, mix at 40-80°C for 2-5 minutes, and after the rubber is evenly mixed, discharge the rubber and put it aside for use.

[0048] The beneficial effects of the present invention are as follows:

[0049] (1) The present invention introduces a lamellar filler into the rubber material system and performs surface modification on the lamellar filler so that the modified lamellar filler has better dispersibility in the rubber matrix, and a chemical interface bonding effect is formed between the modified lamellar filler and the rubber matrix. The introduction of the lamellar filler enhances the oil resistance of the rubber material, and under dynamic action, multiple interface friction micro-regions are formed between the lamellar structure and the carbon black filler particles, thereby improving the damping performance of the rubber material.

[0050] (2) The present invention introduces polymer microspheres, and improves the dispersibility of polymer microspheres in the rubber matrix by adopting a liquid phase composite pre-dispersion method, thereby achieving uniform dispersion of polymer microspheres in the rubber matrix. When the polymer microspheres are subjected to high temperature during the molding of the rubber material, the internal expansion gas expands to form a closed-cell expansion structure, thereby improving the vibration absorption capacity of the rubber material and improving the damping performance of the rubber material. Since the polymer microspheres are closed-cell structures, external insulating oil cannot invade the interior of the microspheres, thereby making the rubber material have better oil resistance.

[0051] (3) The present invention introduces a dual vulcanization system of sulfur vulcanization and peroxide into the vulcanization system, so that a polysulfide bond vulcanization structure with good dynamic performance is formed in the rubber matrix, and a high temperature resistant and stable carbon-carbon single bond vulcanization structure is also formed. Under the action of the dual chemical cross-linking bonds, the high temperature resistance, oil resistance and anti-aging ability of the rubber material are improved, thereby promoting the improvement of the high oil resistance and damping performance of the rubber material. DETAILED DESCRIPTION

[0052] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used for further explanation of the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art to the present invention according to the content of the present invention still belong to the scope of protection of the present invention. If no specific experimental steps or conditions are indicated in the embodiments of the present invention, the operation or conditions of the conventional experimental steps described in the literature in this field can be carried out. If the manufacturer of the reagents or instruments used is not indicated, they are all conventional reagent products that can be obtained commercially.

[0053] Example 1

[0054] This embodiment provides a high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure and a preparation method thereof. The composition of the material is as follows:

[0055]

[0056]

[0057] In this embodiment, the preparation method of the high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure includes the following specific steps:

[0058] 1. Preparation steps of polymer microsphere pre-dispersed masterbatch:

[0059] (1) Preparation of polymer microsphere dispersion: 10 g of polymer microspheres were dispersed in deionized water, and then sodium dodecylbenzene sulfonate was added to the dispersion. The mass ratio of polymer microspheres, sodium dodecylbenzene sulfonate and deionized water was 1:10:200. The mixture was emulsified and mixed in a high shear homogenizer at an emulsification speed of 1000 rpm, an emulsification temperature of 60°C and an emulsification time of 10 minutes, and finally a polymer microsphere dispersion with stable dispersion was obtained.

[0060] (2) Preparation of polymer microsphere pre-dispersed masterbatch: The polymer microsphere dispersion liquid is mixed with rubber latex at a solid mass ratio of 1:5, and the mixed liquid is placed in a stirring device for full mixing, and then the mixed liquid is slowly added to a flocculation reactor and fully stirred until flocculation is complete. The flocculated gel is washed and dried to obtain a pre-dispersed masterbatch.

[0061] 2. Surface organic modification steps of lamellar fillers:

[0062] (1) Preparation of surface modifier: The surface modifier is placed in a mixture of ethanol and water, wherein the volume ratio of ethanol to water is 1:0.1, and the volume concentration of the surface modifier in the alcohol-water mixture is controlled at 5%. The prepared modifier dispersion is stirred and hydrolyzed at 30° C. for 10 hours.

[0063] (2) Surface modification of lamellar fillers: The prepared modifier is dispersed and sprayed evenly on the surface of the lamellar fillers, and then the treated fillers are heat treated at high temperature in an oven at 50°C for 5 minutes to finally obtain the lamellar fillers after surface modification.

