Electric automobile aluminum alloy battery tray and die-casting production method thereof
By optimizing the composition and refining of aluminum alloys, and using scrap aluminum to die-casting and forming the aluminum pallet of electric vehicles, the problems of long process and high cost in the existing technology are solved, the strength and safety of the pallets are improved, and the efficiency and environmental protection are achieved. Production effect.
Patent Information
- Application Number
- CN202410999237.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-29
AI Technical Summary
The production process of existing electric vehicle aluminum alloy pallets is long, has high cost, and has low strength and poor plasticity, which affects the safety and lightweight development of electric vehicles.
Die-casting aluminum alloy battery pallets are used to form a scrap aluminum alloy battery pallet. By optimizing the composition of aluminum alloy composition and refining and purification treatment, the structural strength and safety of the pallet are improved, and the slag removal and hydrogen removal treatment is carried out through online inspection and multi-functional powder refining agent to reduce production cost.
The production process flow is shortened, the production cost is reduced, the strength and plasticity of aluminum alloy pallets are improved, and the efficiency and environmentally friendly refining effect is achieved, which enhances the safety and reliability of the pallets.
Smart Images

Figure CN119040707A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of manufacturing aluminum alloy battery trays for electric vehicles, and specifically relates to an aluminum alloy battery tray for electric vehicles and a die-casting production method thereof. Background Art
[0002] The aluminum alloy battery tray is an important safety structure in electric vehicles. It plays a key role in fixing and protecting the battery pack to work normally and safely. Its weight also directly affects the load distribution and endurance of the electric vehicle.
[0003] A Chinese patent document with publication number CN110241334A discloses a method for processing and manufacturing an electric vehicle battery tray, including smelting aluminum liquid, casting aluminum bars, heating and extruding the aluminum bars, and cooling with water mist to obtain profiles, cutting and bending the profiles, machining the bent profiles to obtain a pallet, and welding the bottom plate and the pallet to obtain a formed pallet.
[0004] A Chinese patent document with publication number CN209896116U discloses a pallet for a power battery of a new energy vehicle, including a pallet frame and a pallet chassis. The pallet frame is integrally formed by low-pressure die casting, and the pallet chassis is extruded by a profile. The pallet chassis is welded to the pallet frame by friction welding.
[0005] A Chinese patent document with publication number CN110643862A discloses an aluminum alloy for a battery housing of a new energy vehicle and a method for preparing the same by pressure casting. The aluminum alloy consists of the following components in mass percentage: Si 9.5-13.5%, Fe 0.03-0.15%, Mg 0.22-0.50%, Mn 0.45-0.80%, Ti 0.05-0.15%, B 0.01-0.03%, Sr 0.012-0.05%, RE 0.05-0.2%, and the rest is Al. The preparation method includes smelting the aluminum alloy and pressure casting.
[0006] A Chinese patent document with publication number CN115896561A discloses a die-cast aluminum battery tray for automobiles and its production process. The composition and mass fraction of the aluminum alloy are as follows: Si10.0-12.5%, Fe 0.8-1.2%, Mg 0.5-0.8%, Mn 0.2-0.4%, Cu 0.05-0.15%, Zn 0.05-0.1%, Ti 0.04-0.11%, Sb 0.1-0.3%, the sum of other impurity elements ≤0.15%, and the remainder is Al. The production process includes melting recycled aluminum ingots, refining, refining and modification, and die casting.
[0007] According to the results of literature retrieval and production practice experience, the aluminum alloy pallets of electric vehicles are currently mainly welded, including all aluminum profiles welded or aluminum profiles and die-castings mixed welded. The production process of welded aluminum alloy pallets is long and has many steps, resulting in relatively high production costs. In order to reduce the production cost of aluminum alloy pallets, electric vehicle companies have begun to develop die-casting molding technology for aluminum alloy pallets in recent years. However, this technology has relatively high requirements for die-casting aluminum alloy materials and die-casting processes. The existing die-casting aluminum alloy pallets still have problems such as low strength, poor plasticity, and large wall thickness, which seriously threaten the safety and reliability of electric vehicles and are not conducive to the lightweight development of electric vehicles. Therefore, the existing aluminum alloy battery pallets for electric vehicles and their manufacturing methods still need to be improved and developed. Summary of the invention
[0008] In view of the problems and shortcomings mentioned in the background technology, the present invention provides an aluminum alloy battery tray for electric vehicles and a die-casting production method thereof, which uses waste aluminum to die-cast the aluminum alloy battery tray. By optimizing the component composition, refining and purification, and refinement and metamorphism of the aluminum alloy, the structural strength and safety of the aluminum alloy battery tray are improved, and the production cost of the aluminum alloy battery tray is reduced.
