Pretreatment-free high-weather-resistance water-based paint for glass fiber composite material as well as preparation method and application thereof

By using high weathering water-resistant coatings on glass fiber composites, combining silane hydrolyzed oligomers and specific fillers, an organic-inorganic cross-linking network is formed, which solves the adhesion and weatherability of traditional coatings and achieves efficient and economical coatings The effect meets the long-term outdoor use needs of photovoltaic panel frames.

CN119039864AActive Publication Date: 2024-11-29NIPPON PAINT CHINA

Patent Information

Application Number
CN202311807248.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2024-11-29
Estimated Expiration
2043-12-26

AI Technical Summary

Technical Problem

Traditional water-based coatings are difficult to adhere to the surface of glass fiber reinforced composite materials, and the aromatic organic resin turns yellow after illumination, which cannot meet the weather resistance requirements of long-term outdoor use of photovoltaic panel frames. Pretreatment is required to increase production costs and reduce efficiency.

Method used

Using high weathering water-resistant coatings, the organic-inorganic hybrid crosslinking network structure is formed by introducing silane hydrolyzed oligomers and specific fillers, which enhances the adhesion and weatherability of the coating. The silane hydrolyzed oligomers are prepared by sol-gel method. , combined with aqueous acrylic resin and isocyanate curing agent, to form a two-component coating, suitable for unpretreated glass fiber reinforced composite materials.

Benefits of technology

It achieves excellent adhesion and good mechanical properties on the surface of glass fiber composite materials, meets weather resistance in different outdoor harsh conditions, reduces production costs, improves production efficiency, and the coating has hard toughness and ultraviolet resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
  • Figure SMS_6
    Figure SMS_6
Patent Text Reader

Abstract

The invention discloses a pretreatment-free high-weather-resistance water-based paint for a glass fiber composite material as well as a preparation method and application of the pretreatment-free high-weather-resistance water-based paint. The high-weather-resistance water-based paint is a double-component paint, and the first component is prepared from the following raw materials in parts by weight: 30 to 80 parts of water-based acrylic resin, 5 to 20 parts of silane hydrolysis oligomer, 2 to 10 parts of organic solvent, 2.1 to 30 parts of auxiliary agent, 5 to 25 parts of filler, 5 to 15 parts of nano color paste and 5 to 25 parts of deionized water; the second component comprises the following raw materials in parts by weight: 70-90 parts of an isocyanate curing agent and 10-30 parts of a solvent. According to the scheme, the problems that a structure (such as a photovoltaic frame) made of a glass fiber reinforced composite material needs to be subjected to pretreatment and can be well coated, and the coated structure is difficult to have good adhesive force and outdoor weather resistance in an extreme environment can be well solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water-based coatings for glass fiber composite materials, and more specifically to a highly weather-resistant water-based coating for glass fiber composite materials without pre-treatment, and a preparation method and application thereof. Background Art

[0002] With the implementation of policies, traditional high-energy consumption energy has been gradually replaced by green and sustainable new energy. In the field of materials, new glass fiber composite materials have excellent properties such as light weight, high strength, insulation, PID resistance, aging resistance, corrosion resistance, fire resistance, high and low temperature resistance, good designability, and low cost. This glass fiber composite substrate has high requirements for coating performance. It requires the coating to be able to resist damage and destruction to the surface of the substrate caused by various extreme weather (extreme heat and cold, wind and sand, etc.), and to meet the high weather resistance of long-term outdoor exposure.

[0003] Water-based paints are widely promoted and used in the fields of automobiles, wood products, construction, waterproofing, etc. because they use water as a solvent, can save a lot of petroleum resources, and have the characteristics of low VOC emissions and low air pollution. However, for special materials such as glass fiber reinforced composite materials (glass fiber composite materials), since this type of material is formed by pultrusion, there will be a lot of release agent left on its surface; and the profiles use a wide variety of resins and glass fibers, resulting in great differences in profile surface energy. Traditional water-based paints are difficult to adhere to their surfaces, so it is necessary to add substrate pre-treatment processes such as grinding, burning, and sandblasting, which increases production costs and reduces efficiency, which is very unfavorable to the development of the photovoltaic industry.

[0004] In addition, the mass-produced glass fiber reinforced composite frame is composed of about 70-80wt% glass fiber and 20-30wt% organic resin. The aromatic organic resin used will turn yellow after exposure to light, and the traditional water-based paint cannot meet the long-term outdoor use requirements of photovoltaic panel frame coating in terms of adhesion and outdoor weather resistance. Summary of the invention

[0005] Based on the above facts, the purpose of the present invention is to provide a highly weather-resistant water-based coating for glass fiber composite materials without pre-treatment, and a preparation method and application thereof, so as to solve the problem that some glass fiber reinforced composite material structures (such as photovoltaic frames, etc.) need to be pre-treated before they can be better painted, and the painted structures are difficult to have good adhesion and outdoor weather resistance in extreme environments.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] In one aspect, the present invention provides a highly weather-resistant water-based coating for glass fiber composite materials without pre-treatment, wherein the highly weather-resistant water-based coating is a two-component coating, wherein:

[0008] The raw materials of the first component include, by weight:

[0009] 30-80 parts of water-based acrylic resin, 5-20 parts of silane hydrolyzed oligomer, 2-10 parts of organic solvent, 2.1-30 parts of additives, 5-25 parts of filler, 5-15 parts of nano color paste and 5-25 parts of deionized water;

[0010] The raw materials of the second component include, by weight:

[0011] 70-90 parts of isocyanate curing agent and 10-30 parts of solvent.

[0012] Furthermore, the silane hydrolysis oligomer is an oligomer obtained by reacting an organic functional silane monomer and silica sol in the presence of an acid catalyst and an organic solvent using a sol-gel method.

[0013] Furthermore, the reaction temperature is 40-80°C and the reaction time is 1-3h.

