Method for removing fluorine and heavy metals and extracting lithium from high-fluorine battery black powder leachate
Through sulfuric acid leaching method and multi-step alkaline treatment, combined with fluorine removal resin technology, the problem of fluorine ions removal in ternary lithium battery black powder is solved, efficient lithium recovery and deep fluorine removal is achieved, and cost and environmental impact is reduced.
Patent Information
- Application Number
- CN202411135001.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-29
AI Technical Summary
In the prior art, it is difficult to effectively remove fluoride ions in the wet recovery process of ternary lithium battery black powder, resulting in subsequent product quality and environmental pollution. The recovery rate of lithium is low, and traditional fluorine-deductors are consumed and costly. High and failed to remove fluorine deeply.
The sulfuric acid leaching method is used to extract lithium, combined with alkaline regulation and fluorine removal resin technology, and through multiple steps, including sulfuric acid leaching, alkaline water washing, fluorine removal resin treatment and lithium hydroxide precipitation, deep removal of fluorine and impurities, and reduce the loss of lithium and the use of fluoride removers.
It realizes efficient removal of fluorine in battery black powder and has high recovery rate of lithium, reducing the consumption of sulfuric acid and alkali liquid, reducing costs, avoiding fluorine entering the subsequent nickel-cobalt-manganese leaching-extraction system, and improving the product Purity and environmental protection.
Smart Images

Figure CN119040634A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion battery recycling, and in particular belongs to a method for removing fluorine and weight from a high-fluorine battery black powder leachate and extracting lithium. Background Art
[0002] Ternary lithium batteries are widely used due to their high energy density, fast charge and discharge speed, and long cycle life. The scale of China's lithium battery industry ranks first in the world. With the constraints of upstream resources in the ternary lithium battery industry, the expansion of the downstream market, and the increasing number of retired and scrapped lithium batteries year by year, the recycling of retired and scrapped ternary lithium batteries has become another major industrial chain. The traditional processing and recycling routes for waste ternary lithium-ion batteries are mainly pretreatment, metal extraction, and product purification and recycling processes. The pretreatment mainly involves discharging, disassembling, crushing, roasting and pyrolysis of ternary lithium-ion batteries to obtain mixed positive and negative electrode black powder, namely ternary black powder. It can be seen that the main elements in ternary black powder are Ni, Co, Mn, Li, Al, Cu, F, etc., among which Ca and Fe content is relatively low, and Al and Cu mainly come from the current collector metal foil in the battery, with a relatively high content.
[0003] At present, the traditional recycling process of ternary battery black powder is mainly a wet process, which has the advantages of high metal recovery rate, high product purity and low energy consumption. Ternary battery black powder contains a lot of fluorine-containing compounds, resulting in a large amount of fluoride ions in the leachate after wet leaching. The presence of fluoride ions in the acidic leachate will seriously affect the quality of subsequent products, and at the same time cause corrosion damage to subsequent process equipment, posing serious environmental pollution and safety hazards. The traditional process does not defluorinate the battery leachate, but extracts the valuable metal elements in the battery leachate into the organic phase, leaving the fluorine in the raffinate wastewater. This process requires the use of a variety of extraction agents and a large part of the fluorine will still enter the nickel-cobalt-manganese-lithium solution during the extraction process, which will affect the subsequent removal of impurities and extraction of valuable metals. At present, there are many studies on wastewater defluorination, and wastewater defluorination is mostly treated by combining calcium salt precipitation method and coagulation precipitation method. In addition, lithium recovery in the wet process is generally carried out by extracting manganese, cobalt and nickel from a nickel-cobalt-manganese-lithium mixed solution and then recovering them. When extracting nickel, lithium will also enter the nickel sulfate system to a certain extent, causing lithium recovery losses, resulting in a low lithium recovery rate.
[0004] The prior art CN 117699829 A uses lithium carbonate salt for defluorination, specifically, fluorine-containing lithium salt powder is acid-dissolved to obtain a fluorine-containing lithium sulfate system, a composite defluoridation agent is added thereto for defluorination, and then impurities are removed and lithium is precipitated with sodium carbonate to obtain defluorinated lithium carbonate, and the content of fluorine element can be controlled at about 100ppm. This method is for the purification and defluorination of lithium carbonate products at the back end, involving the form transformation of lithium carbonate-lithium sulfate-lithium carbonate, and the process is relatively cumbersome and complicated. The prior art CN 117821754 A uses battery black powder sulfuric acid roasting and water leaching to extract lithium, acid leaching and metal removal of water-leached black powder residue, and iron-aluminum slag is used as a defluoridation agent for defluorination, and the lithium recovery rate can reach 99%. The defluorination principle is to utilize the adsorption effect of the added defluoridation agent, but the decomposition temperature of nickel, cobalt and manganese sulfate into oxides during sulfuric acid roasting and lithium extraction is high, and it is difficult to control the temperature so that the nickel, cobalt and manganese content in the lithium extraction solution is low, and additional iron powder needs to be added to remove copper, and then iron and aluminum are removed, resulting in a large amount of iron and aluminum slag. The technical solution also involves direct acid leaching without calcining the battery to extract lithium, but the lithium recovery rate is low, only more than 70%. The prior art CN 118302548 A involves the extraction and defluorination of low-fluorine concentration battery leachate, the principle is to rely on the iron ion element in the organic loaded trivalent iron extractant to complex with fluorine to extract fluorine in the leachate, and the blank part is supplemented with iron and cannot extract fluorine.
