Preparation method of aluminum alloy strip and aluminum alloy strip
Through casting, refining, degassing, cold rolling and annealing processes, combined with the edge quality control of vertical slitting machine, the problems of low tensile strength and poor surface quality of the power battery aluminum alloy strip are solved, and excellent mechanical performance is achieved and the improvement of high-frequency welding performance.
Patent Information
- Application Number
- CN202411152869.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
AI Technical Summary
The existing power battery aluminum alloy strips have low tensile strength and poor surface quality, which cannot meet the high-frequency welding requirements of power battery shells.
The cast-rolling blanks were prepared by casting and rolling. Through multiple refining, degassing, filtration and cold rolling processes, combined with complete and incomplete recrystallization annealing, the rolling lubricant was designed and optimized, and the edge quality control was used for vertical slitting machine. , an aluminum alloy strip with a thickness of 0.3 to 0.5 mm was prepared.
The tensile strength of aluminum alloy strips has been improved to 210~240MPa, the surface quality is uniform and delicate, the aluminum powder peels off less, the cleanliness is high, and the technical requirements of high-frequency welding, the cutting edge quality is excellent, the burr direction is uniformly facing the inner side of the coil material, the edge is The partial shear rate is ≥80%.
Smart Images

Figure CN119040674A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum processing, and in particular to a preparation method of an aluminum alloy strip used for a power battery casing and the aluminum alloy strip. Background Art
[0002] Developing new energy vehicles is an important measure to cope with the current climate change and promote green development. Pure electric vehicles driven by power batteries have received unanimous praise from users. The power battery is small in size, light in weight, and has a long battery life. The advantages of general batteries come from innovative structures. The battery is small in size and light in weight, which can bring better space performance to the vehicle, while reducing its own resistance, reducing power consumption, and further improving the mileage.
[0003] Existing power batteries are essentially lithium iron phosphate batteries. By processing traditional cylindrical single cells into long, thin, sheet-like single cells, the battery volume utilization rate is higher, more battery cells can be accommodated, the volume energy density is increased, and the cruising range is greatly improved.
[0004] However, existing single cylindrical batteries usually produce too many gaps between batteries through stacking, which increases production costs; at the same time, traditional lithium iron phosphate battery casings are produced using hot-rolled materials, and the resulting aluminum alloy strips have low tensile strength, poor surface quality, and color differences that do not meet requirements. Summary of the invention
[0005] The purpose of the embodiment of the present invention is to provide a method for preparing an aluminum alloy strip, so as to solve the problem that the existing aluminum alloy strip used in the aluminum shell of a power battery has low tensile strength and poor surface quality.
[0006] In order to solve the above technical problems, in a first aspect, an embodiment of the present invention provides a method for preparing an aluminum alloy strip, the preparation method comprising the following steps:
[0007] Step S1, according to the following components and mass percentages: Si 0.50-0.60%, Fe 0.65-0.75%, Cu 0.25-0.35%, Mg ≤ 0.001%, Mn 0.95-1.25%, Ti 0.025-0.035%, Al as the balance, mass fraction Fe / Si = 1.2-1.5, a casting and rolling method is used to prepare a cast-rolled billet; specifically comprising the steps of:
[0008] Step S11, selecting elements Fe, Si, Mn, and Ti to prepare alloy elements according to the above mass fractions, wherein Fe adopts 80Fe agent with potassium fluoroaluminate as flux, Si adopts quick-dissolving silicon, Cu adopts AlCu50 master alloy, and Mn adopts 80Mn agent additive supplement; Ti is added in a manner including adding titanium blocks in an amount of 1kg / t in the pouring furnace launder during pouring and adding a single aluminum titanium boron wire grain refiner online, and the remaining alloys are not prepared and added separately, and smelting is performed to obtain aluminum liquid;
[0009] Step S12, stirring the aluminum liquid evenly, transferring the aluminum liquid into a holding furnace for first refining, allowing the aluminum liquid to stand after refining, and then skimming to obtain first refined aluminum liquid;
[0010] Step S13, adding metal additives to the first refined aluminum liquid, and then performing a second refining, and after the refining is completed, the aluminum liquid is allowed to stand, and then slag is removed and the furnace is poured to obtain a second refined aluminum liquid;
[0011] Step S14, the aluminum liquid refined for the second time is refined for the third time, and after the refining is completed, slag removal, degassing, filtering and casting are carried out in sequence, and the holding furnace is refined once every 4 hours to obtain a cast-rolled billet with a thickness of 6.0-7.0 mm;
[0012] Step S2, transferring the cast-rolled billet to each cold rolling process, and outputting a cold-rolled finished thickness strip;
[0013] Specifically, it comprises the steps of: cold rolling the cast-rolled billet to an intermediate pass thickness, performing complete recrystallization or incomplete recrystallization annealing, and cold rolling the strip after annealing to a finished thickness strip to obtain a cold-rolled strip;
[0014] Step S3, cutting the cold-rolled strip into finished products through a vertical slitting machine to obtain finished strips with a thickness of 0.3 to 0.5 mm; wherein the side curvature of the finished strip is less than 0.04 mm / m.
