Irradiation crosslinking low-smoke halogen-free low-toxicity insulation material for B1-level flame-retardant twisted-pair electric wire and preparation method thereof
By using a flame-retardant system of magnesium hydroxide, antimony trioxide, and melamine cyanurate with a particle size of 0.5μm in B1-grade flame-retardant twisted-pair cloth wire, combined with EVA resin and other additives, the problem of insufficient flame-retardant performance in the prior art has been solved, and multiple performance improvements of the insulation material have been achieved, making it suitable for wires and cables.
Patent Information
- Application Number
- CN202411248206.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-06
AI Technical Summary
Existing B1-grade flame-retardant twisted-pair cloth wires, under certain process conditions and flame-retardant systems, are difficult to achieve low flammability ratings, flammable dripping levels, and flammable heat release. They are also difficult to achieve good processing performance, self-extinguishing performance, and insulation performance.
Magnesium hydroxide with a d50 particle size of 0.5 μm was used as the sole hydroxide flame retardant component, combined with antimony trioxide and melamine cyanurate as flame retardant synergists. By limiting the dosage and combination, a new flame retardant system was formed. EVA resin, EVM rubber, ethylene propylene rubber, light stabilizer and antioxidant were added to the insulation material to optimize the composition and preparation process of the insulation material.
This invention achieves good processing performance, self-extinguishing performance, and insulation performance of the insulating material while having a low flammability rating, low burning droplet rating, and low heat release during combustion. It is suitable for use in wires and cables and meets the B1 flame retardant requirements.
Smart Images

Figure BDA0005031479190000051 
Figure BDA0005031479190000061 
Figure BDA0005031479190000071
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of insulating materials, and more specifically, to a radiation cross-linked low-smoke, halogen-free, and low-toxic insulating material for B1-level flame-retardant twisted-pair wiring and a preparation method thereof. Background Art
[0002] With the development of society, fire safety issues are receiving increasing attention. When a fire occurs, wires and cables may become a path for the fire to spread, and their flammable insulation or sheath materials may cause the fire accident to expand, burn the power supply and lines of fire-fighting equipment, affect the normal operation of fire-fighting electrical equipment, delay the fire-fighting time, and easily cause casualties and property losses. In addition, the heat, toxic gases and thick smoke emitted by the insulation and sheath materials of wires and cables when they burn can also cause further damage to life and property.
[0003] The flame-retardant cables commonly used in my country before were manufactured in accordance with the technical standards of GB / T 19666-2005 General Rules for Flame-retardant and Fire-resistant Cables. The standard for judging the flame-retardant grade of wires and cables is GB / T 18380-2008, which evaluates the combustion grade of wires and cables by the carbonization height after combustion. In order to make fire safety more scientific and reasonable and reduce the possible fire hazards to the minimum, my country issued the mandatory national standard GB 31247-2014 "Classification of Combustion Performance of Cables and Optical Cables" on December 5, 2014. This standard puts forward higher requirements for the performance of flame-retardant cables by quantifying the technical indicators of the classification of the combustion performance of cables and optical cables. In this context, the development and use of B1-level flame-retardant cables has become an inevitable trend to improve the flame-retardant performance of wires and cables, reduce heat release and smoke production when a fire occurs, reduce the level of burning drops / particles, smoke toxicity and corrosiveness, etc., and ensure the safety of life and property of personnel.
[0004] B1 flame retardant twisted pair wire has a special structure, usually wrapped with mica tape outside the five types of soft conductors, and then extruded with insulating materials on the outside of the mica tape by extrusion tube production method, and finally irradiated and cross-linked. At present, the flame retardant system of B1 cable materials on the market generally uses metal hydroxide as a flame retardant, and nano carbonizing agent as a flame retardant synergist.
[0005] Regarding the above-mentioned related technologies, the inventors believe that the special structure of B1-class flame-retardant twisted pair cloth wire is not conducive to achieving flame retardancy, and radiation cross-linking will also affect the insulating properties of the insulating material. The flame retardant system composed of metal hydroxide and nano-carbon-forming agent is actually not suitable for use in B1-class flame-retardant twisted pair cloth wire. This makes it difficult for B1-class flame-retardant twisted pair cloth wire to have a low combustion level, combustion dripping level and combustion heat release under the existing process conditions and flame retardant system, and it is also difficult to have good processing performance, self-extinguishing performance and insulation performance. Summary of the invention
[0006] In the related art, it is difficult for B1-level flame-retardant twisted-pair wires to have a low combustion level, combustion dripping level, and combustion heat release under existing process conditions and flame-retardant systems, and it is also difficult to have good processing performance, self-extinguishing performance, and insulation performance. In order to improve this defect, the present application provides a radiation cross-linked low-smoke, halogen-free, and low-toxic insulating material for B1-level flame-retardant twisted-pair wires and a preparation method thereof.
