High-strength ultraviolet curing organic silicon rubber and preparation method thereof
By combining specific silicone oil and silicone rubber to reinforce the crosslinking network, combined with the three-stage curing process, the problem of low strength of silicone rubber is solved, significantly improving its mechanical properties and stability.
Patent Information
- Application Number
- CN202411301407.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-29
AI Technical Summary
The existing silicone rubber has low strength during the preparation process, making it difficult to maintain stability in harsh environments, and is prone to damage.
The preparation method of high-strength ultraviolet cured silicone rubber is adopted to form cross-sectional cross-sectional by combining end-hydroxy modified silicone oil, end-alkoxy modified silicone oil, silicone rubber reinforcement prepolymer and acryloyloxy modified MQ silicone resin. Connect the network and adopt a three-stage curing process to improve mechanical performance.
The tensile strength, elongation and hardness of silicone rubber are significantly improved, and its stability and mechanical properties are enhanced in harsh environments.
Smart Images

Figure BDA0005047772400000091 
Figure BDA0005047772400000101 
Figure BDA0005047772400000111
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rubber production and processing, and in particular relates to a high-strength ultraviolet-cured organic silicon rubber and a preparation method thereof. Background Art
[0002] In recent years, electronic devices such as smartphones, LCDs, and automotive components have been pursuing not only higher performance, but also space saving and energy saving. Therefore, in response to such social demands, electronic devices are becoming increasingly miniaturized and detailed, and their assembly processes are becoming more complicated year by year, and silicone rubber is often used.
[0003] Silicone rubber is also called organosiloxane or silicone rubber. The main chain of the molecule is Si-O bond, and it is a linear high molecular polymer with monovalent organic groups as side groups. The bond energy of Si-O bond is much higher than that of CC bond, and the molecular chain is flexible, so it has excellent high and low temperature resistance. The operating temperature is -70-300℃. At the same time, it has excellent electrical insulation performance and is non-toxic to human tissue. It is suitable for high temperature resistant seals, insulating parts, profiles, hose diaphragms and medical and sanitary products for air systems.
[0004] At present, the silicone rubber on the market is mostly prepared directly by mixing rubber raw materials with adhesives during the preparation process, which results in low strength of traditional silicone rubber. It is easy to be damaged when used for a long time or in harsh environments. Summary of the invention
[0005] The invention provides a high-strength ultraviolet-cured organic silicon rubber and a preparation method thereof, which are used to solve the technical problem that the existing organic silicon rubber has low strength.
[0006] In view of this, the present invention provides a high-strength UV-curable silicone rubber, which includes a first component and a second component, wherein the first component includes the following raw materials in parts by weight: 5-20 parts of terminal hydroxyl-modified silicone oil, 5-20 parts of terminal alkoxy-modified silicone oil, 20-60 parts of terminal acryloxy silicone oil, 20-60 parts of silicone rubber reinforcing prepolymer, 1-10 parts of acryloxy-modified MQ silicone resin, and 3-11 parts of white carbon black;
[0007] The second component comprises the following raw materials in parts by weight: 3-8 parts of polyamino organic silicon compound, 3-12 parts of strong active diluent, 3-12 parts of weak active diluent, 0.5-5 parts of moisture curing catalyst, and 0.5-5 parts of photosensitive initiator.
[0008] Optionally, the terminal hydroxyl modified silicone oil is prepared by the following method:
[0009] A1: Mix three substances, namely, a dialkoxysiloxane containing epoxy functional groups, a dialkoxysiloxane containing a carbon-carbon double bond structure, and a siloxane rich in hydroxyl or alkoxy groups, add water, mix evenly, heat to raise the temperature, add an alkaline catalyst, mix evenly, and hydrolyze under normal pressure and in a closed environment to obtain a pre-hydrolyzate of a terminal hydroxyl-modified silicone oil;
[0010] A2: Add hydroxyl-rich siloxane to the prehydrolyzate of terminal hydroxyl-modified silicone oil, continue heating and heating, reduce pressure, react, terminate the reaction, vacuum degas, cool, and obtain terminal hydroxyl-modified silicone oil.