[0015] Preferably, the first refining, the second refining and the third refining are all performed by refining with argon gas and a granular refining agent.
[0016] Preferably, in the steps S12-S14, a granular refining agent is used for refining, and the full furnace is refined at 10-15 kg / time, and 100±20 kg of cold material is added; the half furnace is refined at 5 kg / time, and 80±20 kg of cold material is added; after 3 hours, 5 sample plates are added to each of the two furnace doors without refining; the casting and rolling speed is 860-900 mm / min, and the aluminum liquid temperature of the front box is 698±2°C; and the slag is removed once every hour.
[0017] Preferably, in step S14, the flame spraying parameters of casting and rolling include the spraying running speed, the horizontal height of the barrel and the width of the gun tip beyond the edge of the strip; wherein, the spraying running speed is 8±2s for one way, the horizontal height of the barrel is 20-25cm below the center line of the roll, and the distance between the gun tip and the roll is 10±1cm; the width of the gun tip beyond the edge of the strip is 2±1cm; the casting and rolling speed is 860-900mm / min, and the aluminum water temperature of the front box is 698±2℃; and the slag is removed once every hour.
[0018] Preferably, the step S2 specifically comprises: firstly performing homogenization annealing on the cast-rolled billet, and the annealing process is kept at 510-520°C for 3-4 hours; then cold rolling to an intermediate billet thickness of 2.8-3.2 mm for intermediate annealing, and the annealing process is a metal temperature of 450-460°C, and the heat preservation is 1.5-2.5 hours to obtain a completely recrystallized structure; and cold rolling is continued to be rolled to a finished product thickness of 0.3-0.5 mm; wherein, from the cast-rolled billet rolling to the cold-rolled finished product thickness, the total cold rolling processing rate is controlled within 85-92%.
[0019] Preferably, the step S2 specifically further includes: the cast-rolled billet is rolled to an intermediate billet thickness of 0.6 to 1.2 mm, and an intermediate incomplete recrystallization annealing is performed to obtain an aluminum alloy strip in H24 state, the annealing process is a metal material temperature of 400 to 410° C. and insulation for 2.0 to 3.0 hours, and the tensile strength of the intermediate billet is obtained to be 170 to 175 MPa; and then cold rolling is continued to be rolled to a finished product thickness of 0.3 to 0.5 mm; wherein, from the cast-rolled billet to the cold-rolled finished product thickness, the total cold rolling processing rate is controlled within 50-60%.
[0020] Preferably, the step S2 specifically further includes: rolling the cast-rolled billet to an intermediate billet thickness of 0.4 to 0.65 mm, performing intermediate incomplete recrystallization annealing to obtain an aluminum alloy strip in H26 state, the annealing process is that the metal material temperature is 360 to 370°C, and the heat preservation is 2.0 to 3.0 hours, and the tensile strength of the intermediate billet is 180 to 185 MPa; and then cold rolling to a finished product thickness of 0.3 to 0.5 mm; wherein, from the cast-rolled billet rolling to the cold-rolled finished product thickness, the total cold rolling processing rate is controlled within 25-30%.
[0021] Preferably, in step S2, the cold rolling oil base oil adopts a dearomatized solvent oil model D105-110 base oil with a viscosity of 2.5 to 2.7 mm 2 / s; a rolling lubricant is obtained by adding an ester and alcohol composite additive to a base oil; the hydroxyl value of the rolling lubricant is controlled at 22-26 mgKOH / g, and the saponification value is controlled at 2.8-3.6 mgKOH / g; the ratios of the ester and alcohol composite additives in the rolling lubricant are 1.25±0.05% and 8.75±0.05%, respectively.