[0005] Commonly used defluoridation agents in the prior art include aluminum defluoridation agents and calcium salt defluoridation agents. If the fluorine in the lithium-containing solution needs to be removed to within 100-200 mg / L, a large amount of defluoridation agent needs to be added, which is not economical and environmentally friendly, and the defluoridation effect is also average. The test results of the applicant show that the use of aluminum salt defluoridation agent in the ternary black powder high-fluorine leachate can control the defluoridation effect to 100-200 mg / L, and the defluoridation effect does not change significantly with the increase of the amount of aluminum defluoridation agent used in a single defluoridation. After the defluoridation agent is defluorinated, adding a large amount of defluoridation agent to the defluoridation liquid for the second time cannot deeply defluorinate, and the fluorine concentration is controlled at 60-140 mg / L. This process will consume a large amount of defluoridation agent and produce a large amount of aluminum slag. Calcium salt defluoridation agent can only produce a large amount of calcium fluoride precipitation under alkaline pH, has a significant defluoridation effect, and the solubility of calcium fluoride precipitation in high sulfate leachate is greatly increased (He Huan. Research on defluoridation technology of high-fluorine zinc sulfate solution [D]. Kunming University of Science and Technology, 2016.).
[0006] The existing technology CN 113106257 B has the following problems: 1. The lithium extraction method of calcining battery black powder in reducing atmosphere and multi-stage countercurrent washing is adopted. The lithium leaching rate is greater than or equal to 95%, and some lithium will still be lost in the lithium-removing black powder. After the washing liquid is subjected to aluminum precipitation and impurity removal, the lithium is precipitated to prepare crude lithium carbonate, and the lithium-containing liquid is not deeply impurized. The impurity content in the crude lithium carbonate is relatively high. 2. The technology focuses on the impurity removal and recovery treatment of the lithium-removing black powder, which mainly includes: acid leaching, reducing acid leaching, deep copper removal using copper extractant and displacement method, and then P204 extraction and impurity removal of the copper-removed liquid, adding fluoride salt to remove calcium and magnesium to obtain a nickel-cobalt-manganese mixed solution, etc. The process does not describe the defluorination. Instead, fluorine is introduced in the subsequent calcium and magnesium removal process, and the solubility of calcium fluoride in the sulfuric acid system will greatly increase, making it difficult to use calcium salt for deep defluorination or fluoride salt for deep decalcification. Summary of the invention
[0007] In view of the shortcomings of the above-mentioned technology, the present invention provides a method for removing fluorine, removing weight and extracting lithium from high-fluorine battery black powder leachate, and the specific steps are as follows:
[0008] (1) reacting ternary black powder with a sulfuric acid leaching agent, adjusting the pH at the reaction endpoint, and separating the solid and liquid after the reaction to obtain a high-fluorine leaching solution and leaching residue;
[0009] (2) The high-fluorine leachate is leached with an alkaline reagent to adjust the pH of the leachate to remove Al and F, and the aluminum-fluoride-removed leachate and aluminum-fluoride slag are obtained by filtering, and the aluminum-fluoride slag and the leachate slag in step (1) are washed with water respectively.
[0010] (3) the aluminum-fluoride-removing leaching solution is introduced into a fluorine-removing resin for fluorine removal to obtain a resin-fluorine-removing leaching solution;
[0011] (4) adding an alkaline agent to adjust the pH of the resin defluorination leachate to recover Ni, Co, and Mn therein, and filtering to obtain a lithium extraction solution and nickel-cobalt-manganese slag;
[0012] (5) washing the nickel-cobalt-manganese slag with water to obtain nickel-cobalt-manganese washed slag, mixing the nickel-cobalt-manganese washed slag with the leached slag washed slag in step (2) in proportion, and entering into a nickel-cobalt-manganese leaching-extraction system to remove impurities and separate nickel, cobalt and manganese;
[0013] (6) The lithium extraction solution in step (4) is passed through a calcium and magnesium removal resin for deep impurity removal to obtain a refined lithium hydroxide solution, and sodium carbonate is added to the refined lithium hydroxide solution to precipitate lithium to prepare lithium carbonate.