[0011] Furthermore, the terminal hydroxyl modified silicone oil is prepared by the following method:
[0012] A1: Put epoxy functional group-containing dialkoxysiloxane (commonly used: γ-(2,3-epoxypropoxy)propylmethyldimethoxysilane, γ-(2,3-epoxypropoxy)propylmethyldiethoxysilane), carbon-carbon double bond structure-containing dialkoxysiloxane (commonly used: methacryloxypropylmethyldimethoxysilane, methacryloxypropylmethyldiethoxysilane), hydroxyl- or alkoxy-rich siloxane (commonly used: silicone hydrolyzate, linear body, dimethyldimethoxysilane, dimethyldiethoxysilane) into water, mix well, heat to 50-80°C, add alkaline catalyst (commonly used tetramethylammonium hydroxide, potassium hydroxide, etc.), mix well, hydrolyze at normal pressure and closed for 0.5-2h, and obtain the pre-hydrolyzate of terminal hydroxyl modified silicone oil;
[0013] A2: Add hydroxyl-rich siloxane to the pre-hydrolyzate of terminal hydroxyl-modified silicone oil, supplement the siloxane segment according to the epoxy content and olefin content requirements, continue heating to 100-120°C, reduce the pressure to -0.08-0.1MPa, react for 2-6h, terminate the reaction (when the alkaline catalyst is tetramethylammonium hydroxide, heat to about 130°C, when the alkaline catalyst is potassium hydroxide, add phosphoric acid for neutralization), vacuum degassing, cool to 22±3°C, and obtain terminal hydroxyl-modified silicone oil;
[0014] Among them, the terminal hydroxyl modified silicone oil has three characteristics:
[0015] Feature 1: The modified functional groups in the terminal hydroxyl modified silicone oil include epoxy functional groups and olefin functional groups. The number of acryloxy functional groups in a single terminal hydroxyl modified silicone oil molecule is more than 2 on average.
[0016] Feature 2: The epoxy functional group is an epoxy-terminated organic group, generally an epoxy polyether group, the most commonly used of which is γ-(2,3-epoxypropoxy)propyl.
[0017] Feature 3: The functional group has an olefin structure. The functional group is an organic group having an olefin structure, and generally an organic group having an acryloyloxy end-capping is used, and methacryloyloxypropyl is the most commonly used.
[0018] In this embodiment, the dialkoxysiloxane containing epoxy functional groups is selected from γ-(2,3-epoxypropoxy)propylmethyldimethoxysilane, the dialkoxysiloxane containing carbon-carbon double bond structure is selected from methacryloxypropylmethyldimethoxysilane, the siloxane rich in alkoxy groups is selected from dimethyldimethoxysilane, and the siloxane rich in hydroxy groups is selected from organic silicon hydrolyzate; the ratio of the molar number of pure water to the molar number of alkoxy groups in the mixture is 1:2;
[0019] The molar ratio of γ-(2,3-epoxypropoxy)propylmethyldimethoxysilane and methacryloxypropylmethyldimethoxysilane is 0.1-20:2, the molar number of the segment of the organosilicon hydrolyzate is calculated based on the molecular weight of the dimethylsiloxy chain segment of 74, the dimethyldimethoxysilane and the organosilicon hydrolyzate can be replaced with each other in equal moles, the ratio of the total molar number of dimethyldimethoxysilane and the organosilicon hydrolyzate to the total molar number of the former two is 0.5-20:1, the added amount of water is 50% of the total molar number of the mixture of γ-(2,3-epoxypropoxy)propylmethyldimethoxysilane, methacryloxypropylmethyldimethoxysilane and dimethyldimethoxysilane, the alkaline catalyst is tetramethylammonium hydroxide, and the added amount of the alkaline catalyst is 5-100 millionths of the total mass of the materials.
[0020] Optionally, the terminal alkoxy-modified silicone oil is prepared by the following method:
[0021] B1: Dialkoxysiloxane, dialkoxysiloxane containing a carbon-carbon double bond structure, and hydroxyl-rich siloxane are mixed, water is added, the mixture is uniformly mixed, the mixture is heated, an alkaline catalyst is added, the mixture is uniformly mixed, and hydrolysis is performed under normal pressure and in a closed environment to obtain a prehydrolyzate of terminal hydroxyl-modified silicone oil;
[0022] B2: Add siloxane ring to the pre-hydrolyzate of terminal hydroxyl modified silicone oil, continue heating and heating, reduce pressure, react, terminate the reaction, vacuum degas, cool and obtain terminal alkoxy modified silicone oil.