[0064] 3. Preparation steps of rubber blending compound:

[0065] (1) Preliminary mixing: Add 50g of rubber matrix to a rubber internal mixer, add zinc oxide, stearic acid, antioxidant 4010NA in sequence, and then add 60g of polymer microsphere pre-dispersed masterbatch, and mix at 60°C for 5 minutes. Then add carbon black N330, organic modified graphene, and butyl benzyl phthalate, and mix at 100°C for 2 minutes. After the rubber materials are mixed evenly, discharge the mixed rubber and leave it for 48 hours.

[0066] (2) Final mixing: Put the rubber mix back into the rubber internal mixer, add sulfur, vulcanization accelerator DM, diisopropylbenzene peroxide, and TAIC in sequence, mix at 50°C for 3 minutes, and discharge the rubber after the rubber is evenly mixed and put aside for later use.

[0067] The specific experimental steps or conditions described in the above examples, if not specifically noted, were carried out in accordance with conventional experimental steps and conditions in the art. The reagents or instruments used, if not indicated by the manufacturer, were conventional reagent products that can be purchased on the market.

[0068] In order to reflect the technical advantages of the present invention, comparative example 1-1 (without pre-dispersion treatment of polymer microspheres) and comparative example 1-2 (direct addition of interface modifier without the filler modification method of the present invention) were compared with Example 1, and performance tests and comparisons were performed on all samples.

[0069] Comparative Example 1-1 (no pre-dispersion treatment of polymer microspheres):

[0070] This embodiment provides a high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure and a preparation method thereof, and the material composition is as follows:

[0071]

[0072]

[0073] The preparation method of the high damping oil-resistant rubber vibration-damping material with a closed-cell foam structure in this comparative example comprises the following specific steps, and the preparation steps of the surface organic modification of the lamellar filler are as follows:

[0074] (1) The surface modifier is placed in a mixture of ethanol and water, wherein the volume ratio of ethanol to water is 1:0.1, and the volume concentration of the surface modifier in the alcohol-water mixture is controlled at 5%. The prepared modifier dispersion is stirred and hydrolyzed at 30° C. for 10 hours.

[0075] (2) The prepared modifier is dispersed and sprayed evenly on the surface of the lamellar filler, and the mass ratio of the modifier to the filler is 5%. The treated filler is then heat-treated in an oven at 50° C. for 5 minutes to finally obtain a lamellar filler with surface modification.

[0076] The steps for preparing rubber blends are as follows:

[0077] (1) Add 100 g of rubber matrix into a rubber internal mixer, followed by zinc oxide, stearic acid, antioxidant 4010NA, and then 10 g of polymer microspheres, and mix at 60°C for 5 minutes; then add carbon black N330, organic modified graphene, and butyl benzyl phthalate, and mix at 100°C for 2 minutes; after the rubber materials are evenly mixed, discharge the mixed rubber and leave it for 48 hours.

[0078] (2) Put the rubber mix back into the rubber internal mixer, add sulfur, vulcanization accelerator DM, diisopropylbenzene peroxide, and TAIC in sequence, mix at 50°C for 3 minutes, and discharge the rubber after the rubber is evenly mixed and put it aside for use.

[0079] Comparative Example 1-2 (directly adding the interface modifier without using the filler modification method of the present invention)

[0080] This comparative example provides a high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure and a preparation method thereof, and the material composition is as follows:

[0081]

[0082]

[0083] The method for preparing a high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure in this comparative example comprises the following specific steps, and the steps for preparing a polymer microsphere pre-dispersed masterbatch are as follows:

[0084] (1) Preparation of polymer microsphere dispersion: 10 g of polymer microspheres were dispersed in deionized water, and then sodium dodecylbenzene sulfonate was added to the dispersion, wherein the mass ratio of polymer microspheres, sodium dodecylbenzene sulfonate, and deionized water was 1:10:200. The mixture was emulsified and mixed in a high shear homogenizer, wherein the emulsification speed was 1000 rpm, the emulsification temperature was 60° C., and the emulsification time was 10 minutes, and finally a polymer microsphere dispersion with stable dispersion was obtained.