[0014] Furthermore, in the method of preparing the silane hydrolyzed oligomer by the sol-gel method, the amount of the organic functional silane monomer is 20-60 parts, the amount of silica sol is 5-15 parts, the amount of the acid catalyst is 1-5 parts, and the amount of the organic solvent is 10-20 parts.

[0015] Furthermore, the preparation of the silane hydrolysis oligomer comprises the following steps:

[0016] Premixing the organic functional silane monomer and the organic solvent at a rotation speed of 400-700 rpm to obtain a premixed liquid;

[0017] After the temperature of the premixed liquid is raised to 80°C, silica sol and acid catalyst are added dropwise respectively, and the addition of silica sol and acid catalyst is controlled to be completed within 0.5h and 1h respectively. Finally, the obtained mixture is kept warm and reacted for 1h, then subjected to rotary evaporation at 40°C to remove small molecular by-products and matured to obtain the silane hydrolysis oligomer.

[0018] Furthermore, the filler is one or more of spherical fillers, flake fillers, fibrous fillers and rod-shaped fillers.

[0019] Furthermore, the fibrous filler is selected from one or more of wollastonite, feldspar powder, brucite and pyrophyllite.

[0020] Furthermore, the rod-shaped filler is selected from one or more of carbon nanotubes, graphene, rod-shaped cerium dioxide, rod-shaped aluminum oxide and rod-shaped aluminum silicate.

[0021] Furthermore, the spherical filler is selected from one or more of barium sulfate, calcium carbonate, quartz powder and fumed silica.

[0022] Furthermore, the particle size of the spherical filler is 350 mesh-2500 mesh.

[0023] Furthermore, the flaky filler is selected from one or more of kaolin, talc, mica, graphite powder, bentonite and attapulgite.

[0024] Furthermore, the particle size of the flaky filler is 325 mesh-2500 mesh.

[0025] Furthermore, the filler is a mixture of spherical fillers and flake fillers in a mass ratio of 1:1-10:1.

[0026] Furthermore, the mass ratio of the water-based acrylic resin to the filler is (2-8):1.

[0027] Furthermore, the auxiliary agent contains 1-10 parts of ultraviolet light absorber and 1-10 parts of ultraviolet light stabilizer.

[0028] In another aspect, the present invention provides a method for preparing the highly weather-resistant water-based coating as described above, the preparation method comprising the following steps:

[0029] Preparation of the first component:

[0030] The water-based acrylic resin and the silane hydrolyzed oligomer are dissolved in an organic solvent, mixed evenly, and then an auxiliary agent, a filler and a nano-color paste are added, mixed evenly, and the viscosity is adjusted with deionized water to obtain the first component;

[0031] Preparation of the second component:

[0032] The isocyanate curing agent is mixed with a solvent to obtain the second component.

[0033] In another aspect, the present invention provides use of the highly weather-resistant water-based coating as described above in coating of a glass fiber reinforced composite material structure.

[0034] Furthermore, the substrate of the glass fiber reinforced composite material structure is not pre-treated before painting.

[0035] Furthermore, the structure is a photovoltaic frame.

[0036] In another aspect, the present invention provides a glass fiber reinforced composite material structure, which comprises a substrate and a coating formed by the above-mentioned highly weather-resistant water-based coating applied on the surface of the substrate.

[0037] Furthermore, the structure is a photovoltaic frame.

[0038] In another aspect, the present invention provides a method for preparing the glass fiber reinforced composite material structure as described above, comprising the following steps:

[0039] The highly weather-resistant water-based paint is applied on a substrate to form a coating, wherein the substrate is not pre-treated before coating.

[0040] The beneficial effects of the present invention are as follows:

[0041] In the water-based coating provided by the present invention, by introducing an organosilane hydrolyzed oligomer, while ensuring excellent adhesion between the coating and the substrate, the cross-linking strength of the paint film can also be enhanced, thereby improving the ability of the coating to resist external damage; in addition, it is preferred that a specific filler can release the internal stress generated by the cross-linking of the paint film, so that the paint film has hard and tough characteristics, and it is further preferred to utilize the stacking shielding effect of spherical particles of different particle sizes, the covering effect of flaky fillers of different particle sizes on the coating surface, and the synergistic effect of water-based acrylic resin so that the coating can well increase chemical resistance and excellent UV resistance.

[0042] The VOC of the water-based paint provided in the present invention is lower than 200 g / L. After directly coating the glass fiber composite material without pre-treatment, the obtained coating can provide "0" level adhesion and has strict outdoor weather resistance. In addition, the water-based paint is easy to apply and is very suitable for coating the surface of the glass fiber composite material. DETAILED DESCRIPTION

[0043] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.

[0044] The glass fiber reinforced pultruded composite material structure (such as a photovoltaic frame) has the following problems: 1) before coating, the structure needs to be pre-treated (including grinding, burning, sandblasting, etc.) to improve the adhesion of the coating, which increases the production cost of the product and reduces the production efficiency; 2) in the glass fiber reinforced aromatic organic resin composite material structure, the aromatic organic resin is prone to yellowing after exposure to light, and the outdoor weather resistance and adhesion cannot meet the long-term outdoor use. A specific embodiment of the present invention provides a high weather-resistant water-based coating for glass fiber composite materials without pre-treatment. The high weather-resistant water-based coating is a two-component coating, wherein:

[0045] The raw materials of the first component include, by weight:

[0046] 30-80 parts of water-based acrylic resin, 5-20 parts of silane hydrolyzed oligomer, 2-10 parts of organic solvent, 2.1-30 parts of additives, 5-25 parts of filler, 5-15 parts of nano color paste and 5-25 parts of deionized water;

[0047] The raw materials of the second component include, by weight:

[0048] 70-90 parts of isocyanate curing agent and 10-30 parts of solvent.