[0023] Furthermore, the terminal alkoxy modified silicone oil is prepared by the following method:
[0024] B1: Mix dialkoxysiloxane (commonly used: dimethyldimethoxysilane, dimethyldiethoxysilane), dialkoxysiloxane containing carbon-carbon double bond structure (commonly used: methacryloxypropylmethyldimethoxysilane, methacryloxypropylmethyldiethoxysilane), hydroxyl-rich siloxane (optional component, commonly used: silicone hydrolyzate, linear body) and other substances, add water, mix evenly, heat to 50-80°C, add alkaline catalyst (commonly used tetramethylammonium hydroxide, potassium hydroxide, etc.), mix evenly, hydrolyze at normal pressure and closed for 0.5-2h, and obtain the pre-hydrolyzate of terminal alkoxy modified silicone oil;
[0025] B2: Add siloxane ring body (commonly used: octamethylcyclotetrasiloxane, dimethylsiloxane mixed ring body) to the pre-hydrolyzate of terminal alkoxy modified silicone oil, supplement the siloxane segment according to the target viscosity requirement, continue heating (heat to about 110°C when the alkaline catalyst is tetramethylammonium hydroxide, and heat to about 150°C when the alkaline catalyst is potassium hydroxide), reduce the pressure to -0.02-0.1MPa, react for 2-6h, terminate the reaction (heat to about 130°C when the alkaline catalyst is tetramethylammonium hydroxide, and add phosphoric acid to neutralize when the alkaline catalyst is potassium hydroxide), vacuum degassing, and cooling to 22±3°C to obtain terminal alkoxy modified silicone oil;
[0026] Among them, terminal alkoxy modified silicone oil has three characteristics:
[0027] Feature 1: The modified functional groups in the terminal alkoxy modified silicone oil include functional groups with alkoxy groups and functional groups with olefin structures. The average number of acryloyloxy functional groups in a single alkoxy modified silicone oil molecule is more than 2.
[0028] Feature 2: Alkoxy groups generally use methoxy and ethoxy groups. Methoxy groups are used in highly active formulas, and ethoxy groups are used in environmentally friendly formulas.
[0029] Feature 3: The functional group has an olefin structure. The functional group is an organic group having an olefin structure, and generally an organic group having an acryloyloxy end-capping is used, and methacryloyloxypropyl is the most commonly used.
[0030] In this embodiment, the dialkoxysiloxane is dimethyldimethoxysilane, the dialkoxysiloxane containing a carbon-carbon double bond structure is methacryloxypropylmethyldimethoxysilane, and the siloxane ring body is octamethylcyclotetrasiloxane;
[0031] The molar ratio of dimethyldimethoxysilane and methacryloxypropylmethyldimethoxysilane is 0.5-20:1, the added amount of water is 50% of the total molar number of the first two, the added amount of octamethylcyclotetrasiloxane is 0.5-20:1 to the total molar number of the first two, the added amount of the alkaline catalyst is 5-100 parts per million of the total mass of the materials, and the alkaline catalyst is tetramethylammonium hydroxide.
[0032] Optionally, the silicone rubber reinforcement prepolymer is prepared by the following method: hydroxyl-terminated siloxane, MQ resin and white carbon black are uniformly mixed, heated, reduced pressure, reacted, and cooled to obtain the silicone rubber reinforcement prepolymer.
[0033] Furthermore, the silicone rubber reinforcement prepolymer is prepared by the following method: hydroxyl-terminated siloxane (usually with a viscosity of 500-50000mm 2 / s, commonly used 1000, 5000, 10000, 20000mm 2 / s four specifications), MQ resin (MQ ratio is 0.5-1.4:1), white carbon black, mix in a certain proportion according to needs, heat to 180-220°C, slightly negative pressure or normal pressure (-0.02-0.1MPa), continue to react for 2-6h, cool to 22±3°C, and obtain silicone rubber reinforcement prepolymer;
[0034] The silicone rubber reinforced prepolymer is a high molecular weight siloxane mixture reinforced with MQ resin and white carbon black and rich in silanol groups, and the high molecular weight siloxane mixture rich in silanol groups is selected from high viscosity hydroxyl-terminated siloxane;
[0035] The weight ratio of hydroxyl-terminated siloxane, MQ resin and white carbon black is 80-95:0-12:2-8.