[0014] In the step (1), the ternary black powder is obtained from the positive electrode material containing aluminum current collector or the positive and negative electrode materials containing current collector; the battery black powder type is one or more of nickel cobalt manganese oxide battery black powder, nickel cobalt aluminum oxide battery black powder, and lithium cobalt oxide and lithium manganese oxide battery black powder.
[0015] In the step (1), the reaction time of the ternary black powder and the sulfuric acid leaching agent is 2 to 4 hours, the reaction temperature is 60 to 80° C., and the pH value at the reaction end point is controlled at 2 to 3; the lithium ion concentration in the high-fluoride leaching solution is 10 to 25 g / L, 25 to 40 g / L, the fluoride ion concentration is 2 to 3 g / L, 3 to 4 g / L, and the aluminum ion concentration is 5 to 13 g / L.
[0016] In the step (2), the pH of the high-fluorine ternary battery leachate is adjusted to 4.3-4.7 with an alkaline reagent, preferably 4.4-4.5; the alkaline reagent can be one or more of liquid alkali, sodium carbonate, calcium hydroxide slurry, calcium oxide, calcium carbonate, etc., preferably calcium hydroxide and liquid alkali are used in combination; the reaction temperature is 60-90°C, and the reaction time is 30min-60min.
[0017] Calcium hydroxide can react with sulfate to form calcium sulfate. The solubility of calcium sulfate is very low, and the calcium ion concentration in the solution is low and equivalent to the original solution. Under the condition of almost no introduction of calcium ions, the combination of calcium hydroxide and liquid alkali can effectively control the amount of slag and use calcium sulfate as a filter medium to greatly accelerate the solid-liquid separation time. Fluoride is removed by using F and Al ions to form complexes, react to form precipitates such as Na3AlF6, and by using the adsorption and entrainment of the hydrolysis product Al(OH)3.
[0018] The washing process of the aluminum-fluorine slag and the leached slag in step (2) is as follows: washing with acidic water having a pH of 2 to 3 for 3 times, washing with ordinary water for 2 times, adjusting the pH of the ordinary water for the second washing to 2 to 3 and using it as acidic water for the next slag washing, and using the water from the two slag washings as water for leaching the ternary black powder raw material; the Li content in the leached slag after washing is less than 0.2%, the nickel content in the slag after washing the aluminum-fluorine slag is less than 0.5 to 0.7%, the cobalt content is less than 0.5%, and the manganese content is less than 0.1%.
[0019] In the step (3), the defluorination resin is a zirconium-based defluorination resin containing active zirconium groups, the injection rate of the aluminum defluorination leaching solution is 2 to 5 BV / h, the F concentration of the effluent is 0.5 to 2.5 mg / L, and the F concentration of the effluent increases slowly with the increase of the water treatment volume. When the fluorine concentration of the resin defluorination leaching solution flowing out of the resin reaches 10 mg / L, the defluorination resin is regenerated.
[0020] In the step (4), the pH of the defluoridation leaching solution is adjusted to 11-12 with an alkaline reagent. The alkaline reagent can be one or more of liquid caustic soda, calcium oxide, calcium hydroxide, sodium carbonate, calcium carbonate, etc. The reaction temperature is 25-65° C. and the reaction time is 30 min-60 min.
[0021] In the step (5), the nickel-cobalt-manganese slag is washed with ordinary water for 2 to 3 times, the Li content in the nickel-cobalt-manganese slag is much lower than 0.1%, the mass ratio of the nickel-cobalt-manganese washed slag to the leached washed slag is 8:1 to 12:1, and the nickel-cobalt-manganese leaching-extraction system is leached by reduction acid leaching, the reduction acid leaching uses sulfuric acid leaching, the reducing agent uses hydrogen peroxide, sodium pyrosulfite, sodium sulfite, etc., and the extracting agent uses P204, P507, etc.
[0022] The resin in step (6) is lithium hydroxide calcium and magnesium removal resin, the injection flow rate is 2 to 6 BV / h, the injection is carried out under alkaline conditions, and the injection pH is 11 to 12.
[0023] In the traditional black powder wet recovery process, low pH and high acid leaching are used in the acid leaching stage to obtain a higher metal leaching rate. A large amount of alkaline solution is required for precipitation and separation of nickel, cobalt and manganese during subsequent impurity removal. The separated nickel, cobalt and manganese precipitates require a large amount of acid for leaching, which greatly increases the acid and alkali consumption of this method. The applicant's experiments have proved that the sulfuric acid leaching method alone does not require a very low pH to achieve a leaching rate of Li of more than 99%, while low pH and leaching aids such as hydrogen peroxide are used to increase the leaching rate of high-valent nickel, cobalt and manganese in the black powder and oxidize the metal elements that are more difficult to leach, such as Cu. Therefore, the use of such reagents can be reduced in the process of leaching lithium from ternary black powder, saving costs.