[0022] Preferably, in step S3, the edge trimming quality requirements are that the horizontal burr is ≤0.1mm, the vertical burr is ≤0.015mm, and the burr direction is uniformly toward the inside of the coil, and the edge shear rate is ≥80%, wherein the edge shear rate refers to the edge blade shear thickness of the vertical slitting machine after slitting accounts for ≥80% of the total thickness of the strip, and the tear thickness accounts for <20% of the strip thickness.
[0023] In a second aspect, the present invention provides an aluminum alloy strip, which is made by the above-mentioned method for preparing an aluminum alloy strip, and the aluminum alloy strip is used to manufacture an aluminum shell of a power battery.
[0024] Compared with the prior art, the preparation method of the aluminum alloy strip in the present invention can obtain the cold-rolled strip with excellent mechanical properties, uniform and fine surface quality, less aluminum powder peeling and high cleanliness through the production process design of casting and rolling smelting, refining, degassing and deslagging, rolling mill process, complete recrystallization in the middle of cold rolling and incomplete intermediate annealing process and rolling process, and lubricating performance design of cold rolling lubricating oil; at the same time, through the innovative edge quality control technology of the vertical slitting machine, the high-frequency welding technical requirements are met; in addition, the aluminum alloy strip has a thickness of 0.3-0.5 mm, a tensile strength of 210-240 MPa, and a Vickers hardness value of HV55-65; the surface quality is excellent, without defects such as color difference and bright lines; its trimming quality requires that the burr in the horizontal direction (i.e., parallel to the width direction) is ≤0.1 mm, the burr in the vertical direction (i.e., vertical to the width direction) is ≤0.015 mm, and the burr direction is uniformly toward the inside of the coil, and the edge shear rate is ≥80%. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:
[0026] Figure 1 The present invention provides a flowchart of a method for preparing an aluminum alloy strip according to an embodiment of the present invention. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Embodiment 1
[0029] Please see attached Figure 1 As shown, an embodiment of the present invention provides a method for preparing an aluminum alloy strip, and the preparation method comprises the following steps:
[0030] Step S1, according to the following components and mass percentages: Si 0.50-0.60%, Fe 0.65-0.75%, Cu 0.25-0.35%, Mg ≤ 0.001%, Mn 0.95-1.25%, Ti 0.025-0.035%, Al as the balance, mass fraction Fe / Si = 1.2-1.5. A casting and rolling method is used to prepare a casting and rolling billet; specifically comprising the following steps:
[0031] Step S11, selecting elements Fe, Si, Mn, and Ti to prepare alloy elements according to the above mass fractions, wherein Fe adopts 80Fe agent with potassium fluoroaluminate as flux, Si adopts quick-dissolving silicon, Cu adopts AlCu50 master alloy, and Mn adopts 80Mn agent additive supplement; Ti is added in a manner including adding titanium blocks in an amount of 1kg / t in the pouring furnace launder during pouring and adding a single aluminum titanium boron wire grain refiner online, and the remaining alloys are not prepared and added separately; and smelting is performed to obtain aluminum liquid;
[0032] Step S12, stirring the aluminum liquid evenly, transferring the aluminum liquid into a holding furnace for first refining, allowing the aluminum liquid to stand after refining, and then skimming to obtain first refined aluminum liquid;
[0033] Step S13, adding metal additives to the first refined aluminum liquid, and then performing a second refining, and after the refining is completed, the aluminum liquid is allowed to stand, and then slag is removed and the furnace is poured to obtain a second refined aluminum liquid;
[0034] Step S14, the aluminum liquid refined for the second time is refined for the third time, and after the refining is completed, slag removal, degassing, filtering and casting are carried out in sequence, and the holding furnace is refined once every 4 hours to obtain a cast-rolled billet with a thickness of 6.0-7.0 mm;
[0035] Step S2, transferring the cast-rolled billet to each cold rolling process, and outputting a cold-rolled finished thickness strip;
[0036] Specifically, it comprises the steps of: cold rolling the cast-rolled billet to an intermediate pass thickness, performing complete recrystallization or incomplete recrystallization annealing, and cold rolling the strip after annealing to a finished thickness strip to obtain a cold-rolled strip;
[0037] Step S3, cutting the cold-rolled strip into finished products through a vertical slitting machine to obtain finished strips with a thickness of 0.3 to 0.5 mm; wherein the side curvature of the finished strip is less than 0.04 mm / m.