[0049] The highly weather-resistant water-based coating provided in the present technical solution is particularly suitable for coating the surface of glass fiber reinforced composite materials structures (such as photovoltaic frames). The coating obtained after coating has good decorative appearance and excellent adhesion (good mechanical properties and adhesion, etc.), and can also enable the coated glass fiber reinforced composite materials structure to meet the weather resistance requirements for use in different harsh outdoor conditions.

[0050] In the present technical scheme, since the silane in the silane hydrolysis oligomer undergoes a hydrolysis condensation reaction during the film-forming process of the water-based coating, the generated silanol group can be anchored to the substrate, and the organic functional group (such as vinyl, amino, etc.) at the other end of the structure can react with the resin to form a covalent bond, for example, aminosilane can undergo a ring-opening reaction with the epoxy group in the epoxy resin to form a -NH-CH2- covalent bond, and vinylsilane can undergo a chain extension reaction with the group with an unsaturated double bond on the resin to form a -CH2-CH2- covalent bond, etc., thereby playing a good bridging role between the substrate and the coating, so that the coating can produce excellent adhesion with various glass fiber reinforced composite substrates without pre-treatment, and even the presence of a glass fiber reinforced composite surface release agent can be ignored, which greatly simplifies the coating process and improves production efficiency; secondly, the coating formed by the chemical reaction constitutes a dense network structure of organic-inorganic hybrid cross-linking, which can effectively improve the chemical resistance and aging resistance of the coating, thereby meeting the weather resistance requirements of the coated glass fiber reinforced composite structure under different harsh outdoor conditions.

[0051] In some examples, the silane hydrolyzed oligomer is an oligomer obtained by reacting an organic functional silane monomer and silica sol in the presence of an acid catalyst and an organic solvent using a sol-gel method.

[0052] In some examples, the reaction temperature is 40-80° C. and the reaction time is 1-3 h.

[0053] In some preferred examples, the reaction temperature is 80° C. and the reaction time is 1 h.

[0054] In this embodiment, the silane hydrolyzed oligomer preferably has a solid content of 20% to 60%.

[0055] In some specific examples, in the method of preparing silane hydrolyzed oligomers by a sol-gel method, the amount of the organic functional silane monomer is 20-60 parts, the amount of silica sol is 5-15 parts, the amount of the acid catalyst is 1-5 parts, and the amount of the organic solvent is 10-20 parts.

[0056] The silane hydrolyzed oligomer prepared by the above method can better improve the adhesion between the coating and the substrate, the coating hardness and the long-term weather resistance of the coating obtained after the above water-based coating is applied to the glass fiber reinforced composite material (without pretreatment).

[0057] In some specific embodiments, the organic functional silane monomer includes but is not limited to the compounds selected from the following:

[0058] For example, the organic functional silane monomer may be a monofunctional organic silane, i.e., an organic silane containing one hydrolyzable group. More specific substances include, for example, trimethylmethoxysilane, trimethylethoxysilane, triethylmethoxysilane, triethylethoxysilane, vinyldimethylmethoxysilane, vinyldimethylethoxysilane, γ-aminopropyldimethylmethoxysilane or γ-glycidoxypropyldimethylmethoxysilane, etc.;

[0059] Alternatively, the organic functional silane monomer is a bifunctional silane, i.e., an organic silane containing two hydrolyzable groups. Specific substances include, for example, dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane, diethyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, vinylmethyldimethoxysilane, vinylmethyldiethoxysilane or γ-aminopropylmethyldimethoxysilane, etc.;

[0060] Alternatively, the organic functional silane monomer is a trifunctional silane, i.e., an organic silane containing three hydrolyzable groups. Specific substances include, for example, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, γ-aminopropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane or γ-(2,3-epoxypropoxy)propyltrimethoxysilane (i.e., γ-glycidyloxypropyltrimethoxysilane), etc.

[0061] Alternatively, the organic functional silane monomer is a tetrafunctional silane, that is, an organic silane containing four hydrolyzable groups, such as tetramethyl silicate, tetraethyl silicate (also known as tetraethoxysilane), and the like.

[0062] In some specific examples of the present embodiment, one or more organic functional silane monomers can be selected to prepare the silane hydrolyzed oligomer. When the organic functional silane monomer is selected from the above two or more combinations, preferred combinations include a composition of methyl trimethoxy silane and γ-(2,3-epoxypropoxy)propyl trimethoxy silane, a composition of methyl trimethoxy silane and γ-epoxypropoxypropyl dimethyl methoxy silane, a composition of tetraethyl silicate and γ-(2,3-epoxypropoxy)propyl trimethoxy silane, and a composition of methyl triethoxy silane, tetraethyl silicate and γ-(2,3-epoxypropoxy)propyl trimethoxy silane (the mass ratio of the three is preferably (6-8):1:(1.5-5)).

[0063] In the technical solution, the silica sol is preferably an aqueous silica sol. In some examples, the silica sol is an acidic silica sol or an alkaline silica sol. Examples of silica sols include, but are not limited to, ST-OXS, ST-O, ST-OUP, ST-PS-SO, etc. selected from Nissan Chemical.

[0064] In some examples, the acid catalyst is selected from one or more of dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid, phosphoric acid, formic acid, acetic acid and citric acid.

[0065] In some examples, in the method of preparing silane hydrolyzed oligomers by sol-gel method, the organic solvent is selected from alcohol ether solvents, for example, one or more of ethanol, isopropanol, n-butanol, isobutanol, propylene glycol methyl ether, ethylene glycol butyl ether, dipropylene glycol monomethyl ether, diethylene glycol monobutyl ether and dipropylene glycol monobutyl ether.