[0007] In the first aspect, the present application provides a radiation cross-linked low-smoke, halogen-free, and low-toxic insulating material for B1-level flame-retardant twisted-pair wiring, which adopts the following technical solution: A radiation cross-linked low-smoke, halogen-free and low-toxic insulating material for B1-level flame-retardant twisted-pair wiring, comprising the following components in parts by weight: 80-100 parts of a base material composition, 180-220 parts of magnesium hydroxide, 20-50 parts of antimony trioxide, 9.5-10.5 parts of melamine cyanurate, and 9-10 parts of an auxiliary agent, wherein the auxiliary agent comprises a silane coupling agent, an antioxidant, a cross-linking sensitizer, a lubricant and a light stabilizer, the components of the base material composition comprise an EVA resin and a compatibilizer, the magnesium hydroxide has a d 50 The particle size is 0.5-1μm.
[0008] By adopting the above technical solution, the present invention designs a new flame retardant system in combination with the characteristics of B1 flame retardant twisted pair wires, and selects d 50 Magnesium hydroxide with a particle size of 0.5 μm is used as the only hydroxide flame retardant component, and the dosage range of magnesium hydroxide is limited. According to the dosage specified in this application, magnesium hydroxide can fully promote the combustion and crusting of the insulating material when the insulating material does not contain a nano-carbon-forming agent. The combustion and crusting effect is significantly better than the case of adding aluminum hydroxide or a magnesium-aluminum composite flame retardant system, and a carbon layer with a high degree of integrity can be obtained after combustion. This application also selects antimony trioxide and melamine cyanurate as flame retardant synergists. Antimony trioxide isolates air and combustible gases through a condensed phase flame retardant mechanism when the insulating material burns, while melamine cyanurate dilutes combustible gases and oxygen through a gas phase flame retardant mechanism. In addition, the promotion of magnesium hydroxide on combustion and crusting can fully improve the self-extinguishing performance of the insulating material. On this basis, by limiting the amount of antimony trioxide and melamine cyanurate, the insulating material of the present application can ensure that the corrosive level and smoke toxicity index meet the standards while meeting the self-extinguishing performance standards, overcoming the high price, high specific gravity, and large addition amount of antimony trioxide and the defects of the gas released by the combustion of melamine cyanurate affecting the material toxicity index. For the above reasons, the insulating material of the present application not only has a lower combustion level, combustion dripping level, and combustion heat release, but also has better processing performance, self-extinguishing performance, and insulation performance, and is more suitable for use in wires and cables than B1-level cable materials on the market.
[0009] Preferably, the amount of the EVA resin used accounts for 40-87.5% of the total weight of the base material composition.
[0010] By adopting the above technical scheme, the present application optimizes the dosage of EVA resin. The insulating material prepared within the above range has good compatibility with the flame retardant system of the present application, can have a lower combustion level, combustion dripping level and combustion heat release, and has good self-extinguishing performance.
[0011] Preferably, the compatibilizer is EVA grafted with maleic anhydride.
[0012] By adopting the above technical scheme, the present application selects EVA grafted maleic anhydride as a compatibilizer when determining the base material composition, which can improve the compatibility of the base material composition with the inorganic component, is beneficial to the uniform dispersion of magnesium hydroxide and antimony trioxide, and helps to improve the flame retardant properties of the insulating material.
[0013] Preferably, the base material composition further comprises EVM rubber and ethylene-propylene rubber.
[0014] By adopting the above technical scheme, on the basis of selecting EVA resin, the addition of EVM rubber and EPDM rubber can make the mechanical properties of the material qualified with a certain margin, and on the other hand, EVM rubber and EPDM rubber are easier to be radiation cross-linked than EVA resin, so a more ideal cross-linking degree can be obtained under lower radiation dose conditions.
[0015] Preferably, the light stabilizer includes hindered amine light stabilizer and benzotriazole light stabilizer.
[0016] By adopting the above technical solution, the hindered amine light stabilizer mainly reduces the damage to the insulating material caused by radiation by capturing the free radicals generated by the photooxidation reaction, while the benzotriazole light stabilizer mainly reduces the damage to the insulating material caused by radiation by absorbing ultraviolet rays. The insulating material of the present application can be cross-linked under conditions of lower radiation doses, and the synergistic combination of the two light stabilizers can reduce the impact of radiation on the flame retardant properties and mechanical properties of the insulating material.