[0024] The method used in the present invention uses sulfuric acid to leach lithium ions in the ternary black powder raw material leaching stage, and then nickel, cobalt and manganese need to be separated in the lithium extraction process. Therefore, there is no need to add sulfuric acid additionally, and leaching aids such as hydrogen peroxide and pyrochlore are used, which reduces the waste of sulfuric acid and leaching aids and the consumption of alkali solution when recovering nickel, cobalt and manganese. This method will allow some of the valuable metals that have not been leached to remain in the leaching residue, and the leaching residue can enter the nickel, cobalt and manganese recovery system together with the nickel, cobalt and manganese precipitation residue for leaching again. This method uses the high content of aluminum in the ternary black powder itself to remove fluorine, and does not use other aluminum-based and calcium-based defluorinating agents additionally. It removes fluorine while removing aluminum impurities itself. The defluorination effect is stable and can reduce F to 100-200 mg / L. The defluorination effect is generally the same as the defluorination effect of adding additional defluorinating agents, which is much better than the defluorination effect of adding activated alumina and aluminum hydroxide adsorbents, thereby saving costs and improving defluorination efficiency. After that, the defluorination resin is used to further defluorinate in depth to achieve two open circuits of fluorine in the raw material, avoiding fluorine from entering the subsequent nickel, cobalt and manganese leaching-extraction system.
[0025] The present invention provides a method for removing fluorine, removing weight and extracting lithium from high-fluorine battery black powder leachate, which has the following advantages:
[0026] (1) The present invention uses sulfuric acid leaching to leach ternary black powder. Under the condition of achieving a high lithium leaching rate, the consumption of auxiliary materials such as sulfuric acid, hydrogen peroxide, and sodium pyrosulfite is reduced, and the consumption of alkali solution in the aluminum removal and nickel, cobalt, and manganese precipitation steps is greatly reduced. The leached residue can be entered into the nickel, cobalt, and manganese recovery system together with the nickel, cobalt, and manganese precipitation residue for re-leaching to achieve full leaching of nickel, cobalt, and manganese.
[0027] (2) The present invention is mainly aimed at the defluorination of high-fluorine battery black powder leaching raw material liquid with a F content of 2 to 4 g / L. It is difficult to effectively reduce the F content to below 10 mg / L using a single defluorination agent, chemical precipitation method, or resin adsorption. A two-stage defluorination method combining precipitation adsorption and ion exchange is used to effectively reduce the F content of the high-fluorine battery black powder leaching raw material to below 10 mg / L.
[0028] (3) The present invention utilizes the Al element in the ternary black powder to remove impurities and fluorine at the same time with calcium hydroxide-liquid alkali, without the need to introduce other defluorinating agents and aluminum-calcium adsorbents, thereby greatly reducing the cost of defluorinating and the amount of slag. The defluorinating circuit opens the way to aluminum slag and resin, thus preventing fluorine from entering the subsequent nickel-cobalt-manganese leaching-extraction system.
[0029] (4) The present invention removes fluorine and extracts lithium without introducing other ionic impurities such as chlorine, phosphorus, iron, etc., which is green and environmentally friendly; the lithium extraction process adopts chemical precipitation-ion exchange method, and the impurity content of the obtained lithium liquid is low, thus avoiding the loss of lithium in extraction and separation, and can be used to prepare low-fluorine battery-grade lithium carbonate. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a process flow chart for removing fluorine, de-heavyness and extracting lithium from black powder leachate of high-fluorine battery in the present invention;
[0031] Figure 2 The aluminum-fluoride removal effect diagram of different alkaline reagents corresponding to the aluminum-fluoride slag filtration time, fluoride removal effect, and slag weight in Examples 1, 3, and 4 of the present invention. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described in more detail below in combination with the embodiments of the present invention and related drawings. However, the described embodiments are only a part of the present invention, not all of it, and the scope of protection of the present invention is not limited thereto.