[0066] In some more specific examples, the preparation of the silane hydrolysis oligomer comprises the following steps:

[0067] Premixing the organic functional silane monomer and the organic solvent at a rotation speed of 400-700 rpm to obtain a premixed liquid;

[0068] After the temperature of the premixed liquid is raised to 80°C, silica sol and acid catalyst are added dropwise respectively, and the addition of silica sol and acid catalyst is controlled to be completed within 0.5h and 1h respectively. Finally, the obtained mixture is kept warm and reacted for 1h, then subjected to rotary evaporation at 40°C to remove small molecular by-products and matured to obtain the silane hydrolysis oligomer.

[0069] In some more specific examples, the preparation of the silane hydrolysis oligomer comprises the following steps:

[0070] First, add 20-60 parts of organic functional silane monomer and 10-20 parts of alcohol ether solvent into a three-necked flask and premix at a rotation speed of 400-700rpm; then take 5-15 parts of aqueous silica sol and 1-5 parts of acid catalyst into a dropping funnel, and add them dropwise after the temperature of the premixed liquid rises to 80°C, and control the aqueous silica sol and the acid catalyst to be added dropwise within 0.5h and 1h respectively. Finally, keep the obtained mixture warm and continue to react for 1h, then perform rotary evaporation at 40°C to remove small molecular by-products, and mature overnight to obtain silane hydrolysis oligomers.

[0071] In some examples, the silane hydrolyzed oligomer includes, but is not limited to, one selected from the group consisting of the silane hydrolyzed oligomer prepared by the above method, KR-513, X-41-1805, etc. Preferably, the silane hydrolyzed oligomer is a silane hydrolyzed oligomer prepared by the above method.

[0072] In some examples, the content of silane hydrolyzed oligomer in the raw materials of the first component includes but is not limited to 10-20 parts, 10-15 parts, 5-15 parts, 15 parts, etc.

[0073] In some examples, the water-based acrylic resin can be selected from one or more combinations of water-based hydroxyl acrylic resin, epoxy-modified water-based acrylic resin, polyurethane-modified water-based acrylic resin, silicone-modified water-based acrylic resin, organic fluorine-modified water-based acrylic resin, alkyd resin-modified hybrid water-based acrylic resin, and nano-modified water-based acrylic resin.

[0074] In some examples, the solid content of the water-based hydroxyl acrylic resin is 40%-60%, and the hydroxyl value is 80-140 mgKOH / g. In some more specific examples, the water-based hydroxyl acrylic resin includes but is not limited to selected from Wanhua 2035, 2042, 2033, Covestro's Bayhydrol A 2695, Bayhydrol A2470, Bayhydrol A 2651, etc.

[0075] Exemplarily, the epoxy-modified waterborne acrylic resin includes, but is not limited to, at least one selected from a graft copolymer of epoxy resin and acrylate, a copolymer of epoxysilane and acrylate, and a copolymer of glycidyl ether (GMA) and acrylate.

[0076] Exemplarily, the polyurethane-modified waterborne acrylic resin includes, but is not limited to, at least one copolymer of polyurethane and acrylate prepared by reacting one or more of toluene-2,4-diisocyanate, diphenylmethane-4,4'-diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, trimethylhexane diisocyanate, meta-xylylene diisocyanate, and isophorone diisocyanate with a polyol.

[0077] Exemplarily, the organosilicon-modified waterborne acrylic resin includes, but is not limited to, at least one selected from the group consisting of polyorganosilane, polyorganosiloxane, polyorganosilane and copolymers of acrylates.

[0078] Exemplarily, the organic fluorine-modified waterborne acrylic resin includes, but is not limited to, a waterborne acrylic resin graft-modified by copolymers of one or more fluoroolefins selected from tetrafluoroethylene, vinylidene fluoride, vinyl fluoride, etc. and alkyl vinyl ethers or esters. For example, it includes, but is not limited to, commercially available HD-8669, HD-827, HD-830, etc. of Shanghai Xunda New Materials.

[0079] In some preferred examples, the water-based acrylic resin is the above-mentioned water-based hydroxy acrylic resin, or the above-mentioned water-based hydroxy acrylic resin is mixed with an organic fluorine-modified water-based acrylic resin. More preferably, it is a mixture of a water-based hydroxy acrylic resin and an organic fluorine-modified water-based acrylic resin. At this time, the paint film obtained has better aging resistance and long-term weather resistance. Exemplarily, when the water-based acrylic resin is a mixture of the above-mentioned water-based hydroxy acrylic resin and an organic fluorine-modified water-based acrylic resin, the mass ratio of the two is preferably (0.4-5): 1, (0.4-3): 1, (0.4-2.5): 1, (0.4-1): 1, (0.4-0.8): 1, (1.5-5): 1, (1.5-3): 1, (2-3): 1, etc.

[0080] Exemplarily, the alkyd resin modified hybrid waterborne acrylic resin includes but is not limited to at least one alkyd resin modified hybrid waterborne acrylic resin synthesized from at least one of soybean oil fatty acid, tung oil fatty acid, linseed oil fatty acid, tall oil fatty acid, and castor oil fatty acid.

[0081] Exemplarily, the nano-modified water-based acrylic resin includes, but is not limited to, at least one water-based acrylic resin modified by at least one of nano-silicon dioxide, nano-titanium dioxide, nano-zinc dioxide, nano-calcium carbonate, and nano-ferric oxide.

[0082] In some examples, in the raw materials of the first component of the water-based coating, the weight proportion of the water-based acrylic resin includes but is not limited to 30-60 parts, 50-80 parts, 40-60 parts, 50 parts, etc.

[0083] In some preferred examples, the additive contains 1-10 parts of ultraviolet light absorber and 1-10 parts of ultraviolet light stabilizer. In this case, the yellowing, gloss loss or powdering of the paint film can be effectively delayed. The exemplary content of the ultraviolet light absorber is 1-5 parts, 1-2 parts, etc. The exemplary content of the ultraviolet light stabilizer is 1-5 parts, 1-2 parts, etc.