[0017] Preferably, the light stabilizer consists of light stabilizer 944 and light stabilizer 326.
[0018] By adopting the above technical scheme, the present application preferably selects specific types of hindered amine light stabilizers and benzotriazole light stabilizers, among which light stabilizer 326 not only has a certain antioxidant property itself, but also has a synergistic effect when used with an antioxidant, which can fully reduce the thermal oxidative degradation of the insulating material during the processing.
[0019] Preferably, the antioxidant comprises hindered phenol antioxidant and phosphite antioxidant.
[0020] Preferably, the antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and tris(2,4-di-tert-butylphenyl) phosphite.
[0021] By adopting the above technical solution, the present application further optimizes the composition of the antioxidants. The above two antioxidants, in combination with the light stabilizer 326, can effectively reduce the thermal oxidation degradation of the insulating material during processing, and help reduce the loss of mechanical properties of the insulating material during processing.
[0022] Preferably, the lubricant comprises silicone powder, polyethylene wax and zinc stearate.
[0023] By adopting the above technical solution, the silicone powder, polyethylene wax and zinc stearate can be used together to give the insulating material good lubricity, which helps to reduce the friction of the insulating material during the processing, and can effectively reduce energy consumption and improve production efficiency.
[0024] In a second aspect, the present application provides a method for preparing a radiation cross-linked low-smoke, halogen-free and low-toxic insulating material for B1-level flame-retardant twisted pair wiring, using the following technical solution.
[0025] A method for preparing a radiation cross-linked low-smoke, halogen-free, and low-toxic insulating material for B1-level flame-retardant twisted-pair wires, comprising the following steps: (1) accurately weighing the base material composition, magnesium hydroxide, antimony trioxide, melamine cyanurate and additives according to the formula and setting them aside; (2) placing weighed magnesium hydroxide, antimony trioxide, melamine cyanurate and the silane coupling agent in the auxiliary agent in a high-speed mixer and stirring to obtain a flame retardant composite; (3) preparing an antioxidant, a light stabilizer, a lubricant and a part of the base material composition through a banbury mixer, granulating with a single screw, and then air cooling to obtain an additive masterbatch; (4) The flame retardant compound, the auxiliary agent masterbatch, the cross-linking sensitizer and the remaining base material composition are sent to a reciprocating machine for mixing, and then subjected to single-screw extrusion granulation and cooling to obtain a radiation cross-linked low-smoke, halogen-free and low-toxic insulating material for B1-level flame retardant twisted pair wire.
[0026] By adopting the above technical scheme, after weighing each raw material component, the present application first uses a silane coupling agent to treat magnesium hydroxide, antimony trioxide and melamine cyanurate, which helps to reduce the agglomeration of these flame retardant components and improves the dispersion effect of the flame retardant components, and helps to obtain a B1-level flame retardant twisted pair wire with a radiation cross-linked low-smoke, halogen-free and low-toxic insulation material having a low combustion grade, combustion dripping grade and combustion heat release, and good processing performance, self-extinguishing performance and insulation performance.
[0027] In summary, this application has the following beneficial effects: 1. The insulating material of the present application not only has a lower combustion level, combustion dripping level and combustion heat release, but also has better processing performance, self-extinguishing performance and insulation performance. Compared with the B1 grade cable material on the market, it is more suitable for use in power facilities.
[0028] 2. The present application optimizes the composition of the base material composition. On the basis of selecting EVA resin, the addition of EVM rubber and EPDM rubber can make the mechanical properties of the material qualified with a certain margin. On the other hand, EVM rubber and EPDM rubber are easier to be radiation cross-linked than EVA resin, so a more ideal degree of cross-linking can be obtained under lower radiation dose conditions.
[0029] 3. Since the insulating material of the present application can be cross-linked under conditions of relatively low radiation doses, coupled with the synergistic combination of hindered amine light stabilizers and benzotriazole light stabilizers, the effect of radiation on the flame retardant properties and mechanical properties of the insulating material can be fully reduced. DETAILED DESCRIPTION
[0030] The present application is further described in detail below in conjunction with examples and comparative examples. The raw materials involved in the present application can all be obtained commercially. Example
[0031] Examples 1-5 The following description is given by taking Example 1 as an example.