[0038] Specifically, through the above steps S1 to S3, the cold-rolled strip can have excellent mechanical properties, uniform and fine surface quality, less aluminum powder peeling and high cleanliness through the production process design of casting and rolling smelting, refining, degassing and deslagging, rolling mill process, complete recrystallization in the middle of cold rolling, incomplete intermediate annealing process and rolling process, and lubricating performance design of cold rolling lubricating oil. At the same time, the innovative edge quality control technology of the vertical slitting machine can meet the high-frequency welding technical requirements. In addition, the aluminum alloy strip has a thickness of 0.3-0.5 mm, a tensile strength of 210-240 MPa, and a Vickers hardness value of HV 55-65; the surface quality is excellent, without defects such as color difference and bright lines; the trimming quality requires that the burr in the horizontal direction (i.e., parallel to the width direction) is ≤0.1 mm, the burr in the vertical direction (i.e., perpendicular to the width direction) is ≤0.015 mm, and the burr direction is uniformly toward the inside of the coil, and the edge shear rate is ≥80%.
[0039] In this embodiment, the first refining, the second refining and the third refining are all performed by argon gas plus granular refining agent, and the refining effect is good, and the obtained cast-rolled billet product is of high quality.
[0040] In this embodiment, in the steps S12-S14, granular refining agent is used for refining, and the full furnace is refined at 10-15 kg / time, and 100±20 kg of cold material is added; the half furnace is refined at 5 kg / time, and 80±20 kg of cold material is added; after 3 hours, 5 sample plates are added to each of the two furnace doors without refining; the casting and rolling speed is 860-900 mm / min, and the aluminum liquid temperature of the front box is 698±2°C; and the slag is removed once every hour.
[0041] Specifically, by removing slag once an hour in the degassing box, the argon hydrogen flash generated by the graphite rotor is obvious, and pure aluminum water is obtained. During the high-frequency welding of the power battery aluminum shell, there will be no defects such as pores and slag inclusions. The qualified rate of the battery shell can reach more than 99.6%, and the product quality is good.
[0042] In this embodiment, in step S14, the flame spraying parameters of casting and rolling include the spraying running speed, the horizontal height of the gun barrel, and the width of the gun tip beyond the edge of the strip; wherein the spraying running speed is 8±2s per trip, the horizontal height of the gun barrel is 20-25cm below the center line of the roll, the distance between the gun tip and the roll is 10±1cm; the width of the gun tip beyond the edge of the strip is 2±1cm; the casting and rolling speed is 860-900mm / min, the aluminum water temperature of the front box is 698±2℃; and the slag is removed once every hour. In this way, the lubrication of the flame spraying can be fully guaranteed, and the surface quality of the casting and rolling billet is excellent.
[0043] In this embodiment, the step S2 specifically includes: first homogenizing annealing the cast billet, the annealing process is 510-520℃ for 3-4 hours; then cold rolling to the intermediate billet thickness of 2.8-3.2mm for intermediate annealing, the annealing process is metal temperature 450-460℃, insulation for 1.5-2.5 hours, to obtain a completely recrystallized structure; continue cold rolling to 0.3-0.5mm finished product thickness; wherein, from the cast billet rolling to the cold rolled finished product thickness, the total cold rolling processing rate is controlled within 85-92%. In this way, a power battery aluminum shell aluminum alloy strip with excellent mechanical properties can be obtained, and the blasting test fully meets the customer's use requirements and fully guarantees the safety performance of the battery shell.
[0044] In this embodiment, the step S2 specifically includes: the cast-rolled billet is rolled to an intermediate billet thickness of 0.6-1.2 mm, and an intermediate incomplete recrystallization annealing is performed to obtain an aluminum alloy strip in the H24 state. The annealing process is a metal material temperature of 400-410°C for 2.0-3.0 hours, and the tensile strength of the intermediate billet is 170-175 MPa; and then cold rolling is continued to the finished product thickness of 0.3-0.5 mm; wherein, from the cast-rolled billet rolling to the cold-rolled finished product thickness, the total cold rolling processing rate is controlled within 50-60%. In this way, an aluminum alloy strip for a power battery aluminum shell with excellent mechanical properties can be obtained, and the blasting test fully meets the customer's use requirements and fully guarantees the safety performance of the battery shell.