[0036] Among them, the viscosity of hydroxyl-terminated siloxane is between 500-50000mm 2 / s, preferably high viscosity, most preferably 1000, 5000, 10000 or 20000mm 2 / s; the total mass ratio of MQ resin and white carbon black is between 5-15%. In low viscosity formula, the MQ ratio is high and the white carbon black ratio is low, and the two are between 2:1-1:1; in high viscosity formula, the opposite is true, and the two are between 1:1-0:1.
[0037] Optionally, the acryloxy-modified MQ silicone resin is prepared by the following method: hydrogen-containing MQ resin, organic matter containing acryloxy and olefin groups, and solvent oil are evenly mixed, heated, a platinum catalyst is added, reacted, and after the reaction is completed, vacuum degassing and cooling are performed to obtain acryloxy-modified MQ resin.
[0038] Furthermore, the acryloxy-modified MQ resin is prepared by the following method: hydrogen-containing MQ resin, organic matter containing acryloxy and olefin groups, and solvent oil are uniformly mixed, heated to 60-90° C., a platinum catalyst is added, and the reaction is performed for 2-4 hours. After the reaction is completed, vacuum degassing is performed, and the temperature is cooled to 22±3° C. to obtain the acryloxy-modified MQ resin;
[0039] Among them, the terminal acryloyloxy group generally adopts an organic group having an acryloyloxy end-capping group, and the most commonly used is methacryloyloxypropyl;
[0040] The organic matter containing acryloxy and olefin groups is allyl methacrylate, the solvent oil is 120 solvent oil, the molar number of Si-H groups in the hydrogenated MQ resin and the molar number of allyl methacrylate are in a ratio of 0.8-1.2:0.8-1.2, the amount of solvent oil added is 10-200 percent of the total weight of the first two, the amount of platinum catalyst added is 1-100 millionths of the total mass of the materials, and the platinum catalyst is a Castel catalyst.
[0041] Optionally, the highly reactive diluent generally adopts a small organosilicon molecule with a highly reactive olefin structure, preferably a methacryloxypropyl silane coupling agent, and the weakly reactive diluent generally adopts a small organosilicon molecule with a low reactive olefin structure, preferably a vinyl silane coupling agent.
[0042] Optionally, the moisture curing catalyst is one or more of organic tin, organic bismuth, and titanate.
[0043] Optionally, the photoinitiator is an aryl alkyl ketone photoinitiator.
[0044] Furthermore, the photoinitiator is an aryl alkyl ketone photoinitiator, which can be selected from one or more of the free radical photoinitiators TPO, TPO-L, 1173, 184, 907, and 369.
[0045] A method for preparing high-strength ultraviolet-cured silicone rubber comprises the following steps:
[0046] S1: Preparation of the first component: Evenly mix terminal hydroxyl-modified silicone oil, terminal alkoxy-modified silicone oil, terminal acryloxy-modified silicone oil, and silicone rubber reinforcing prepolymer, add acryloxy-modified MQ resin and white carbon black, mix evenly, reduce pressure, perform heat treatment, cool, and then package into a light-shielding, airtight container to obtain the first component;
[0047] S2: Preparation of the second component: uniformly mix the polyamino organic silicon compound, the strong active diluent, the weak active diluent, the moisture curing catalyst, and the photosensitive initiator, and package them into a light-shielding, airtight container to obtain the second component;
[0048] S3: Mix the first component and the second component, heat to increase the temperature, reduce the pressure, and degas to obtain the silicone rubber.
[0049] Furthermore, a method for preparing high-strength UV-curable silicone rubber comprises the following steps:
[0050] S1: Preparation of the first component: Evenly mix the terminal hydroxyl modified silicone oil, the terminal alkoxy modified silicone oil, the terminal acryloxy silicone oil and the silicone rubber reinforcing prepolymer, add the acryloxy modified MQ resin and the white carbon black, mix evenly, reduce the pressure to -0.06-normal pressure, heat treat at a temperature of 40-150°C for 1-3h, cool to 22±3°C, and package in a light-shielding, airtight container to obtain the first component; when the first component of the rubber compound has high viscosity and poor fluidity, an appropriate amount of strong active diluent and weak active diluent may be added, but it should not exceed 5 parts;
[0051] S2: Preparation of the second component: uniformly mix the polyamino organic silicon compound, the strong active diluent, the weak active diluent, the moisture curing catalyst, and the photosensitive initiator, and package them into a light-shielding, airtight container to obtain the second component;
[0052] S3: Mix the first component and the second component, heat to 40-60°C, reduce the pressure to vacuum -0.03-(-0.1)MPa, and degas for 5-30 minutes to obtain the silicone rubber.