[0032] Example 1 This embodiment provides a B1-level flame-retardant twisted-pair wire irradiation cross-linked low-smoke halogen-free low-toxicity insulation material, including the following components by weight: 100 kg of base material composition, 200 kg of magnesium hydroxide, 30 kg of antimony trioxide, 10 kg of melamine cyanurate, and 9 kg of additives. The model of magnesium hydroxide is PSF-150, provided by Shendao Chemical, d 50 The particle size is 0.5μm.
[0033] Among the above components, the base material composition is composed of 50kg of EVA resin, 20kg of EVM rubber, 20kg of ethylene propylene rubber and 10kg of compatibilizer, and the compatibilizer is EVA grafted maleic anhydride. The auxiliary agent is composed of 2kg of silane coupling agent, 1kg of antioxidant, 1kg of cross-linking sensitizer, 1kg of light stabilizer, and 4kg of lubricant, wherein the lubricant is composed of 1kg of silicone powder, 2kg of polyethylene wax and 1kg of zinc stearate; the silane coupling agent is composed of silane coupling agent A172 and silane coupling agent S230 mixed in a weight ratio of 1:1; the antioxidant is composed of antioxidant 1010 and antioxidant 168 mixed in a weight ratio of 1:1; the light stabilizer is composed of light stabilizer 944 and light stabilizer 326 mixed in a weight ratio of 1:1.
[0034] This embodiment provides a method for preparing a radiation cross-linked low-smoke, halogen-free, and low-toxic insulating material for a Class B1 flame-retardant twisted pair wiring harness, comprising the following steps: (1) accurately weighing the base material composition, magnesium hydroxide, antimony trioxide, melamine cyanurate and auxiliary agent according to the formula and setting them aside; (2) placing weighed magnesium hydroxide, antimony trioxide, melamine cyanurate and the silane coupling agent in the auxiliary agent in a high-speed mixer and stirring to obtain a flame retardant composite; (3) the antioxidant, the light stabilizer, the lubricant and the base material composition accounting for 1 / 10 of the total weight of the base material composition are subjected to internal mixing, single-screw granulation, and then air-cooling to obtain an additive masterbatch; (4) The flame retardant compound, the auxiliary agent masterbatch, the cross-linking sensitizer and the remaining base material composition are sent to a reciprocating machine for mixing, and then subjected to single-screw extrusion granulation and cooling to obtain a radiation cross-linked low-smoke, halogen-free and low-toxic insulating material for B1-level flame retardant twisted pair wire.
[0035] As shown in Table 1, the difference between Examples 1-5 is mainly in the different raw material ratios. The magnesium hydroxide d 50 The particle size is 0.7 μm, and the magnesium hydroxide of Example 4-5 is 50 The particle size is 1.0μm.
[0036] Table 1 Raw material ratio and source of insulating materials Comparative Example Comparative Example 1 The difference between this comparative example and Example 1 is that magnesium hydroxide (PSF-150, Shendao Chemical, d 50 0.5 μm) was replaced by magnesium hydroxide (H-5, Albemarle, USA, d 50 The particle size is 1.5 μm).
[0037] Comparative Example 2 The difference between this comparative example and Example 1 is that magnesium hydroxide (PSF-150, Shendao Chemical, d 50 0.5 μm) was replaced by aluminum hydroxide (107LEO, Albemarle, USA, d 50 The particle size is 1.5 μm).
[0038] Comparative Example 3 The difference between this comparative example and Example 1 is that antimony trioxide and melamine cyanurate are removed on the basis of Example 1.
[0039] Comparative Example 4 The difference between this comparative example and Example 1 is that, on the basis of Example 1, the amount of antimony trioxide is adjusted to 20 kg, and the amount of melamine cyanurate is adjusted to 20 kg.
[0040] Comparative Example 5 The difference between this comparative example and Example 1 is that, on the basis of Example 1, the amount of magnesium hydroxide is adjusted to 190 kg, and the light stabilizer is removed.
[0041] Comparative Example 6 The difference between this comparative example and Example 1 is that, on the basis of Example 1, the compatibilizer is changed from EVA grafted maleic anhydride to PE grafted maleic anhydride (grafting rate 1.2%).
[0042] Performance testing methods With reference to relevant standards such as GB 31247-2014 Classification of Combustion Performance of Electric Cables and Optical Cables and GB / T 31248-2014 Test Method for Flame Spread, Heat Release and Smoke Generation Characteristics of Electric Cables or Optical Cables under Fire Conditions, the insulating materials of each embodiment and comparative example were processed into samples and irradiated and cross-linked at a dose of 100 kGy. In addition, on the basis of Example 1, irradiation and cross-linking were performed at a dose of 150 kGy, and this group was recorded as the control group. Then, the performance tests were performed on the samples of Examples 1-5, Comparative Examples 1-6 and the control group, and the results are shown in Tables 2 and 3.