[0085] (2) Preparation of polymer microsphere pre-dispersed masterbatch: The polymer microsphere dispersion liquid is mixed with rubber latex at a solid mass ratio of 1:5. The mixed liquid is placed in a stirring device for thorough mixing. The mixed liquid is then slowly added to a flocculation reactor and stirred thoroughly until flocculation is complete. The flocculent gel is washed and dried.

[0086] The steps for preparing rubber blends are as follows:

[0087] (1) Add 50g of rubber matrix into a rubber internal mixer, followed by zinc oxide, stearic acid, antioxidant 4010NA, and then 60g of polymer microsphere pre-dispersed masterbatch, and mix at 60°C for 5 minutes; then add carbon black N330, 5g of graphene, 5g of glycidyl ether-terminated long-chain polyether silane, and butyl benzyl phthalate, and mix at 100°C for 2 minutes; after the rubber materials are evenly mixed, discharge the mixed rubber and leave it for 48 hours.

[0088] (2) Put the rubber mix back into the rubber internal mixer, add sulfur, vulcanization accelerator DM, diisopropylbenzene peroxide, and TAIC in sequence, mix at 50°C for 3 minutes, and discharge the rubber after the rubber is evenly mixed and put it aside for use.

[0089] Example 2

[0090] This embodiment provides a high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure and a preparation method thereof, and the material composition is as follows:

[0091]

[0092] The method for preparing the high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure in this embodiment includes the following specific steps:

[0093] 1. Preparation steps of polymer microsphere pre-dispersed masterbatch:

[0094] (1) Preparation of polymer microsphere dispersion: A certain amount of polymer microspheres was dispersed in deionized water, and then a surfactant was added to the dispersion, wherein the mass ratio of polymer microspheres, surfactant, and deionized water was 1:20:1000. The mixture was emulsified and mixed in a high shear homogenizer at an emulsification speed of 5000 rpm, an emulsification temperature of 80°C, and an emulsification time of 60 minutes, and finally a polymer microsphere dispersion with stable dispersion was obtained.

[0095] (2) Preparation of polymer microsphere pre-dispersed masterbatch: The polymer microsphere dispersion liquid is mixed with rubber latex at a solid mass ratio of 1:6. The mixed liquid is placed in a stirring device for thorough mixing. The mixed liquid is then slowly added to a flocculation reactor and stirred thoroughly until flocculation is complete. The flocculent gel is washed and dried.

[0096] 2. Surface organic modification steps of lamellar fillers:

[0097] (1) Preparation of surface modifier: The surface modifier is placed in a mixture of ethanol and water, wherein the volume ratio of ethanol to water is 1:0.2, and the volume concentration of the surface modifier in the alcohol-water mixture is controlled at 10%. The prepared modifier dispersion is stirred and hydrolyzed at 40° C. for 10 hours.

[0098] (2) Surface modification of lamellar fillers: The prepared modifier is dispersed and sprayed evenly on the surface of the lamellar filler, and then the treated filler is heat-treated at 120° C. in an oven for 20 minutes to finally obtain a lamellar filler with a surface modified surface.

[0099] 3. Preparation steps of rubber blending compound:

[0100] (1) Preliminary mixing: Add the rubber matrix into a rubber internal mixer, followed by zinc oxide, stearic acid, antioxidant, and then add the foaming agent pre-dispersed masterbatch, and mix at 60°C for 3 minutes; then add the spherical filler, organic modified lamellar filler, and plasticizer, and mix at 80°C for 4 minutes; after the rubber materials are evenly mixed, discharge the mixed rubber and leave it for 24 hours.

[0101] (2) Final mixing: Put the rubber mix back into the rubber internal mixer, add sulfur, vulcanization accelerator, peroxide vulcanizing agent, and co-vulcanizing agent in sequence, mix at 80°C for 2 minutes, and after the rubber is evenly mixed, discharge the rubber and put it aside for use.