[0053] A method for using high-strength ultraviolet-cured silicone rubber comprises the following steps:
[0054] When in use, the silicone rubber is applied by brushing, mold casting, etc. After the surface is leveled, it is cured by ultraviolet light for the first stage, then left to stand for the second stage of curing, and finally the third stage of curing is carried out under a certain humidity.
[0055] Furthermore, a method for using high-strength UV-curable silicone rubber comprises the following steps:
[0056] When in use, the silicone rubber is applied by brushing, mold casting, etc. After the surface is leveled, it is cured by ultraviolet light for 5-120s, and then amino epoxy is cured in the second stage at room temperature for 24h or heated for 2-4h. The physical and chemical properties meet the conditions for product sale and transportation. It is then cured in the third stage at room temperature for 7d and 50% humidity, and the indicators are improved to the values required by customers.
[0057] It can be seen from the above technical solutions that the embodiments of the present invention have the following advantages:
[0058] 1. The present invention adopts terminal hydroxyl-modified silicone oil and terminal alkoxy-modified silicone oil, which can react with the hydrosilylation in other components to form a cross-linked network, thereby improving the strength of the silicone rubber; the silicone rubber reinforcing prepolymer includes white carbon black, and the raw material of the first component also includes white carbon black, which can form a physical or chemical interaction with the silicone rubber matrix and has good dispersibility, and can increase the contact area with the silicone rubber molecules, thereby further enhancing the mechanical properties of the silicone rubber.
[0059] 2. The present invention adopts a three-stage curing process, which can not only utilize the rapid response characteristics of light curing to improve production efficiency, but also utilize the subsequent two-stage curing to improve the physical and chemical indicators to a higher level; the three curing mechanisms can all be cured at room temperature, which is convenient for customers to construct; the three curing mechanisms and curing rates have obvious gradients, which can avoid the competitive reactions of different curing mechanisms to form internal stress, resulting in a decrease in physical and chemical indicators, and form a good synergistic effect.
[0060] 3. The present invention adopts a combination of strong active diluent and weak active diluent, which can balance the reaction rate of different formulas and the spatial stress of light curing, improve the flexibility of formula adjustment, and enhance the adaptability of the formula to different customer needs; it also adopts high-temperature pretreated silicone rubber reinforced prepolymer to avoid the problems of low bond strength and poor physical and chemical properties of conventional room temperature curing rubber. DETAILED DESCRIPTION
[0061] In order to make the technical scheme of the present invention better understood by the personnel of the technical field, the technical scheme in the embodiment of the present invention is clearly and completely described below. Obviously, the described embodiment is only a part of the embodiment of the present invention, rather than all the embodiments. Based on the embodiment in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or can be prepared by existing methods.
[0062] The terminal acryloxy silicone oil generally adopts an organic group with an acryloxy end-capping, and the most commonly used is methacryloyloxypropyl; the amino group in the polyamino silicone compound generally adopts an amino-terminated silicone group with a primary amine or / and secondary amine structure, and the commonly used ones are aminopropyl and N-(2-aminoethyl)-3-aminopropyl; the amino value is as high as possible (5-12mmol / g) and the viscosity is as low as possible (30-200mm 2 / s); highly active diluents generally use small silicone molecules with highly reactive olefin structures, and the most commonly used one is methacryloyloxypropyl silane coupling agent; weakly active diluents generally use small silicone molecules with low reactive olefin structures, and the most commonly used one is vinyl silane coupling agent; moisture curing catalysts are organic tin, organic bismuth or titanate, and the most commonly used one is organic tin, and the environmentally friendly and safe option is organic bismuth; photoinitiators are highly active free radical mechanism photoinitiators, and the most commonly used ones are TPO and TPO-L.
[0063] The polyamino organic silicon compound in the present application is N-(2-aminoethyl)-3-aminopropyl; the moisture curing catalyst is organic bismuth; and the photosensitive initiator is TPO.