[0033] Example 1
[0034] (1) Mix the ternary black powder and the leaching water to form a slurry. The leaching water for the black powder is aluminum fluoride slag and leaching slag washing water. Then, the reaction temperature is controlled at 70°C. Concentrated sulfuric acid is added to the slurry to control the pH of the reaction system and the reaction end point to 2. The reaction time is 3h. After the reaction, the high-fluoride leaching liquid and the leaching slag are filtered out, and the leaching slag is washed with water. (2) The high-fluoride leaching liquid is adjusted to a pH of 4.5 with a mixed slurry prepared with 100mL of liquid alkali and 10g of calcium hydroxide. The reaction temperature is 80°C and the reaction is carried out for 30min. After the reaction, the aluminum fluoride removal leaching liquid and aluminum fluoride slag are filtered out, and the aluminum fluoride slag is washed with water. (3) The aluminum fluoride removal leaching liquid enters the zirconium-based defluorination resin at a rate of 3BV / h. The initial F concentration of the resin defluorination leaching liquid is 1.4mg / L. When the F concentration of the effluent is 10mg / L, the resin is regenerated. (4) Adding liquid alkali to adjust the pH of the resin defluorination leachate to 11, the reaction temperature is 50°C, the reaction time is 30 minutes, filtering to obtain lithium extraction liquid and nickel-cobalt-manganese slag, and washing the nickel-cobalt-manganese slag with water. (5) The lithium extraction liquid enters the calcium-magnesium removal resin at 4BV / h to obtain a refined lithium hydroxide solution, and sodium carbonate is added to the refined lithium hydroxide solution to precipitate lithium to prepare lithium carbonate. (6) The nickel-cobalt-manganese slag is washed with ordinary water twice. The Li content in the nickel-cobalt-manganese slag is far less than 0.1%. The mass ratio of the nickel-cobalt-manganese washed slag to the leached washed slag is 10:1 and enters the nickel-cobalt-manganese leaching-extraction system, leaching with sulfuric acid and hydrogen peroxide, P204 for impurity removal, and P507 for separation of nickel and cobalt.
[0035] The washing process of aluminum-fluorine slag and leached slag in step (2) is as follows: washing with acidic water with a pH of 2-3 for 3 times, washing with ordinary water for 2 times, adjusting the pH of the ordinary water for the second washing to 2-3 and using it as acidic water for the next washing, and using the two washing waters for leaching ternary black powder raw materials; the content of Li in the leached slag after washing is less than 0.2%, the content of nickel in the slag after washing is less than 0.5-0.7%, the content of cobalt is less than 0.5%, and the content of manganese is less than 0.1%. The content of fluorine in the nickel-cobalt-manganese leaching solution in step (6) is less than 10 mg / L.
[0036] The element content of the material in the process of removing fluorine, extracting lithium and removing impurities from the high-fluorine leachate in Example 1 was detected, and the leaching rate of each element and the fluorine removal effect were calculated. The final results are shown in the following table.
[0037] Table 1 Data table of element contents in the process of removing fluorine, extracting lithium and removing impurities from high fluorine leaching solution in Example 1
[0038] Test items Co Ni Li Mn Al Cu Ca F High fluoride leaching solution g / L 19.87 13.40 12.78 12.41 7.24 0.0004 0.39 3158mg / L Leaching rate% 91.25 89.75 99.68 99.64 99.70 0.01 45.41 99.8 Aluminum and fluoride removal leaching solution g / L 21.47 14.27 14.67 14.44 0.064 0.0001 0.47 128mg / L Resin defluorination leaching liquid g / L 21.57 14.44 14.54 14.68 0.007 0.0002 0.44 1.4mg / L Lithium extraction solution g / L 0.0001 0.0001 15.77 0.0002 0.0010 0.0002 0.024 4.8mg / L Refined lithium hydroxide g / L 0.0001 0.0001 16.08 0.0001 0.0006 0.0001 0.0002 4.1mg / L
[0039] Example 2
[0040] (1) The same as the steps in (1) of Example 1. (2) The pH of the high-fluorine leachate is adjusted to 4.5 with a mixed slurry prepared with 50 mL of liquid caustic soda and 20 g of calcium hydroxide, the reaction temperature is 65°C, the reaction is carried out for 30 minutes, and after the reaction is completed, the aluminum-fluoride-removing leachate and aluminum-fluoride slag are filtered to obtain the aluminum-fluoride-removing leachate and aluminum-fluoride slag, and the aluminum-fluoride slag is washed with water. (3) The aluminum-fluoride-removing leachate is introduced into the zirconium-based defluoridation resin at a rate of 4BV / h, and the initial F concentration of the effluent is 2.2 mg / L. When the F concentration of the effluent is 10 mg / L, the resin is regenerated. (4) Liquid caustic soda is added to adjust the pH of the resin defluoridation leachate to 11, the reaction temperature is 60°C, the reaction time is 30 minutes, and the lithium extraction liquid and nickel-cobalt-manganese slag are filtered to obtain the nickel-cobalt-manganese slag, and the nickel-cobalt-manganese slag is washed with water. (5) The lithium extraction liquid is introduced into the calcium-magnesium removal resin at 3BV / h to obtain a refined lithium hydroxide solution, and sodium carbonate is added to the refined lithium hydroxide solution to precipitate lithium to prepare lithium carbonate. (6) The nickel-cobalt-manganese slag is washed with ordinary water for 3 times, and the Li content in the nickel-cobalt-manganese slag is less than 0.05%. The mass ratio of the nickel-cobalt-manganese washed slag to the leached washed slag is 12:1. The slag enters the nickel-cobalt-manganese leaching-extraction system, and is leached with sulfuric acid, hydrogen peroxide, and sodium metabisulfite. P204 is used for impurity removal, and P507 is used for nickel and cobalt separation.