[0102] Example 3

[0103] This embodiment provides a high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure and a preparation method thereof, and the material composition is as follows:

[0104]

[0105]

[0106] The method for preparing the high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure in this embodiment includes the following specific steps:

[0107] 1. Preparation steps of polymer microsphere pre-dispersed masterbatch:

[0108] (1) Preparation of polymer microsphere dispersion: A certain amount of polymer microspheres was dispersed in deionized water, and then a surfactant was added to the dispersion, wherein the mass ratio of polymer microspheres, surfactant, and deionized water was 1:20:1000. The mixture was emulsified and mixed in a high shear homogenizer at an emulsification speed of 5000 rpm, an emulsification temperature of 80°C, and an emulsification time of 60 minutes, and finally a polymer microsphere dispersion with stable dispersion was obtained.

[0109] (2) Preparation of polymer microsphere pre-dispersed masterbatch: The polymer microsphere dispersion liquid is mixed with rubber latex at a solid mass ratio of 1:6. The mixed liquid is placed in a stirring device for thorough mixing. The mixed liquid is then slowly added to a flocculation reactor and stirred thoroughly until flocculation is complete. The flocculent gel is washed and dried.

[0110] 2. Surface organic modification steps of lamellar fillers:

[0111] (1) Preparation of surface modifier: The surface modifier is placed in a mixture of ethanol and water, wherein the volume ratio of ethanol to water is 1:0.2, and the volume concentration of the surface modifier in the alcohol-water mixture is controlled at 10%. The prepared modifier dispersion is stirred and hydrolyzed at 40° C. for 10 hours.

[0112] (2) Surface modification of lamellar fillers: The prepared modifier is dispersed and sprayed evenly on the surface of the lamellar filler, and then the treated filler is heat-treated at 120° C. in an oven for 20 minutes to finally obtain a lamellar filler with a surface modified surface.

[0113] 3. Preparation steps of rubber blending compound:

[0114] (1) Preliminary mixing: Add the rubber matrix into a rubber internal mixer, followed by zinc oxide, stearic acid, antioxidant, and then add the foaming agent pre-dispersed masterbatch, and mix at 60°C for 3 minutes; then add the spherical filler, organic modified lamellar filler, and plasticizer, and mix at 80°C for 4 minutes; after the rubber materials are evenly mixed, discharge the mixed rubber and leave it for 24 hours.

[0115] (2) Final mixing: Put the rubber mix back into the rubber internal mixer, add sulfur, vulcanization accelerator, peroxide vulcanizing agent, and co-vulcanizing agent in sequence, mix at 80°C for 2 minutes, and after the rubber is evenly mixed, discharge the rubber and put it aside for use.

[0116] Example 4

[0117] This embodiment provides a high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure and a preparation method thereof, and the material composition is as follows:

[0118]

[0119] The method for preparing the high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure in this embodiment includes the following specific steps:

[0120] 1. Preparation steps of polymer microsphere pre-dispersed masterbatch:

[0121] (1) Preparation of polymer microsphere dispersion: A certain amount of polymer microspheres was dispersed in deionized water, and then a surfactant was added to the dispersion, wherein the mass ratio of polymer microspheres, surfactant, and deionized water was 1:20:1000. The mixture was emulsified and mixed in a high shear homogenizer at an emulsification speed of 5000 rpm, an emulsification temperature of 80°C, and an emulsification time of 60 minutes, and finally a polymer microsphere dispersion with stable dispersion was obtained.

[0122] (2) Preparation of polymer microsphere pre-dispersed masterbatch: The polymer microsphere dispersion liquid is mixed with rubber latex at a solid mass ratio of 1:6. The mixed liquid is placed in a stirring device for thorough mixing. The mixed liquid is then slowly added to a flocculation reactor and stirred thoroughly until flocculation is complete. The flocculent gel is washed and dried.

[0123] 2. Surface organic modification steps of lamellar fillers:

[0124] (1) Preparation of surface modifier: The surface modifier is placed in a mixture of ethanol and water, wherein the volume ratio of ethanol to water is 1:0.2, and the volume concentration of the surface modifier in the alcohol-water mixture is controlled at 10%. The prepared modifier dispersion is stirred and hydrolyzed at 40° C. for 10 hours.