[0064] Preparation Example
[0065] Preparation Example 1
[0066] A hydroxyl-terminated silicone oil is prepared by the following method:
[0067] A1: 440 kg of γ-(2,3-epoxypropoxy)propylmethyldimethoxysilane, 432 kg of methacryloxypropylmethyldimethoxysilane and 240 kg of dimethyldimethoxysilane were put into 54 kg of water, mixed evenly, heated to 65 ° C, added with 15 g of tetramethylammonium hydroxide, mixed evenly, and hydrolyzed under normal pressure and closed conditions for 1.2 hours to obtain a pre-hydrolyzate of terminal hydroxyl modified silicone oil;
[0068] A2: Add 296 kg of silicone hydrolyzate to the pre-hydrolyzate, continue heating to 110°C, reduce the pressure to -0.09 MPs, react for 3.5 hours, increase the temperature to 130°C, vacuum degas, cool to 25°C, and obtain terminal hydroxyl modified silicone oil.
[0069] Preparation Example 2
[0070] A terminal alkoxy modified silicone oil is prepared by the following method:
[0071] B1: 120 kg of dimethyldimethoxysilane and 216 kg of methacryloxypropylmethyldimethoxysilane were put into 54 kg of water, mixed evenly, heated to 65 ° C, added with 13 g of tetramethylammonium hydroxide, mixed evenly, and hydrolyzed under normal pressure and closed conditions for 1.2 hours to obtain a pre-hydrolyzate of terminal alkoxy modified silicone oil;
[0072] B2: Add 444 kg of octamethylcyclotetrasiloxane to the pre-hydrolyzate, continue heating to 110°C, reduce the pressure to -0.01 MPa, react for 3.5 hours, increase the temperature to 130°C, vacuum degas, cool to 25°C, and obtain terminal alkoxy modified silicone oil.
[0073] Preparation Example 3
[0074] A silicone rubber reinforced prepolymer is prepared by the following method:
[0075] 880 kg of hydroxyl-terminated siloxane, 80 kg of MQ resin and 40 kg of white carbon black were mixed evenly, heated to 200° C., reduced pressure to 0.05 MPa, reacted for 4 hours, and cooled to 25° C. to obtain a silicone rubber reinforced prepolymer.
[0076] Preparation Example 4
[0077] An acryloxy-modified MQ resin is prepared by the following method:
[0078] 450 kg of 0.3% hydrogen-containing MQ resin, 224 kg of allyl methacrylate and 437 kg of solvent oil were mixed evenly, heated to 80°C, 4 g of platinum catalyst was added, and the reaction was carried out for 3 hours. After the reaction was completed, the mixture was vacuum-evaporated and cooled to 25°C to obtain acryloxy-modified MQ resin.
[0079] Example
[0080] Example 1
[0081] A high-strength ultraviolet curing silicone rubber, the raw material ratio of which is shown in Table 1.
[0082] A method for preparing high-strength ultraviolet-cured silicone rubber comprises the following steps:
[0083] S1: Preparation of the first component: The terminal hydroxyl-modified silicone oil prepared in Preparation Example 1, the terminal alkoxy-modified silicone oil prepared in Preparation Example 2, the terminal acryloxy silicone oil, and the silicone rubber reinforcing prepolymer prepared in Preparation Example 3 are mixed evenly, and the acryloxy-modified MQ resin and white carbon black prepared in Preparation Example 4 are added, mixed evenly, reduced pressure to -0.08 MPa, heat treated at 100° C. for 2 h, cooled to 25° C., and packaged in a light-shielding, sealed container to obtain the first component;
[0084] S2: Preparation of the second component: uniformly mix the polyamino organic silicon compound, the strong active diluent, the weak active diluent, the moisture curing catalyst, and the photosensitive initiator, and package them into a light-shielding, airtight container to obtain the second component;
[0085] S3: Mix the first component and the second component, heat to 50°C, reduce the pressure to -0.02MPa, and degas for 18 minutes to obtain silicone rubber.
[0086] Example 2-11
[0087] A high-strength UV-curable silicone rubber, which is different from Example 1 in that the raw material ratio of the silicone rubber is different. The raw material ratio is shown in Table 1.
[0088] Table 1 Weight of each raw material of silicone rubber (kg)
[0089]
[0090]
[0091] Comparative Example
[0092] Comparative Example 1
[0093] A high-strength UV-curable silicone rubber, which is different from Example 1 in that the silicone rubber has a different source, and the silicone rubber in Comparative Example 1 is commercially available silicone rubber.