[0084] Exemplarily, the ultraviolet light absorber is selected from at least one of Tinuvin 1130, Tinuvin 1600 and Tinuvin 171.

[0085] Exemplarily, the ultraviolet light stabilizer is selected from at least one of Tinuvin 123, Tinuvin 249 and Tinuvin 292.

[0086] In this embodiment, the additives may further include one or more additional additives including substrate wetting agents (such as Tego Wet 270, etc.), leveling agents (such as BYK-333, etc.), defoamers (such as BYK-024, etc.), and rheological additives (such as TegoViscoPlus 3060, etc.) according to actual needs. Those skilled in the art will appreciate that the above additives have specific uses, but their specific use should be determined by formulation selection and process.

[0087] In some examples, the first component includes 0.05-3 parts of a substrate wetting agent, 0.05-3 parts of a leveling agent, 0.05-3 parts of a defoaming agent, and 0.05-5 parts of a rheological additive.

[0088] Exemplarily, the functional filler is selected from one or more of spherical fillers, flake fillers, fibrous fillers, and rod-shaped fillers.

[0089] Exemplarily, suitable spherical fillers include, but are not limited to, one or more of barium sulfate, calcium carbonate, quartz powder, and fumed silica.

[0090] Exemplarily, suitable flake fillers include, but are not limited to, one or more of kaolin, talc, mica, graphite powder, bentonite, and attapulgite.

[0091] Exemplarily, suitable fibrous fillers include, but are not limited to, one or more of wollastonite, feldspar powder, brucite, and pyrophyllite.

[0092] Exemplarily, suitable rod-shaped fillers include, but are not limited to, one or more of carbon nanotubes, graphene, rod-shaped cerium dioxide, rod-shaped aluminum oxide, and rod-shaped aluminum silicate.

[0093] In some examples, the filler is a mixture of spherical fillers and flaky fillers. In addition to enhancing the performance of the paint film, the use of spherical fillers can also relieve the large internal stress generated by silane hydrolyzed oligomers during the reaction cross-linking process; because of their high specific surface area, flaky fillers can form a physical shielding effect in the paint film, such as reflecting light and blocking water vapor; through the synergistic effect of flaky fillers and spherical fillers, the density of the paint film can be effectively improved, thereby improving the various resistances of the coating; more importantly, the regular arrangement of these two fillers on the surface of the coating can greatly reflect and hinder the damage of ultraviolet rays to the coating, thereby extending the life of the structure coated with the coating (especially the glass fiber reinforced composite structure) for long-term outdoor use.

[0094] In some examples, the particle size of the spherical filler is preferably 350 mesh to 2500 mesh, and the particle size of the flake filler is preferably 325 mesh to 2500 mesh. In this case, the obtained coating has better hardness, flexibility and weather resistance.

[0095] The filler contained in the water-based paint of this scheme can release the internal stress generated by the cross-linking of the paint film, so that the paint film has hard and tough characteristics; in addition, through the stacking shielding effect of spherical particles of different particle sizes, the shielding effect of flaky fillers (reflecting ultraviolet rays) and the synergistic effect of water-based acrylic resin, the coating can well increase chemical resistance and excellent ultraviolet resistance. In some preferred examples, the mass ratio of the water-based acrylic resin to the filler is (2-8): 1. At this time, the above-mentioned effect is better. Exemplarily, the mass ratio of the water-based acrylic resin to the filler includes but is not limited to (2-5): 1, (2-4): 1, (3-4): 1, (3-3.5): 1, etc.

[0096] Preferably, the spherical filler is selected from barium sulfate. In some specific examples, the particle sizes of the spherical fillers from coarse to fine are 350 mesh, 600 mesh, 1000 mesh, 1250 mesh, 2000 mesh, 2500 mesh, etc.

[0097] In some other preferred examples, the spherical filler is a mixture of barium sulfate with a particle size of 1000 mesh and 2000 mesh. The mixing ratio of the two is preferably (1-3):7, 2:7, etc. Barium sulfate has a large density and is often located at the bottom of the paint film. Since it can reflect light in a certain wavelength range (300-400nm), it can protect the paint film from light aging. The main reason for selecting barium sulfate with different particle sizes is to obtain the best paint film density based on the close packing effect of large particles and small particles.

[0098] Preferably, the flaky filler is selected from mica. In some specific examples, the particle sizes of the flaky filler from coarse to fine are 325 mesh, 600 mesh, 800 mesh, 1250 mesh, 2000 mesh, and 2500 mesh.

[0099] In some other preferred examples, the flaky filler is a mixture of mica with a particle size of 1250 mesh and 2000 mesh. The mixing ratio of the two is preferably (1-3):5, 2:5, etc. Mica has a low density and its own flaky shape, so it is easy to disperse on the surface of the paint film, has a good reflective effect on light and can also block moisture. Since the paint film will shrink to a certain extent during the film formation process, the flaky filler cannot be ideally spread on the surface of the paint film. The spatial complementary effect of flaky fillers with different particle sizes can form a physical barrier on the surface.

[0100] In some preferred examples, the mass ratio of the spherical filler to the flake filler is 1:1-10:1. Exemplarily, the mass ratio of the spherical filler to the flake filler includes but is not limited to (1-5):1, (1-3):1, (1-2):1, 9:7, etc. In this case, the obtained paint film has better surface density, yellowing resistance, outdoor weather resistance and adhesion.

[0101] In some examples, in the raw materials of the first component of the water-based coating, the weight proportion of the filler includes but is not limited to 10-25 parts, 10-20 parts, 10-16 parts, 15-25 parts, 15-20 parts, 16 parts, etc.

[0102] In this embodiment, there is no requirement for the color and selection of the nano-color paste, and any nano-color paste conventionally used in the art for glass fiber composite material substrates can be used. In some examples, the nano-color paste includes but is not limited to one or more selected from AQUECO 9000 water-based color paste-black, AQUECO 9000 water-based color paste-white, AQUECO 9000 water-based color paste-yellow, AQUECO9000 water-based color paste-red, etc.