[0125] (2) Surface modification of lamellar fillers: The prepared modifier is dispersed and sprayed evenly on the surface of the lamellar filler, and then the treated filler is heat-treated at 120° C. in an oven for 20 minutes to finally obtain a lamellar filler with a surface modified surface.

[0126] 3. Preparation steps of rubber blending compound:

[0127] (1) Preliminary mixing: Add the rubber matrix into a rubber internal mixer, followed by zinc oxide, stearic acid, antioxidant, and then add the foaming agent pre-dispersed masterbatch, and mix at 60°C for 3 minutes; then add the spherical filler, organic modified lamellar filler, and plasticizer, and mix at 80°C for 4 minutes; after the rubber materials are evenly mixed, discharge the mixed rubber and leave it for 24 hours.

[0128] (2) Final mixing: Put the rubber mix back into the rubber internal mixer, add sulfur, vulcanization accelerator, peroxide vulcanizing agent, and co-vulcanizing agent in sequence, mix at 80°C for 2 minutes, and after the rubber is evenly mixed, discharge the rubber and put it aside for use.

[0129] Example 5

[0130] This embodiment provides a high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure and a preparation method thereof, and the material composition is as follows:

[0131]

[0132]

[0133] The method for preparing the high damping oil-resistant rubber vibration reduction material with a closed-cell foam structure in this embodiment includes the following specific steps:

[0134] 1. Preparation steps of polymer microsphere pre-dispersed masterbatch:

[0135] (1) Preparation of polymer microsphere dispersion: A certain amount of polymer microspheres was dispersed in deionized water, and then a surfactant was added to the dispersion, wherein the mass ratio of polymer microspheres, surfactant, and deionized water was 1:20:1000. The mixture was emulsified and mixed in a high shear homogenizer at an emulsification speed of 5000 rpm, an emulsification temperature of 80°C, and an emulsification time of 60 minutes, and finally a polymer microsphere dispersion with stable dispersion was obtained.

[0136] (2) Preparation of polymer microsphere pre-dispersed masterbatch: The polymer microsphere dispersion liquid is mixed with rubber latex at a solid mass ratio of 1:6. The mixed liquid is placed in a stirring device for thorough mixing. The mixed liquid is then slowly added to a flocculation reactor and stirred thoroughly until flocculation is complete. The flocculent gel is washed and dried.

[0137] 2. Surface organic modification steps of lamellar fillers:

[0138] (1) Preparation of surface modifier: The surface modifier is placed in a mixture of ethanol and water, wherein the volume ratio of ethanol to water is 1:0.2, and the volume concentration of the surface modifier in the alcohol-water mixture is controlled at 10%. The prepared modifier dispersion is stirred and hydrolyzed at 40° C. for 10 hours.

[0139] (2) Surface modification of lamellar fillers: The prepared modifier is dispersed and sprayed evenly on the surface of the lamellar filler, and then the treated filler is heat-treated at 120° C. in an oven for 20 minutes to finally obtain a lamellar filler with a surface modified surface.

[0140] 3. Preparation steps of rubber blending compound:

[0141] (1) Preliminary mixing: Add the rubber matrix into a rubber internal mixer, followed by zinc oxide, stearic acid, antioxidant, and then add the foaming agent pre-dispersed masterbatch, and mix at 60°C for 3 minutes; then add the spherical filler, organic modified lamellar filler, and plasticizer, and mix at 80°C for 4 minutes; after the rubber materials are evenly mixed, discharge the mixed rubber and leave it for 24 hours.

[0142] (2) Final mixing: Put the rubber mix back into the rubber internal mixer, add sulfur, vulcanization accelerator, peroxide vulcanizing agent, and co-vulcanizing agent in sequence, mix at 80°C for 2 minutes, and after the rubber is evenly mixed, discharge the rubber and put it aside for use.

[0143] The performance comparison of the samples in the comparative example and the embodiment is shown in Table 1 below.