[0009] The present invention achieves the above-mentioned purpose by adopting the following technical solutions:
[0010] The first aspect of the present invention provides an aluminum alloy battery tray for an electric vehicle, characterized in that the aluminum alloy battery tray is composed of the following components in mass percentage: Si 11.6-12.1%, Cu 1.8-2.2%, Zn 1.5-2.0%, Mn0.6-0.8%, Ti 0.04-0.06%, Sr0.003-0.005%, P 0.001-0.003%, Fe≤0.2%, and the balance is Al and other inevitable impurity elements, the individual content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.2%.
[0011] Among them, the main function of Si is to improve the die-casting fluidity of aluminum alloy. The die-casting of aluminum alloy trays requires that the aluminum alloy must have excellent die-casting fluidity to obtain a die-cast aluminum alloy battery tray that is fully filled and dense. Si can form an Al+Si eutectic phase with Al during the solidification process of the aluminum alloy, thereby improving the die-casting fluidity of the aluminum alloy. Low Si content will lead to insufficient fluidity and it will be impossible to obtain a fully filled aluminum alloy tray. Too high Si content will lead to a decrease in the plasticity of the aluminum alloy.
[0012] The main function of Cu is to enhance the strength of aluminum alloy. Cu has a good solid solution strengthening effect in aluminum alloy and can significantly enhance the strength of aluminum alloy. However, too high Cu content will also increase the thermal cracking tendency of die-cast aluminum alloy trays and reduce the corrosion resistance of die-cast aluminum alloy trays.
[0013] The main function of Zn is to enhance the die-casting fluidity of aluminum alloy and enhance the strength of aluminum alloy. However, the Zn content should not be too high, otherwise it will increase the thermal cracking tendency of die-cast aluminum alloy trays and cause thermal cracking defects in die-cast aluminum alloy trays.
[0014] The main function of Mn is to enhance the strength of aluminum alloy through dispersion strength. Mn can form MnAl6 particles in aluminum alloy. MnAl6 particles dispersed in aluminum alloy can not only enhance the strength of die-cast aluminum alloy trays, but also improve the high temperature resistance of die-cast aluminum alloy trays.
[0015] The main function of Ti is to refine the α-Al grains and improve the die-casting fluidity of aluminum alloys. Without the addition of Ti, the aluminum alloy will form coarse dendritic α-Al grains when solidifying, which will hinder the flow of the eutectic liquid phase and reduce the fluidity of the aluminum alloy. When the α-Al grains change from coarse dendritic to granular or spherical, the filling fluidity of the aluminum alloy is greatly improved. If the Ti content is too low, the refining effect is not obvious. However, if the Ti content is too high, it will not significantly improve the grain refining effect, but will increase the production cost.
[0016] The main function of Sr is to refine the modified eutectic Si phase. The eutectic Si phase is usually distributed in the aluminum alloy matrix in the form of coarse needles, which not only reduces the fluidity of the aluminum alloy, but also splits the aluminum alloy matrix, reducing the strength and plasticity of the aluminum alloy. Adding 0.003-0.005% Sr can change the morphology of the eutectic Si phase from coarse needles to fine particles or fibers, which can significantly improve the fluidity of the aluminum alloy and the strength and plasticity of the die-cast aluminum alloy tray.
[0017] The main function of P is to refine the modified primary Si phase. In addition to forming the eutectic Si phase, Si in the aluminum alloy also forms a coarse block of primary Si phase, which not only reduces the fluidity of the aluminum alloy, but also reduces the strength and plasticity of the die-cast aluminum alloy tray. Adding 0.001-0.003% P can transform the coarse block of primary Si into fine and uniform particles, which can not only improve the fluidity of the aluminum alloy, but also improve the strength, plasticity and wear resistance of the die-cast aluminum alloy tray.
[0018] Fe is an inevitable impurity element in aluminum alloys, usually existing in the form of coarse needle-like Fe-rich phases, which will seriously split the matrix of aluminum alloys and reduce the strength and plasticity of aluminum alloys. Therefore, the content of impurity element Fe must be strictly controlled.