[0103] In this embodiment, in the raw materials of the first component, the organic solvent is mainly used to dissolve the water-based acrylic resin. For example, the suitable organic solvent can be an alcohol ether solvent. Exemplarily, the organic solvent in the raw materials of the first component is selected from one or more combinations of ethylene glycol monobutyl ether, n-butanol, isobutyl alcohol, ethylene glycol isooctyl ether, propylene glycol methyl ether, dipropylene glycol monobutyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, ethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, and 1-2-propylene glycol diacetate.

[0104] In some examples, the isocyanate curing agent is a hydrophilic polyisocyanate.

[0105] Furthermore, the hydrophilic polyisocyanate is selected from at least one of the group consisting of aliphatic isocyanate polymers (including aliphatic isocyanate dimers, aliphatic isocyanate trimers, etc.), aromatic isocyanate polymers (including aromatic isocyanate dimers, aromatic isocyanate trimers, etc.), and alicyclic isocyanate polymers (including alicyclic isocyanate dimers, alicyclic isocyanate trimers, etc.).

[0106] Exemplarily, the aliphatic isocyanate polymer is a polymer of at least one selected from the group consisting of tetramethylene 1,4-diisocyanate, hexamethylene 1,6-diisocyanate, 2,2,4-trimethylhexane 1,6-diisocyanate, ethylene diisocyanate, and 1,12-dodecyl diisocyanate.

[0107] Exemplarily, the alicyclic isocyanate polymer is selected from at least one polymer of the group consisting of isophorone diisocyanate, cyclobutane 1,3-diisocyanate, cyclohexane 1,3-diisocyanate, cyclohexane 1,4-diisocyanate, methylcyclohexyl diisocyanate, 4,4-methylene dicyclohexyl diisocyanate, and hydrogenated diphenylmethane diisocyanate.

[0108] In some specific examples, the isocyanate curing agent is one or more of Bayhydur Ultra 2655, Bayhydur Ultra 307, Bayhydur Ultra 304, etc., manufactured by Covestro.

[0109] The solvent is mainly used to dissolve the isocyanate curing agent. Exemplarily, the solvent is selected from one or more combinations of n-butyl alcohol, isobutyl alcohol, ethylene glycol isooctyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, dipropylene glycol monobutyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, ethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, and propylene glycol diacetate (PGDA).

[0110] In some examples, the weight ratio of the first component to the second component raw materials is 100:10-90, preferably 100:20-50, and more preferably 100:40.

[0111] In some examples, the total weight of the raw materials of the first component is 100 parts.

[0112] In some examples, the total weight of the raw materials of the second component is 100 parts.

[0113] According to another specific embodiment of the present invention, a method for preparing the highly weather-resistant water-based coating as described above is provided, comprising the following steps:

[0114] Preparation of the first component:

[0115] The water-based acrylic resin and the silane hydrolyzed oligomer are dissolved in an organic solvent, mixed evenly, and then an auxiliary agent, a filler and a nano-color paste are added, mixed evenly, and the viscosity is adjusted with deionized water to obtain the first component;

[0116] Preparation of the second component:

[0117] The isocyanate curing agent is mixed with a solvent to obtain the second component.

[0118] Exemplarily, the preparation of the second component includes: under nitrogen protection, adjusting the water content of the solvent, adding an isocyanate curing agent, and stirring evenly to obtain the second component.

[0119] According to another specific embodiment of the present invention, there is provided use of the highly weather-resistant water-based coating as described above in coating of a glass fiber reinforced composite material structure.

[0120] In some examples, the substrate of the glass fiber reinforced composite material structure is not pre-treated before painting. The pre-treatment herein includes but is not limited to grinding, burning, sandblasting, etc.

[0121] In some examples, the structure is a photovoltaic frame.

[0122] According to another specific embodiment of the present invention, a glass fiber reinforced composite material structure is provided, which includes a substrate and a coating formed by the highly weather-resistant water-based coating as described above and coated on the surface of the substrate.

[0123] Exemplarily, the substrate refers to a base formed by a glass fiber reinforced composite material without coating.

[0124] Exemplarily, the structure is a photovoltaic frame.

[0125] According to another specific embodiment of the present invention, there is provided a method for preparing the glass fiber reinforced composite material structure as described above, comprising the following steps:

[0126] The highly weather-resistant water-based paint is applied on a substrate to form a coating, wherein the substrate is not pre-treated before coating.

[0127] The substrate refers to a base formed by a glass fiber reinforced composite material without coating.

[0128] Exemplarily, the structure is a photovoltaic frame.

[0129] It should be noted that, in this embodiment, the highly weather-resistant water-based paint can be used to coat substrates that have not been pre-treated, and can also be used to coat substrates that have been pre-treated. After coating the pre-treated substrate, the coated structure also has good adhesion and outdoor weather resistance in extreme environments, which will not be described in detail here.

[0130] In some specific examples, the method for preparing the glass fiber reinforced composite material structure comprises the following steps:

[0131] Under the environmental conditions of 25±2°C and relative humidity of 50±5%, the first component and the second component of the highly weather-resistant water-based coating are mixed evenly in corresponding proportions, and then deionized water is added to adjust the construction viscosity to 4 cups, the viscosity is within 30-40 seconds, and spray 3-4 times;

[0132] The substrate refers to a base formed by a glass fiber reinforced composite material that is not coated with paint, and the substrate may not be pre-treated before coating.

[0133] In some examples, in the preparation method, the dry film thickness of the coating obtained by coating is 30-40 μm.