[0094] Performance testing
[0095] The organic silicone rubber in Example 1-11 and Comparative Example 1-2 was constructed by brushing, mold casting, etc. After the surface was leveled, ultraviolet light was used for 60 seconds for one-stage curing, and then it was left to stand for 24 hours, and then amino epoxy was cured for two stages. Finally, three stages of curing were carried out at a humidity of 50% for 7 days, and the following performance tests were performed:
[0096] Tensile strength: The tensile strength of silicone rubber was measured in accordance with GB / T528-1998 “Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber”. The test results are shown in Table 2.
[0097] Elongation at break: The elongation at break of silicone rubber was measured in accordance with GB / T528-1998 “Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber”. The test results are shown in Table 2.
[0098] Hardness: The hardness of silicone rubber was measured in accordance with GB / T2411-2008 "Determination of indentation hardness (Shore hardness) of plastics and hard rubber using a hardness tester". The test results are shown in Table 2.
[0099] Table 2 Test results
[0100]
[0101] As can be seen from Table 2, the high-strength UV-cured silicone rubber of the present application improves the mechanical properties of the silicone rubber, such as tensile strength, elongation at break, and hardness, through the interaction between the raw materials. Among them, the tensile strength is 4.5-6.0 MPa, the elongation at break is 576-600%, and the Shore hardness is 24-30A.
[0102] Combining Example 1 and Comparative Example 1, it can be seen that the tensile strength of the silicone rubber in Example 1 is 4.5 MPa, the elongation at break is 576%, and the Shore hardness is 24A, which are significantly better than Comparative Example 1, indicating that the silicone rubber of the present application has more excellent mechanical properties. The present application adopts terminal hydroxyl-modified silicone oil, terminal alkoxy-modified silicone oil, silicone rubber reinforcing prepolymer, white carbon black, etc., which can form physical or chemical interactions with the silicone rubber matrix, and also have good dispersibility, and can increase the contact area with the silicone rubber molecules, thereby further enhancing the mechanical properties of the silicone rubber and improving the tensile strength and elongation at break of the silicone rubber.
[0103] It can be seen from Examples 1-3 that the tensile strength of the silicone rubber in Example 2 is 5.2 MPa, the elongation at break is 580%, and the Shore hardness is 25A, which are better than other examples, indicating that the amount of the terminal hydroxyl-modified silicone oil added in Example 2 is more appropriate. In combination with Examples 2 and 4-5, it can be seen that the tensile strength of the silicone rubber in Example 4 is 5.6 MPa, the elongation at break is 585%, and the Shore hardness is 26A, which are better than other examples, indicating that the amount of the terminal alkoxy-modified silicone oil added in Example 3 is more appropriate; when the amount of the terminal hydroxyl-modified silicone oil and the terminal alkoxy-modified silicone oil added is too little, the effect is weak and the mechanical properties of the silicone rubber cannot be improved better. When the amount of the terminal hydroxyl-modified silicone oil and the terminal alkoxy-modified silicone oil added is too much, the viscosity of the silicone rubber will be increased, affecting the fluidity of the silicone rubber, thereby affecting the adhesion and stability.
[0104] Combining Example 4 and Example 6, it can be seen that the tensile strength of the silicone rubber in Example 6 is 5.8 MPa, the elongation at break is 587%, and the Shore hardness is 27A, which are better than those of other examples, indicating that the amount of silicone rubber reinforcing prepolymer added in Example 6 is more appropriate. The main function of the silicone rubber reinforcing prepolymer is to improve the strength and hardness of the silicone rubber. When the amount added is small, it does not play a better role and will affect the mechanical properties of the silicone rubber.
[0105] It can be seen from Examples 7-11 that, except for the terminal hydroxyl-modified silicone oil, the terminal alkoxy-modified silicone oil and the silicone rubber reinforcing prepolymer, the other components have little effect on the performance of the silicone rubber when they vary within a certain range.
[0106] As described above, the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A high-strength UV-curable silicone rubber, characterized in that: It comprises a first component and a second component, wherein the first component comprises the following raw materials in parts by weight: 5-20 parts of terminal hydroxyl-modified silicone oil, 5-20 parts of terminal alkoxy-modified silicone oil, 20-60 parts of terminal acryloxy silicone oil, 20-60 parts of silicone rubber reinforcing prepolymer, 1-10 parts of acryloxy-modified MQ silicone resin, and 3-11 parts of white carbon black; The second component comprises the following raw materials in parts by weight: 3-8 parts of polyamino organic silicon compound, 3-12 parts of strong active diluent, 3-12 parts of weak active diluent, 0.5-5 parts of moisture curing catalyst, and 0.5-5 parts of photosensitive initiator.