[0144] Table 1 Comparison of material properties in the examples and comparative examples

[0145]

[0146] As can be seen from Table 1, when the results of Example 1 are compared with those of Comparative Example 1-1, it is found that when the polymer microspheres are not pre-dispersed, the damping performance of the rubber material prepared is significantly lower than that of Example 1. This indicates that pre-dispersing the polymer microspheres can improve their dispersibility in the rubber matrix, thereby significantly improving the damping performance of the material as well as improving the mechanical strength and oil resistance of the material.

[0147] Comparison of the results of Example 1 with Comparative Examples 1-2 shows that the modification method of the filler has an important influence on the performance of the rubber material. The modified filler has better dispersion performance in the rubber matrix, and the modified filler can give the rubber material excellent damping performance, mechanical properties and oil resistance.

[0148] Further, by analyzing the results of Example 2, Example 3, Example 4 and Example 5, it can be seen that:

[0149] Example 2 has the highest tensile strength and elongation at break, indicating that its mechanical properties are the best. At the same time, its damping factor and volume change after oil immersion are also good, indicating that the material has high stability in high temperature and oil immersion environments.

[0150] The tensile strength and elongation at break of Example 3 are slightly lower than those of Example 2, but the hardness change after oil immersion is small, indicating that the dimensional stability in the oil immersion environment is good.

[0151] The damping factor of Example 4 is the highest, indicating that it has the best vibration reduction performance. At the same time, its volume change after oil immersion is the smallest, indicating that the material has the best stability in the oil-invaded environment.

[0152] The performance indicators of Example 5 are balanced, showing good comprehensive performance. Its tensile strength, elongation at break, damping factor, hardness change and volume change after oil immersion all show good results.

[0153] In summary, by comparing the results of different embodiments and comparative examples, the following conclusions can be drawn:

[0154] The pre-dispersion treatment of polymer microspheres significantly improves the damping and mechanical properties of rubber materials.

[0155] The organic modification of fillers significantly improves the dispersibility and comprehensive properties of rubber materials.

[0156] Different formulations and processing methods in each embodiment have a significant impact on the mechanical properties, damping properties and oil resistance of the material. In specific applications, the optimal formulation and processing method can be selected according to actual needs.

[0157] The above description is only a preferred embodiment of the present invention, so all equivalent changes or modifications made according to the structure, characteristics and principles described in the scope of the patent application of the present invention are included in the scope of the patent application of the present invention.

Claims

1. A rubber vibration damping material with a closed-cell foam structure, characterized in that: Its material composition is as follows: Rubber matrix: 100 parts by mass; Spherical filler: 30-60 parts by mass; Lamellar filler: 1 to 10 parts by mass; Surface modifier: 1 to 10 parts by mass; Plasticizer: 5-20 parts by weight; Antiaging agent: 2 to 6 parts by weight; Polymer microsphere pre-dispersed masterbatch: 2-10 parts by weight; Sulfur: 1 to 5 parts by mass; Zinc oxide: 1 to 5 parts by mass; Stearic acid: 1 to 5 parts by mass; Vulcanization accelerator: 0.5-5 parts by mass; Peroxide curing agent: 1 to 5 parts by mass; Vulcanizing agent: 1 to 5 parts by weight.

2. The rubber vibration damping material according to claim 1, characterized in that: The rubber matrix is ​​one or more of nitrile rubber, hydrogenated nitrile rubber and chloroprene rubber.

3. The rubber vibration damping material according to claim 1, characterized in that: The spherical filler is one or more of carbon black, white carbon black, zinc oxide and aluminum oxide.

4. The rubber vibration damping material according to claim 1, characterized in that: The lamellar filler is one or more of graphene, graphene oxide, kaolin and hydrotalcite.

5. The rubber vibration damping material according to claim 1, characterized in that: The surface modifier is one or more of a glycidyl ether-terminated long-chain polyether silane coupling agent, dodecyl trimethoxy silane, and hexadecyl trimethoxy silane.