[0134] The technical solution of the present invention is described below in conjunction with some specific embodiments:

[0135] Unless otherwise specified, the silane hydrolyzed oligomers used in the examples were prepared by the following method:

[0136] First, add 40 parts of methyltriethoxysilane, 5 parts of tetraethyl silicate, 10 parts of γ-(2,3-epoxypropoxy)propyltrimethoxysilane, 15 parts of anhydrous ethanol, and 5 parts of ethylene glycol butyl ether into a three-necked flask and premix at a speed of 400-700rpm; then take 15 parts of aqueous silica sol ST-O-40 and 1 part of acid catalyst dilute hydrochloric acid (concentration of 0.1mol / L) into a dropping funnel, and add them dropwise after the temperature of the premixed liquid rises to 80°C, and control the aqueous silica sol and the acid catalyst to be added dropwise within 0.5h and 1h respectively. Finally, keep the obtained mixture warm and continue to react for 1h, then perform rotary evaporation at 40°C to remove small molecular by-products, and mature overnight to obtain silane hydrolysis oligomers.

[0137] Example 1

[0138] A highly weather-resistant water-based coating for glass fiber composite materials without pre-treatment, which is a two-component coating, wherein:

[0139] The raw material composition of component A is shown in Table 1 below;

[0140] The B component formula is: 70 parts of Bayhydur Ultra 2655 and 30 parts of propylene glycol diacetate.

[0141] The method for preparing the above-mentioned high weather-resistant water-based coating for glass fiber composite material without pre-treatment comprises the following steps:

[0142] Preparation of component A:

[0143] After adding water-based acrylic resin to the organic solvent, stir at medium speed for 10-15 minutes, then add additives (substrate wetting agent, leveling agent, defoamer, rheological additive, UV absorber, UV stabilizer), filler, nano-color paste and disperse and mix evenly at high speed, finally adjust the viscosity to 100-5000mPas with deionized water, filter, and obtain component A.

[0144] Preparation of component B:

[0145] Under nitrogen protection, the water content of the solvent propylene glycol diacetate was adjusted, and the isocyanate curing agent Bayhydur Ultra 2655 was added and stirred evenly to obtain component B.

[0146] Wherein, component A and component B are mixed at a mass ratio of 100:40 when used to obtain an aqueous coating composition 1.

[0147] Example 2

[0148] A highly weather-resistant water-based coating for glass fiber composite materials without pre-treatment, which is a two-component coating, wherein:

[0149] The raw material composition of component A is shown in Table 1 below;

[0150] The B component formula is: 70 parts of Bayhydur Ultra 2655 and 30 parts of propylene glycol diacetate.

[0151] The method for preparing the above-mentioned high weather-resistant water-based coating for glass fiber composite material without pre-treatment comprises the following steps:

[0152] Preparation of component A:

[0153] After adding water-based acrylic resin and silane hydrolyzed oligomer to the organic solvent, stir at medium speed for 10-15 minutes, then add additives (substrate wetting agent, leveling agent, defoamer, rheological additive, UV absorber, UV stabilizer), filler, nano-color paste and disperse and mix evenly at high speed, finally adjust the viscosity to 100-5000mPas with deionized water, filter, and obtain component A.

[0154] Preparation of component B:

[0155] Under nitrogen protection, the water content of the solvent propylene glycol diacetate was adjusted, and the isocyanate curing agent Bayhydur Ultra 2655 was added and stirred evenly to obtain component B.

[0156] Wherein, component A and component B are mixed at a mass ratio of 100:40 when used to obtain an aqueous coating composition 2.

[0157] Table 1 A component formula

[0158]

[0159] Table 2A Component Formulation

[0160]

[0161] Example 3

[0162] Example 2 was repeated, except that, in the formula of component A in this example, the water-based acrylic resin was a mixture of a water-based hydroxy acrylic dispersion and a water-based acrylic resin modified by organic fluorine in a mass ratio of 7:3, and other conditions remained unchanged, to prepare a water-based coating composition 3.

[0163] Example 4

[0164] Example 3 was repeated, except that, in the formulation of component A in this example, the silane hydrolyzed oligomer was the commercially available product KR-513, and other conditions remained unchanged, to prepare an aqueous coating composition 4.

[0165] Example 5

[0166] Example 3 was repeated, except that in the present example, in the formulation of component A, the silane hydrolyzed oligomer was the commercially available product X-41-1805, and other conditions remained unchanged, to prepare an aqueous coating composition 5.

[0167] Example 6

[0168] Example 3 was repeated, except that, in the formulation of component A in this example, the mass ratio of the aqueous hydroxylated acrylic dispersion to the organic fluorine-modified aqueous acrylic resin was 3:7, and other conditions remained unchanged, thereby preparing an aqueous coating composition 6.

[0169] Example 7

[0170] Example 3 was repeated, except that, in the formulation of component A in this example, the filler did not contain barium sulfate, and other conditions remained unchanged, to prepare an aqueous coating composition 7.

[0171] Example 8

[0172] Example 3 was repeated, except that, in the formulation of component A in this example, the filler did not contain mica powder, and other conditions remained unchanged, to prepare an aqueous coating composition 8.

[0173] Example 9

[0174] Example 3 was repeated, except that, in this example, in the formula of component A, the filler contained only 2000 mesh mica powder, and its content in component A was 7 wt %. Other conditions remained unchanged, and an aqueous coating composition 9 was prepared.

[0175] Example 10

[0176] Example 3 was repeated, except that, in this example, in the formula of component A, the filler only contained 2000 mesh barium sulfate, and its content in component A was 9 wt %. Other conditions remained unchanged, and an aqueous coating composition 10 was prepared.

[0177] The coatings obtained in the above embodiments were applied to the glass fiber composite substrate (without pretreatment) in the same construction method, and the performance of the coating finally obtained was tested. The test results are shown in Tables 3 and 4 below.

[0178] Among them, the specific coating method includes the following steps:

[0179] Under the environmental conditions of 25±2℃ and relative humidity of 50±5%, mix component A and component B in corresponding proportions, add deionized water to adjust the construction viscosity to 4 cups, and use Iwata W-101 spray gun to spray 3-4 times within 30-40 seconds.