[0041] The element content of the materials in the process of removing fluorine, extracting lithium and removing impurities from the high-fluorine leachate in Example 2 was tested, and the results are shown in the following table.
[0042] Table 2 Data table of element contents in the process of removing fluorine, extracting lithium and removing impurities from high fluorine leaching solution in Example 2
[0043] Test items Co Ni Li Mn Al Cu Ca F Aluminum and fluoride removal leaching solution g / L 20.66 13.80 13.54 14.14 0.094 0.0002 0.49 237mg / L Resin defluorination leaching liquid g / L 20.47 14.04 13.34 13.88 0.010 0.0002 0.43 2.2mg / L Lithium extraction solution g / L 0.0001 0.0001 14.77 0.0001 0.002 0.0002 0.044 5.8mg / L Refined lithium hydroxide g / L 0.0001 0.0001 15.08 0.0001 0.0008 0.0001 0.0001 4.6mg / L
[0044] Example 3
[0045] (1) The same as step (1) in Example 1. (2) The pH of the high-fluorine leachate is adjusted to 4.5 with liquid alkali, the reaction temperature is 80°C, the reaction is carried out for 50 minutes, and after the reaction is completed, the aluminum-fluoride-removing leachate and aluminum-fluoride slag are filtered to obtain the aluminum-fluoride-removing leachate and aluminum-fluoride slag, and the aluminum-fluoride slag is washed with water. (3) The aluminum-fluoride-removing leachate enters the zirconium-based defluoridation resin at a rate of 4BV / h, and the initial F concentration of the effluent is 1 mg / L. When the F concentration of the effluent is 10 mg / L, the resin is regenerated. (4) Liquid alkali is added to adjust the pH of the resin defluoridation leachate to 12, the reaction temperature is 50°C, the reaction time is 30 minutes, and the lithium extraction solution and nickel-cobalt-manganese slag are filtered to obtain the nickel-cobalt-manganese slag, and the nickel-cobalt-manganese slag is washed with water. (5) and (6) are the same as steps (5) and (6) in Example 1.
[0046] The element content of the materials in the process of removing fluorine, extracting lithium and removing impurities from the high-fluorine leachate in Example 3 was tested, and the results are shown in the following table.
[0047] Table 3 Data table of element contents in the process of removing fluorine, extracting lithium and removing impurities from high fluorine leaching solution in Example 3
[0048]
[0049]
[0050] Example 4
[0051] (1) Mix the ternary black powder and the leaching water to form a slurry. The leaching water for the black powder is aluminum fluoride slag and leaching slag washing water. Then, the reaction temperature is controlled at 60°C. Concentrated sulfuric acid is added to the slurry to control the pH of the reaction system and the reaction end point to 3. The reaction time is 2h. After the reaction, the high-fluorine leaching liquid and the leaching slag are filtered out, and the leaching slag is washed with water. (2) The pH of the high-fluorine leaching liquid is adjusted to 4.5 with calcium hydroxide slurry. The reaction temperature is 80°C and the reaction is carried out for 30 minutes. After the reaction, the aluminum fluoride-removing leaching liquid and aluminum fluoride slag are filtered out, and the aluminum fluoride slag is washed with water. (3) The aluminum fluoride-removing leaching liquid enters the zirconium-based fluoride-removing resin at a rate of 3BV / h. The initial F concentration of the effluent is 2mg / L. When the F concentration of the effluent is 10mg / L, the resin is regenerated. (4), (5), and (6) are the same as steps (4), (5), and (6) in Example 1.
[0052] The element content of the materials in the process of removing fluorine, extracting lithium and removing impurities from the high-fluorine leachate in Example 4 was tested, and the results are shown in the following table.