[0045] In this embodiment, the step S2 specifically includes: the cast-rolled billet is rolled to an intermediate billet thickness of 0.4-0.65 mm, and an intermediate incomplete recrystallization annealing is performed to obtain an aluminum alloy strip in the H26 state. The annealing process is that the metal material temperature is 360-370°C, and the temperature is kept for 2.0-3.0 hours to obtain an intermediate billet with a tensile strength of 180-185 MPa; and then cold-rolled to a finished product thickness of 0.3-0.5 mm; wherein, from the cast-rolled billet to the cold-rolled finished product thickness, the total cold rolling processing rate is controlled within 25-30%. In this way, an aluminum alloy strip for a power battery aluminum shell with excellent mechanical properties can be obtained, and the blasting test fully meets the customer's use requirements and fully guarantees the safety performance of the battery shell.
[0046] In this embodiment, in step S2, the cold rolling rolling oil base oil adopts dearomatized solvent oil model D105-110 base oil with a viscosity of 2.5-2.7 mm2 / s; the rolling lubricant is obtained by adding ester and alcohol composite additives to the base oil; the hydroxyl value of the rolling lubricant is controlled at 22-26 mgKOH / g, and the saponification value is controlled at 2.8-3.6 mgKOH / g; the ratio of ester and alcohol composite additives in the rolling lubricant is 1.25±0.05% and 8.75±0.05% respectively. In this way, the rolling lubricant has excellent lubrication performance, the surface quality of the battery strip obtained by rolling is excellent, the color is uniform and delicate, and the amount of aluminum powder peeling is small.
[0047] The specific ratios of the ester and alcohol composite additives in the rolling lubricant are shown in Table 1 and Table 2 respectively;
[0048] Table 1. Types and parameters of esters in cold rolling oil
[0049] Ester type Saponification value (mgKOH / g) Proportional (±0.05%) Methyl dodecanoate 258 0.12 Methyl myristate 232 0.25 Methyl hexadecanoate 208 0.38 Methyl octadecanoate 203 0.50 All esters / 1.25
[0050] Table 2. Types and parameters of alcohol in cold rolling oil
[0051]
[0052]
[0053] It can be seen from Tables 1 and 2 above that the rolling lubricant has excellent lubrication performance, the battery strip obtained by rolling has excellent surface quality, uniform and fine color, and less aluminum powder peeling.
[0054] In this embodiment, in step S3, the trimming quality requirements are that the horizontal burr is ≤0.1mm, the vertical burr is ≤0.015mm, and the burr direction is uniformly toward the inside of the coil, and the edge shear rate is ≥80%, wherein the edge shear rate refers to the edge blade shear thickness of the vertical slitting machine after stripping accounts for ≥80% of the total strip thickness, and the tear thickness accounts for <20% of the strip thickness. Among them, the height of the edge trimming burr in the horizontal and vertical directions is within 0.05-0.08mm, and the shear rate can reach 84-85%. The above performance indicators fully meet the requirements of aluminum alloy strips for power battery aluminum shells.
[0055] Specifically, the edge trimming quality requires that the burr in the horizontal direction (i.e. parallel to the width direction) is ≤0.1mm, and the burr in the vertical direction (i.e. perpendicular to the width direction) is ≤0.015mm, and the burr direction is uniformly toward the inside of the coil. The edge shear rate is ≥80%, and the edge shear rate refers to the edge blade shear thickness after the slitting machine is slit to account for ≥80% of the total strip thickness, and the tear thickness accounts for <20% of the strip thickness, which can ensure the high-frequency welding performance of the strip edge, and there is no aluminum oxide compound in the welding. The edge of the aluminum alloy strip is sheared and rubbed with the disc knife blade, that is, the shear surface, which is a bright end face without burrs. The edge of the aluminum alloy strip that has not passed through the disc knife blade contact shear part is a tear surface. The tear surface is rough and uneven, and the aluminum oxide burrs are serious, which affects the high-frequency welding performance of the aluminum alloy strip.