6. The rubber vibration damping material according to claim 1, characterized in that: The plasticizer is one or more of liquid nitrile rubber, butyl benzyl phthalate, tricresyl phosphate and dinonyl phthalate.

7. The rubber vibration damping material according to claim 1, characterized in that: The antioxidant is one or more of antioxidant RD, antioxidant D, antioxidant NBC, antioxidant 4010NA and antioxidant BLE.

8. The rubber vibration damping material according to claim 1, characterized in that: The foaming agent is expandable polymer microspheres with a particle size of 1 to 100 μm.

9. The rubber vibration damping material according to claim 1, characterized in that: The vulcanization accelerator is one or more of accelerator CZ, accelerator DM, accelerator TT, accelerator NS and accelerator ZDC.

10. The rubber vibration damping material according to claim 1, characterized in that: The peroxide curing agent is one or more of diisopropylbenzene peroxide, 2,5-dimethyl-2,5-(di-tert-butylperoxy)hexane and diacyl peroxide.

11. The rubber vibration damping material according to claim 1, characterized in that: The vulcanizing agent is one or more of the vulcanizing agent TAIC, the vulcanizing agent HVA-2 and the vulcanizing agent TMPT.

12. A method for preparing the rubber vibration damping material according to any one of claims 1 to 11, characterized in that The steps include: preparing a polymer microsphere pre-dispersed masterbatch; Organic modification of the surface of the lamellar filler; Preparation of rubber blends.

13. The method for preparing the rubber vibration damping material according to claim 12, characterized in that: The steps of preparing the polymer microsphere pre-dispersed masterbatch are as follows: (1) dispersing a certain amount of polymer microspheres in deionized water, then adding a surfactant to the dispersion, wherein the mass ratio of polymer microspheres, surfactant, and deionized water is 1:(1-20):(50-1000), and emulsifying and mixing the mixture in a high shear homogenizer, wherein the emulsification speed is 1000-12000 rpm, the emulsification temperature is 30-80° C., and the emulsification time is 5-60 minutes to obtain a polymer microsphere dispersion; (2) Mixing the polymer microsphere dispersion with the rubber latex in a solid mass ratio of 1:(5-20), placing the mixture in a stirring device for mixing, and then slowly adding the mixture into a flocculation reactor, stirring sufficiently until flocculation is complete, and washing and drying the flocculent gel.

14. The method for preparing the rubber vibration damping material according to claim 12, characterized in that: The steps of organically modifying the surface of the flaky filler are as follows: (1) placing a surface modifier in a mixture of ethanol and water, wherein the volume ratio of ethanol to water is 1:(0.1-0.5), and the volume concentration range of the surface modifier in the alcohol-water mixture is 1-10%, and stirring and hydrolyzing the prepared modifier dispersion at 20-40° C. for 10 hours; (2) The prepared modifier is dispersed and sprayed evenly on the surface of the lamellar filler, and then the treated filler is heat-treated in an oven at 100-150° C. for 5-30 minutes to finally obtain a lamellar filler with surface modification.

15. The method for preparing the rubber vibration damping material according to claim 12, characterized in that: The steps of preparing the rubber blend are as follows: (1) Adding a rubber matrix into a rubber internal mixer, followed by adding zinc oxide, stearic acid, and an antioxidant, and then adding a foaming agent to pre-disperse the masterbatch, and mixing at 50° C. to 80° C. for 2 to 5 minutes; then adding a spherical filler, an organic modified lamellar filler, and a plasticizer, and mixing at 50° C. to 100° C. for 2 to 5 minutes; after the rubber materials are evenly mixed, discharging the mixed rubber and leaving it for 24 to 48 hours; (2) Put the rubber mix back into the rubber internal mixer, add sulfur, vulcanization accelerator, peroxide vulcanizing agent, and co-vulcanizing agent in sequence, mix at 40-80°C for 2-5 minutes, and after the rubber is evenly mixed, discharge the rubber and put it aside for use.

Citation Information

Cited By

  • Composition, vulcanizate, and vulcanized molded article

    JP7698742B2

  • Composition, vulcanizate, and vulcanized molded body

    JPWO2023136318A1