[0053] Table 4 Data table of element contents in the process of removing fluorine, extracting lithium and removing impurities from high fluorine leaching solution in Example 4
[0054] Test items Co Ni Li Mn Al Cu Ca F High fluoride leaching solution g / L 18.27 12.10 12.75 12.53 7.22 0.0004 0.43 2758mg / L Leaching rate% 89.95 86.15 99.57 99.54 99.66 0.01 56.14 99.72 Aluminum and fluoride removal leaching solution g / L 19.77 13.17 14.18 13.84 0.18 0.0001 0.58 208mg / L Resin defluorination leaching liquid g / L 19.58 12.99 14.04 13.88 0.087 0.0002 0.56 2mg / L Lithium extraction solution g / L 0.0001 0.0001 14.57 0.0001 0.0094 0.0002 0.11 6.7mg / L Refined lithium hydroxide g / L 0.0001 0.0001 14.48 0.0001 0.0010 0.0001 0.0007 4.1mg / L
[0055] Example 5
[0056] (1) Same as Example (1). (2) The pH of the high-fluorine leachate is adjusted to 4.4 with liquid alkali, the reaction temperature is 60°C, the reaction is carried out for 30 minutes, and after the reaction is completed, the aluminum-fluoride-removing leachate and aluminum-fluoride slag are filtered to obtain the aluminum-fluoride-removing leachate and aluminum-fluoride slag, and the aluminum-fluoride slag is washed with water. (3) The aluminum-fluoride-removing leachate enters the zirconium-based fluoride-removing resin at a rate of 3BV / h, and the initial F concentration of the effluent is 2 mg / L. When the F concentration of the effluent is 10 mg / L, the resin is regenerated. (4) and (5) are the same as steps (4) and (5) in Example 1. (6) Except for the use of Cyanex272 for nickel-cobalt separation, the other conditions are the same as in Example 1.
[0057] From Examples 1-5, Figure 2It can be seen that for the above-mentioned high-fluorine ternary black powder leachate, there is no need to add additional defluorinating agents and adsorbing defluorinating agents such as activated alumina. The higher Al content in the solution can achieve better defluorination effect, reducing the fluorine content to 100-200 mg / L, and the liquid alkali has better effect on removing Al and F than calcium hydroxide, and the defluorination effect is better as the temperature increases. Although sodium hydroxide has a better effect on removing aluminum and fluorine, there is a long solid-liquid separation time. The combination of sodium hydroxide and calcium hydroxide can increase the filtration speed. After the steps of resin defluorination, precipitation separation of nickel, cobalt and manganese, and calcium and magnesium removal, the impurity content in the refined lithium liquid is very low, which effectively achieves deep defluorination and impurity removal to complete lithium extraction.
[0058] In summary, the present invention ensures the leaching rate of lithium during leaching, lithium extraction and impurity removal, reduces the consumption of leaching agents such as sulfuric acid, hydrogen peroxide, sodium pyrosulfite, and the consumption of alkali solution when recovering nickel, cobalt and manganese, and greatly reduces the consumption of auxiliary materials compared to the traditional method of full leaching of metals and then impurity removal and separation. The defluorination adopts a two-stage defluorination, combining the advantages of chemical precipitation and resin adsorption. The first stage utilizes the defluorination mechanism of Al itself in the high-fluorine leachate, replacing the use of traditional defluorinating agents and alumina adsorbents, saving costs, reducing slag volume, and improving defluorination efficiency. The second stage uses a defluorination resin to further defluorinate in depth, realizing two open circuits of fluorine in the battery black powder raw material, effectively preventing fluorine from entering the subsequent nickel, cobalt and manganese leaching-extraction system. This method has the advantages of green economy, safety and environmental protection, deep defluorination, and good lithium extraction and impurity removal effects.
[0059] The above content describes the technical principles, beneficial effects and features of the present invention. It should be pointed out that the above is only a preferred implementation mode of the present invention, but is not limited to the above embodiments. For technicians in the technical field to which the present invention belongs, some improvements and optimizations can be made without departing from the content of the present invention, which should be regarded as belonging to the protection scope of the present invention.
Claims
1. A method for removing fluorine and heavy metal from high-fluorine battery black powder leachate to extract lithium, characterized in that: The specific steps are as follows: (1) reacting ternary black powder with a sulfuric acid leaching agent, adjusting the pH at the reaction endpoint, and separating the solid and liquid after the reaction to obtain a high-fluorine leaching solution and leaching residue; (2) adjusting the pH of the high-fluorine leachate with an alkaline reagent to remove Al and F, filtering to obtain an aluminum-fluoride-removed leachate and aluminum-fluoride slag, and washing the aluminum-fluoride slag and the leachate slag in step (1) with water respectively; (3) the aluminum-fluoride-removing leaching solution is introduced into a defluorination resin for defluorination to obtain a resin defluorination leaching solution; (4) adding alkaline reagent to adjust the pH of the resin defluorination leachate to recover Ni, Co, and Mn, and filtering to obtain lithium extraction solution and nickel-cobalt-manganese slag; (5) washing the nickel-cobalt-manganese slag to obtain nickel-cobalt-manganese washed slag, mixing the nickel-cobalt-manganese washed slag with the leaching slag washed slag in proportion and entering into the nickel-cobalt-manganese leaching-extraction system to remove impurities and separate nickel, cobalt and manganese; (6) The lithium extraction solution is passed through a calcium and magnesium removal resin for deep impurity removal to obtain a refined lithium hydroxide solution, and sodium carbonate is added to the refined lithium hydroxide solution to precipitate lithium for the preparation of lithium carbonate.