[0056] Embodiment 2
[0057] The present invention provides an aluminum alloy strip, which is made by the aluminum alloy strip preparation method of the above-mentioned embodiment 1, and the aluminum alloy strip is used to manufacture an aluminum shell of a power battery.
[0058] Compared with the related art, the preparation method of the aluminum alloy strip in the present invention can obtain the cold-rolled strip with excellent mechanical properties, uniform and fine surface quality, less aluminum powder peeling and high cleanliness through the above-mentioned steps S1 to S3, through the production process design of casting and rolling smelting, refining, degassing and slag removal, rolling mill process, complete recrystallization in the cold rolling intermediate and incomplete intermediate annealing process and rolling process, and lubricating performance design of cold rolling lubricating oil. At the same time, through the innovative edge quality control technology of the vertical slitting machine, the high-frequency welding technical requirements are met; in addition, the aluminum alloy strip has a thickness of 0.3-0.5 mm, a tensile strength of 210-240 MPa, and a Vickers hardness value of HV 55-65; the surface quality is excellent, without defects such as color difference and bright lines; its trimming quality requires that the burr in the horizontal direction (i.e., parallel to the width direction) is ≤0.1 mm, the burr in the vertical direction (i.e., vertical to the width direction) is ≤0.015 mm, and the burr direction is uniformly toward the inside of the coil, and the edge shear rate is ≥80%.
[0059] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.
[0060] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing an aluminum alloy strip, characterized in that: The preparation method comprises the following steps: Step S1, according to the following components and mass percentages: Si 0.50-0.60%, Fe 0.65-0.75%, Cu 0.25-0.35%, Mg ≤ 0.001%, Mn 0.95-1.25%, Ti 0.025-0.035%, Al as the balance, mass fraction Fe / Si = 1.2-1.5, a casting and rolling method is used to prepare a cast-rolled billet; specifically comprising the steps of: Step S11, selecting elements Fe, Si, Mn, and Ti to prepare alloy elements according to the above mass fractions, wherein Fe adopts 80Fe agent with potassium fluoroaluminate as flux, Si adopts quick-dissolving silicon, Cu adopts AlCu50 master alloy, and Mn adopts 80Mn agent additive supplement; Ti is added in a manner including adding titanium blocks in an amount of 1kg / t in the pouring furnace launder during pouring and adding a single aluminum titanium boron wire grain refiner online, and the remaining alloys are not prepared and added separately, and smelting is performed to obtain aluminum liquid; Step S12, stirring the aluminum liquid evenly, transferring the aluminum liquid into a holding furnace for first refining, allowing the aluminum liquid to stand after refining, and then skimming to obtain first refined aluminum liquid; Step S13, adding metal additives to the first refined aluminum liquid, and then performing a second refining, and after the refining is completed, the aluminum liquid is allowed to stand, and then slag is removed and the furnace is poured to obtain a second refined aluminum liquid; Step S14, the aluminum liquid refined for the second time is refined for the third time, and after the refining is completed, slag removal, degassing, filtering and casting are carried out in sequence, and the holding furnace is refined once every 4 hours to obtain a cast-rolled billet with a thickness of 6.0-7.0 mm; Step S2, transferring the cast-rolled billet to each cold rolling process, and outputting a cold-rolled finished thickness strip; Specifically, it comprises the steps of: cold rolling the cast-rolled billet to an intermediate pass thickness, performing complete recrystallization or incomplete recrystallization annealing, and cold rolling the strip after annealing to a finished thickness strip to obtain a cold-rolled strip; Step S3, cutting the cold-rolled strip into finished products through a vertical slitting machine to obtain finished strips with a thickness of 0.3 to 0.5 mm; wherein the side curvature of the finished strip is less than 0.04 mm / m.
2. The method for preparing an aluminum alloy strip according to claim 1, characterized in that: The first refining, the second refining and the third refining are all performed by refining with argon gas and granular refining agent.
3. The method for preparing an aluminum alloy strip according to claim 2, characterized in that: In the steps S12-S14, granular refining agent is used for refining, and the full furnace is refined at 10-15 kg / time, and 100±20 kg of cold material is added; the half furnace is refined at 5 kg / time, and 80±20 kg of cold material is added; after 3 hours, 5 sample plates are added to each of the two furnace doors without refining; the casting and rolling speed is 860-900 mm / min, and the aluminum liquid temperature of the front box is 698±2°C; slag is removed once every hour.