[0043] Table 2 Test data of the embodiment Table 3 Test data of comparative example and control group Combining Examples 1-5 and Comparative Examples 1-5 and Tables 2 and 3, it can be seen that the insulating materials of Examples 1-5 have lower combustion levels, combustion dripping levels and combustion heat release, and have better processing performance, self-extinguishing performance and insulation performance, and the overall performance is better than the insulating materials of Comparative Examples 1-5. In Examples 1-5, the examples to which EVM rubber and EPDM rubber are added have lower carbonization height, maximum heat release rate and total heat release than the examples to which the two are not added, indicating that the addition of EVM rubber and EPDM rubber helps to further improve the flame retardant properties of the insulating material.
[0044] Combining Example 1 and Comparative Example 1 and combining Table 2 and Table 3, it can be seen that when the d 50When the particle size does not meet the conditions specified in this application, although the passing rate of the single vertical combustion test and the combustion grade of the 2*2.5 twisted pair wire do not change significantly, the carbonization height, maximum heat release rate, and total heat release all increase significantly, indicating that d 50 Magnesium hydroxide with a particle size of 1.5μm is not sufficient to fully improve the flame retardant properties of the insulating material.
[0045] Combining Example 1 and Comparative Example 2 and Table 2 and Table 3, it can be seen that the combustion level, carbonization height, maximum heat release rate and total heat release of the 2*2.5 twisted pair measured in Comparative Example 2 have all increased significantly, and the dripping level has also been improved to d1, indicating that aluminum hydroxide is not sufficient to fully improve the flame retardant properties of the insulating material and cannot make the insulating material meet the B1 flame retardant requirements.
[0046] Combining Example 1 and Comparative Example 3 and Tables 2 and 3, it can be seen that the single vertical combustion test pass rate measured in Comparative Example 3 is significantly lower than that in Example 1, and the carbonization height, maximum heat release rate, total heat release, and dripping level are significantly increased, indicating that in the absence of antimony trioxide and melamine cyanurate as flame retardant synergists, the flame retardant properties and self-extinguishing properties of the insulating material are less than ideal.
[0047] Combining Example 1 and Comparative Example 4 with Tables 2 and 3, it can be seen that the carbonization height, maximum heat release rate, total heat release, dripping level, and combustion gas conductivity measured in Comparative Example 4 all showed a significant increase, indicating that when antimony trioxide and melamine cyanurate are not added according to the formula dosage of this application, the improvement of the flame retardant performance of the insulating material is limited, and the insulating material no longer meets the B1 flame retardant requirements. Moreover, since the dosage of melamine cyanurate is doubled, and the dosage of antimony trioxide is reduced by 1 / 3 (relative to Example 1), the toxicity index has increased significantly, and it is difficult to meet the standard of low-toxic wires.
[0048] Combining Example 1 and Comparative Example 5 and Table 2 and Table 3, it can be seen that the single vertical combustion test pass rate of Comparative Example 5 has a slight decrease, and the carbonization height, maximum heat release rate, total heat release and dripping level have all increased significantly, indicating that reducing the amount of magnesium hydroxide and removing the light stabilizer is not conducive to fully improving the flame retardant properties of the insulating material, and also has a certain impact on the self-extinguishing performance.
[0049] Combining Example 1 and Comparative Example 6 with Tables 2 and 3, it can be seen that the tensile fracture strain of Comparative Example 6 is significantly lower than that of Example 1, and the carbonization height, maximum heat release rate and total heat release are all higher than those of Example 1. It can be seen that the flame retardant properties and some mechanical properties of the insulating material of Comparative Example 6 are poor. It also shows that EVA grafted maleic anhydride is more helpful to improve the mechanical properties and flame retardant properties of the insulating material when used as a compatibilizer.
[0050] Combining Example 1 and the control group and Tables 2 and 3, it can be seen that the tensile fracture strain of the control group is significantly lower than that of Example 1, and the carbonization height, maximum heat release rate and total heat release are significantly higher than those of Example 1, and the drip level also rises to d1. It can be seen that the flame retardant properties and some mechanical properties of the insulating material of the control group are poor, which also shows that a lower irradiation dose is helpful to obtain an insulating material with better mechanical properties and flame retardant properties.