2. A high-strength UV-curable silicone rubber according to claim 1, characterized in that: The terminal hydroxyl modified silicone oil is prepared by the following method: A1: Mix three substances, namely, a dialkoxysiloxane containing epoxy functional groups, a dialkoxysiloxane containing a carbon-carbon double bond structure, and a siloxane rich in hydroxyl or alkoxy groups, add water, mix evenly, heat to raise the temperature, add an alkaline catalyst, mix evenly, and hydrolyze under normal pressure and in a closed environment to obtain a pre-hydrolyzate of a terminal hydroxyl-modified silicone oil; A2: Add hydroxyl-rich siloxane to the prehydrolyzate of terminal hydroxyl-modified silicone oil, continue heating and heating, reduce pressure, react, terminate the reaction, vacuum degas, cool, and obtain terminal hydroxyl-modified silicone oil.
3. The high-strength UV-curable silicone rubber according to claim 1, characterized in that: The terminal alkoxy modified silicone oil is prepared by the following method: B1: Dialkoxysiloxane, dialkoxysiloxane containing a carbon-carbon double bond structure, and hydroxyl-rich siloxane are mixed, water is added, mixed evenly, heated to a high temperature, an alkaline catalyst is added, mixed evenly, and hydrolyzed under normal pressure and in a closed environment to obtain a pre-hydrolyzate of terminal alkoxy-modified silicone oil; B2: Add siloxane ring body to the pre-hydrolyzate of terminal alkoxy modified silicone oil, continue heating and heating, reduce pressure, react, terminate the reaction, vacuum degas, cool and obtain terminal alkoxy modified silicone oil.
4. The high-strength UV-curable silicone rubber according to claim 1, characterized in that: The silicone rubber reinforcement prepolymer is prepared by the following method: hydroxyl-terminated siloxane, MQ resin and white carbon black are uniformly mixed, heated, reduced pressure, reacted, and cooled to obtain the silicone rubber reinforcement prepolymer.
5. The high-strength UV-curable silicone rubber according to claim 1, characterized in that: The acryloxy-modified MQ silicone resin is prepared by the following method: hydrogen-containing MQ resin, organic matter containing acryloxy groups and olefin groups, and solvent oil are uniformly mixed, heated, a platinum catalyst is added, reacted, and after the reaction is completed, vacuum degassing and cooling are performed to obtain the acryloxy-modified MQ resin.
6. The high-strength UV-curable silicone rubber according to claim 1, characterized in that: The strong active diluent is a methacryloxypropyl silane coupling agent, and the weak active diluent is a vinyl silane coupling agent.
7. The high-strength UV-curable silicone rubber according to claim 1, characterized in that: The moisture curing catalyst is one or more of organic tin, organic bismuth and titanate.
8. The high-strength UV-curable silicone rubber according to claim 1, characterized in that: The photoinitiator is an aryl alkyl ketone photoinitiator.
9. A method for preparing the high-strength UV-curable silicone rubber according to any one of claims 1 to 8, characterized in that: The steps include: S1: Preparation of the first component: Evenly mix terminal hydroxyl-modified silicone oil, terminal alkoxy-modified silicone oil, terminal acryloxy-modified silicone oil, and silicone rubber reinforcing prepolymer, add acryloxy-modified MQ resin and white carbon black, mix evenly, reduce pressure, perform heat treatment, cool, and then package into a light-shielding, airtight container to obtain the first component; S2: Preparation of the second component: uniformly mix the polyamino organic silicon compound, the strong active diluent, the weak active diluent, the moisture curing catalyst, and the photosensitive initiator, and package them into a light-shielding, airtight container to obtain the second component; S3: Mix the first component and the second component, heat to increase the temperature, reduce the pressure, and degas to obtain the silicone rubber.
10. The method for using the high-strength UV-curable silicone rubber according to claim 9, characterized in that: The method comprises the following steps: when in use, the silicone rubber is applied by brushing, mold casting, etc., after the surface is leveled, ultraviolet light is used for primary curing, and then the surface is allowed to stand for secondary curing, and finally the third stage of curing is carried out at a certain humidity.
Citation Information
Cited By
Light-cured pyrimidone-terminated silicone rubber material and preparation method thereof
CN122011784A
A photocurable terminal pyrimidinone-based silicone rubber material and a method for producing the same
CN122011784B