2. The method for removing fluorine and heavy metal from a high-fluorine battery black powder leachate according to claim 1, characterized in that: The ternary black powder in step (1) is a positive electrode material containing an aluminum current collector or a positive and negative electrode material containing a current collector.
3. The method for removing fluorine and heavy metal from a high-fluorine battery black powder leachate according to claim 1, characterized in that: In the step (1), the reaction time of the ternary black powder and the sulfuric acid leaching agent is 2-4 hours, the reaction temperature is 60-80° C., and the pH value at the reaction end point is controlled at 2-3; the lithium ion concentration in the high-fluoride leaching solution is 10-25 g / L or 25-40 g / L, the fluoride ion concentration is 2-3 g / L or 3-4 g / L, and the aluminum ion concentration is 5-13 g / L.
4. The method for removing fluorine and heavy metal from a high-fluorine battery black powder leachate as claimed in claim 1, characterized in that: In the step (2), the high-fluoride leaching solution is adjusted to a pH of 4.3-4.7 using an alkaline reagent; the alkaline reagent can be one or more of liquid caustic soda, sodium carbonate, calcium hydroxide slurry, calcium oxide, and calcium carbonate; the reaction temperature is 60-90° C., and the reaction time is 30 min-60 min.
5. The method for removing fluorine and heavy metal from high-fluorine battery black powder leachate according to claim 1, characterized in that: The washing process of the aluminum-fluorine slag in step (2) and the leached slag in step (1) is as follows: washing with acidic water having a pH of 2-3 for 3 times, washing with ordinary water for 2 times, adjusting the pH of the ordinary water for the second washing to 2-3 and using it as acidic water for the next slag washing, and using the water from the two slag washings as water for leaching the ternary black powder raw material; after the leached slag is washed with water, the Li content in the slag is less than 0.2%, and after the aluminum-fluorine slag is washed with water, the nickel content in the slag is less than 0.5-0.7%, the cobalt content is less than 0.5%, and the manganese content is less than 0.1%.
6. The method for removing fluorine and heavy metal from a high-fluorine battery black powder leachate according to claim 1, characterized in that: The defluorination resin in step (3) is a zirconium-based defluorination resin containing active zirconium groups, the injection rate of the aluminum defluorination leaching solution is 2-5 BV / h, the F concentration of the effluent is 0.5-2.5 mg / L, and the F concentration of the effluent increases slowly with the increase of the water treatment volume. When the fluorine concentration of the resin defluorination leaching solution flowing out of the resin reaches 10 mg / L, the defluorination resin is regenerated.
7. The method for removing fluorine and heavy metal from a high-fluorine battery black powder leachate as claimed in claim 1, characterized in that: In the step (4), the pH of the defluoridation leaching solution is adjusted to 11-12 using an alkaline reagent. The alkaline reagent can be one or more of liquid caustic soda, sodium carbonate, calcium oxide, calcium hydroxide, and calcium carbonate. The reaction temperature is 25-65° C. and the reaction time is 30 min-60 min.
8. The method for removing fluorine and heavy metal from a high-fluorine battery black powder leachate as claimed in claim 1, characterized in that: In the step (5), the nickel-cobalt-manganese slag is washed with ordinary water for 3 to 4 times, and the Li content of the slag after the nickel-cobalt-manganese washing is less than 0.1%.
9. The method for removing fluorine and heavy metal from a high-fluorine battery black powder leachate according to claim 1, characterized in that: In the step (5), the nickel-cobalt-manganese washed slag and the leached washed slag are mixed in a mass ratio of 8:1 to 12:1 and then introduced into the nickel-cobalt-manganese leaching-extraction system; the leaching is carried out by reducing acid leaching, the reducing acid leaching uses sulfuric acid leaching, the reducing agent uses one or more of hydrogen peroxide, sodium pyrosulfite, sodium sulfite, etc., and the extraction uses P204, P507 extraction agent.
10. The method for removing fluorine and heavy metal from a high-fluorine battery black powder leachate according to claim 1, characterized in that: In the step (6), the calcium-magnesium-removing resin is lithium hydroxide calcium-magnesium-removing resin, the injection flow rate is 2-6 BV / h, the injection is carried out under alkaline conditions, and the injection pH is 11-12.
Citation Information
Cited By
Method for recovering metal from battery positive electrode black powder and removing impurities by using eutectic solvent
CN119932321A
Impurity removal method for ternary black powder leachate
CN120666178A
Method for removing fluorine in ternary waste recovery process
CN122542829A
Progressive liquid-solid ratio convergence judgment method for content of water-soluble fluorine in lithium battery black powder
CN122567795A