4. The method for preparing an aluminum alloy strip according to claim 1, wherein: In the step S14, the flame spraying parameters of the casting and rolling include the spraying running speed, the horizontal height of the barrel and the width of the gun tip beyond the edge of the strip; wherein the spraying running speed is 8±2s for one way, the horizontal height of the barrel is 20-25cm below the center line of the roll, the distance between the gun tip and the roll is 10±1cm; the width of the gun tip beyond the edge of the strip is 2±1cm; the casting and rolling speed is 860-900mm / min, the aluminum water temperature of the front box is 698±2℃; and the slag is removed once every hour.
5. The method for preparing an aluminum alloy strip according to claim 1, characterized in that: The step S2 specifically includes: firstly performing homogenization annealing on the cast-rolled billet, and the annealing process is 510-520°C for 3-4 hours; then cold rolling to an intermediate billet thickness of 2.8-3.2 mm for intermediate annealing, the annealing process is a metal temperature of 450-460°C, and the temperature is kept for 1.5-2.5 hours to obtain a completely recrystallized structure; and cold rolling is continued to be rolled to a finished product thickness of 0.3-0.5 mm; wherein, from the rolling of the cast-rolled billet to the cold-rolled finished product thickness, the total cold rolling processing rate is controlled within 85-92%.
6. The method for preparing an aluminum alloy strip according to claim 1, characterized in that: The step S2 specifically includes: rolling the cast-rolled billet to an intermediate billet thickness of 0.6 to 1.2 mm, performing intermediate incomplete recrystallization annealing to obtain an aluminum alloy strip in H24 state, the annealing process is a metal material temperature of 400 to 410° C., and keeping warm for 2.0 to 3.0 hours to obtain an intermediate billet with a tensile strength of 170 to 175 MPa; and then continuing cold rolling to a finished product thickness of 0.3 to 0.5 mm; wherein, from the cast-rolled billet rolling to the cold-rolled finished product thickness, the total cold rolling processing rate is controlled within 50-60%.
7. The method for preparing an aluminum alloy strip according to claim 1, characterized in that: The step S2 specifically includes: rolling the cast-rolled billet to an intermediate billet thickness of 0.4-0.65 mm, performing intermediate incomplete recrystallization annealing to obtain an aluminum alloy strip in H26 state, the annealing process is that the metal material temperature is 360-370° C., and the heat preservation is 2.0-3.0 hours, and the tensile strength of the intermediate billet is 180-185 MPa; and then cold rolling is performed to a finished product thickness of 0.3-0.5 mm; wherein, from the cast-rolled billet rolling to the cold-rolled finished product thickness, the total cold rolling processing rate is controlled within 25-30%.
8. The method for preparing an aluminum alloy strip according to claim 1, characterized in that: In step S2, the cold rolling oil base oil adopts a dearomatized solvent oil model D105-110 base oil with a viscosity of 2.5 to 2.7 mm 2 / s; a rolling lubricant is obtained by adding an ester and alcohol composite additive to a base oil; the hydroxyl value of the rolling lubricant is controlled at 22-26 mgKOH / g, and the saponification value is controlled at 2.8-3.6 mgKOH / g; the ratios of the ester and alcohol composite additives in the rolling lubricant are 1.25±0.05% and 8.75±0.05%, respectively.
9. The method for preparing an aluminum alloy strip according to claim 1, characterized in that: In the step S3, the edge trimming quality requirements are that the horizontal burr is ≤0.1mm, the vertical burr is ≤0.015mm, and the burr direction is uniformly toward the inside of the coil, and the edge shear rate is ≥80%, wherein the edge shear rate refers to the edge blade shear thickness of the vertical slitting machine after slitting accounts for ≥80% of the total thickness of the strip, and the tear thickness accounts for <20% of the strip thickness.
10. An aluminum alloy strip, characterized in that: The aluminum alloy strip is made by the method for preparing the aluminum alloy strip according to any one of claims 1 to 9, and the aluminum alloy strip is used to manufacture an aluminum shell of a power battery.