[0180] Table 3. Performance test results of coatings

[0181]

[0182]

[0183] Table 4. Performance test results of coating

[0184]

[0185]

[0186] The results of Tables 3 and 4 show that the highly weather-resistant water-based coating of the present invention can be well wetted and leveled on the surface of the glass fiber composite substrate (without pretreatment) and provide excellent adhesion and decorative properties. At the same time, the highly weather-resistant water-based coating has good mechanical properties and aging resistance, which can meet the application of the glass fiber composite substrate in various harsh environments.

[0187] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not limitations on the implementation methods of the present invention. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are still within the protection scope of the present invention.

Claims

1. A highly weather-resistant water-based coating for glass fiber composite materials without pre-treatment, characterized in that: The highly weather-resistant water-based coating is a two-component coating, wherein: The raw materials of the first component include, by weight: 30-80 parts of water-based acrylic resin, 5-20 parts of silane hydrolyzed oligomer, 2-10 parts of organic solvent, 2.1-30 parts of additives, 5-25 parts of filler, 5-15 parts of nano color paste and 5-25 parts of deionized water; The raw materials of the second component include, by weight: 70-90 parts of isocyanate curing agent and 10-30 parts of solvent.

2. The highly weather-resistant water-based coating according to claim 1, characterized in that: The silane hydrolysis oligomer is an oligomer obtained by reacting an organic functional silane monomer and a silica sol in the presence of an acid catalyst and an organic solvent using a sol-gel method; Preferably, the reaction temperature is 40-80°C and the reaction time is 1-3h; Preferably, in the method of preparing the silane hydrolyzed oligomer by the sol-gel method, the amount of the organic functional silane monomer is 20-60 parts, the amount of silica sol is 5-15 parts, the amount of the acid catalyst is 1-5 parts, and the amount of the organic solvent is 10-20 parts.

3. The highly weather-resistant water-based coating according to claim 1 or 2, characterized in that: The preparation of the silane hydrolysis oligomer comprises the following steps: Premixing the organic functional silane monomer and the organic solvent at a rotation speed of 400-700 rpm to obtain a premixed liquid; After the temperature of the premixed liquid is raised to 80°C, silica sol and acid catalyst are added dropwise respectively, and the addition of silica sol and acid catalyst is controlled to be completed within 0.5h and 1h respectively. Finally, the obtained mixture is kept warm and reacted for 1h, then subjected to rotary evaporation at 40°C to remove small molecular by-products and matured to obtain the silane hydrolysis oligomer.

4. The highly weather-resistant water-based coating according to claim 1, characterized in that: The filler is one or more of spherical fillers, flake fillers, fibrous fillers and rod-shaped fillers; Preferably, the fibrous filler is selected from one or more of wollastonite, feldspar powder, brucite and pyrophyllite; Preferably, the rod-shaped filler is selected from one or more of carbon nanotubes, graphene, rod-shaped cerium dioxide, rod-shaped aluminum oxide and rod-shaped aluminum silicate; Preferably, the spherical filler is selected from one or more of barium sulfate, calcium carbonate, quartz powder and fumed silica; Preferably, the particle size of the spherical filler is 350 mesh-2500 mesh; Preferably, the flaky filler is selected from one or more of kaolin, talc, mica, graphite powder, bentonite and attapulgite; Preferably, the particle size of the flake filler is 325 mesh to 2500 mesh; Preferably, the filler is a mixture of spherical fillers and flake fillers in a mass ratio of 1:1-10:1; Preferably, the mass ratio of the water-based acrylic resin to the filler is (2-8):

1.

5. The highly weather-resistant water-based coating according to claim 1, characterized in that: The auxiliary agent comprises 1-10 parts of ultraviolet light absorber and 1-10 parts of ultraviolet light stabilizer.

6. The method for preparing a highly weather-resistant water-based coating according to any one of claims 1 to 5, characterized in that: The steps include: Preparation of the first component: The water-based acrylic resin and the silane hydrolyzed oligomer are dissolved in an organic solvent, mixed evenly, and then an auxiliary agent, a filler and a nano-color paste are added, mixed evenly, and the viscosity is adjusted with deionized water to obtain the first component; Preparation of the second component: The isocyanate curing agent is mixed with a solvent to obtain the second component.

7. Use of the highly weather-resistant water-based coating according to any one of claims 1 to 5 in coating of glass fiber reinforced composite material structures, characterized in that: The substrate of the glass fiber reinforced composite material structure is not pre-treated before coating; Preferably, the structure is a photovoltaic frame.

8. A glass fiber reinforced composite material structure, characterized in that: The invention comprises a substrate, and a coating formed by the highly weather-resistant water-based coating as claimed in any one of claims 1 to 5 and coated on the surface of the substrate.

9. The glass fiber reinforced composite material structure according to claim 8, characterized in that: The structure is a photovoltaic frame.

10. The method for preparing a glass fiber reinforced composite material structure according to claim 8 or 9, characterized in that: The steps include: The highly weather-resistant water-based paint is applied on a substrate to form a coating, wherein the substrate is not pre-treated before coating.

Citation Information

Patent Citations

  • Inorganic nano polymer modified high-wear-resistant rubber and preparation method thereof

    CN111825899A

  • Water-based high-weather-resistance coating for composite material and preparation method thereof

    CN112852270A

  • Water-based curable resin composition, water-based coating material, and coated article

    JP2005154587A

  • Process for coating a glass substrate with an aqueous fluoropolymer coating

    US20150086792A1

Cited By

  • Water-based low-temperature baking coating for plastic photovoltaic frame and preparation method thereof

    CN122854912A

  • A water-based two-component polyurethane finish for photovoltaic frames and a preparation method thereof

    CN123004258A