[0051] The above embodiments are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments of the present application without any creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A radiation cross-linked low-smoke, halogen-free, low-toxic insulating material for B1-level flame-retardant twisted-pair wire, characterized in that: The invention comprises the following components in parts by weight: 80-100 parts of a base material composition, 180-220 parts of magnesium hydroxide, 20-50 parts of antimony trioxide, 9.5-10.5 parts of melamine cyanurate, and 9-10 parts of an auxiliary agent, wherein the auxiliary agent comprises a silane coupling agent, an antioxidant, a cross-linking sensitizer, a lubricant, and a light stabilizer. The components of the base material composition comprise an EVA resin and a compatibilizer. The magnesium hydroxide has a d 50 The particle size is 0.5-1μm.
2. The radiation cross-linked low-smoke, halogen-free, and low-toxic insulating material for B1-level flame-retardant twisted-pair wiring according to claim 1 is characterized in that: The amount of the EVA resin used accounts for 40-87.5% of the total weight of the base material composition.
3. The radiation cross-linked low-smoke, zero-halogen, low-toxic insulating material for B1-level flame-retardant twisted-pair wiring according to claim 2, characterized in that: The compatibilizer is EVA grafted with maleic anhydride.
4. The radiation cross-linked low-smoke, zero-halogen, low-toxic insulating material for B1-level flame-retardant twisted-pair wiring according to claim 2, characterized in that: The base material composition also includes EVM rubber and ethylene-propylene rubber.
5. The radiation cross-linked low-smoke, zero-halogen, low-toxic insulating material for B1-level flame-retardant twisted-pair wiring according to claim 4, characterized in that: The light stabilizer includes hindered amine light stabilizer and benzotriazole light stabilizer.
6. The radiation cross-linked low-smoke, zero-halogen, low-toxic insulating material for B1-level flame-retardant twisted-pair wiring according to claim 5, characterized in that: The light stabilizer consists of light stabilizer 944 and light stabilizer 326.
7. The radiation cross-linked low-smoke, zero-halogen, low-toxic insulating material for B1-level flame-retardant twisted-pair wiring according to claim 6, characterized in that: The antioxidants include hindered phenol antioxidants and phosphite antioxidants.
8. The radiation cross-linked low-smoke, zero-halogen, low-toxic insulating material for B1-level flame-retardant twisted-pair wiring according to claim 7, characterized in that: The antioxidants are pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate] and tris(2,4-di-tert-butylphenyl) phosphite.
9. The radiation cross-linked low-smoke, zero-halogen, low-toxic insulating material for B1-level flame-retardant twisted-pair wiring according to claim 1, characterized in that: The lubricant includes silicone powder, polyethylene wax and zinc stearate.
10. The method for preparing the radiation cross-linked low-smoke, halogen-free and low-toxic insulating material for B1-level flame-retardant twisted pair wiring according to any one of claims 1 to 9, characterized in that: The following steps are involved: (1) Accurately weigh the base material composition, magnesium hydroxide, antimony trioxide, melamine cyanurate and additives according to the formula and set aside; (2) Put the weighed magnesium hydroxide, antimony trioxide, melamine cyanurate and the silane coupling agent in the auxiliary agent in a high-speed mixer and stir them to obtain a flame retardant composite; (3) preparing an antioxidant, a light stabilizer, a lubricant and a part of the base material composition through a banbury mixer, granulating with a single screw, and then air cooling to obtain an additive masterbatch; (4) The flame retardant compound, the auxiliary agent masterbatch, the cross-linking sensitizer and the remaining base material composition are sent to a reciprocating machine for mixing, and then subjected to single-screw extrusion granulation and cooling to obtain a radiation cross-linked low-smoke, halogen-free and low-toxic insulation material for B1-level flame retardant twisted pair wire.
Citation Information
Patent Citations
Irradiation crosslinking halogen-free high flame-retardant cable material and preparation method thereof
CN101914236A
Long-life irradiation-crosslinking low-smoke halogen-free high-flame-retarding polyolefin cable material and preparation method thereof
CN109553846A
Long-life silane-crosslinking low-smoke halogen-free high-flame-retarding polyolefin cable material and preparation method thereof
CN109553847A
B1-grade flame-retardant irradiation crosslinking low-smoke halogen-free insulated cable material and preparation method thereof
CN109627567A
105DEG C B1-level irradiation cross-linked halogen-free low-smoke flame-retardant polyolefin elastomer insulation material and preparation method thereof
CN110776690A