[0019] The second aspect of the present invention provides a die-casting production method for an aluminum alloy battery tray for an electric vehicle, which is characterized in that it comprises the following steps in sequence:
[0020] Step 1: sorting and pre-treating the scrap aluminum, and then heating and melting it into aluminum alloy liquid;
[0021] Step 2: Online detection and adjustment of the composition of aluminum alloy liquid;
[0022] Step 3: performing refining agent injection refining and mixed gas injection refining on the aluminum alloy liquid in sequence;
[0023] Step 4: vacuum die-casting the aluminum alloy liquid into an aluminum alloy battery tray blank;
[0024] Step 5: The aluminum alloy battery tray blank is cut, sandblasted and polished, and CNC-processed to obtain the aluminum alloy battery tray.
[0025] Furthermore, the waste aluminum in step one includes shavings, flash, unqualified die-cast aluminum alloy parts and recycled waste die-cast aluminum alloy parts generated in the production of die-cast aluminum alloy.
[0026] Existing aluminum alloy battery trays mainly use raw aluminum ingots, which are smelted and prepared into aluminum alloy liquid by adding alloy elements, and then die-cast to form aluminum alloy battery trays. As we all know, raw aluminum ingots are obtained by electrolysis of alumina, and alumina electrolysis is energy-intensive, which not only consumes a lot of electricity and pollutes the environment, but also increases production costs. The present invention uses waste aluminum to smelt and prepare aluminum alloy liquid and die-cast aluminum alloy battery trays, which not only saves a lot of precious metal elements, but also greatly reduces production costs.
[0027] Furthermore, the sorting and pretreatment of the scrap aluminum described in step one is to remove the iron, rubber, plastic, wood, stone, mud and other inclusions carried or embedded in the scrap aluminum by manual or mechanical methods to obtain scrap aluminum that can be recycled. The iron includes iron wire, iron nails, iron blocks, etc. Scrap aluminum without inclusions can be directly recycled, but scrap aluminum containing inclusions must be sorted and pretreated. The sorting and pretreatment method can be manual picking and removal, or mechanical. The mechanical method first crushes the scrap aluminum with a crusher, and then removes the inclusions in the scrap aluminum by magnetic separation, air separation or water separation. The cost of manual sorting and pretreatment is low, and the mechanical method is suitable for mass production, but the disadvantage is that the investment is large and the cost is high. Manual and mechanical methods each have their own advantages and disadvantages, and it can be decided whether to use manual sorting or mechanical sorting according to the specific situation of the scrap aluminum.
[0028] Furthermore, in step one, heating and melting the waste aluminum into aluminum alloy liquid is to put the waste aluminum into an aluminum melting furnace and heat it at 720-760°C to melt it into aluminum alloy liquid. The heating temperature should not be lower than 720°C, otherwise the melting speed of the waste aluminum is too slow. The heating temperature should not be higher than 760°C, otherwise it will aggravate the oxidation and burning of the waste aluminum. The aluminum melting furnace can be a regenerative gas-fired aluminum melting furnace or a medium frequency induction furnace, among which the regenerative gas-fired aluminum melting furnace has high thermal utilization efficiency, which is conducive to reducing energy consumption and production costs, and is currently a widely used aluminum melting furnace for die-casting aluminum alloy enterprises. The medium frequency induction furnace has a high heating and melting speed and high production efficiency, but it consumes a lot of electricity, which is not conducive to reducing energy consumption and production costs. Therefore, a regenerative gas-fired aluminum melting furnace is preferably used to heat and melt the waste aluminum.
[0029] Furthermore, the online detection of the composition of the aluminum alloy liquid in step 2 is to cast the aluminum alloy liquid into an aluminum alloy sample, and after turning and flattening, use a desktop direct-reading spectrometer or a handheld spectrometer to on-site detect the composition of the aluminum alloy sample; the online adjustment of the composition of the aluminum alloy liquid is to compare the composition of the aluminum alloy sample with the composition requirements of the target aluminum alloy. If the content of an element is lower than the composition requirements of the target aluminum alloy, the content of the element in the aluminum alloy liquid is increased by adding pure metal or alloy of the element; if the content of an element exceeds the composition requirements of the target aluminum alloy, the content of the element in the aluminum alloy liquid is diluted by adding aluminum ingots, so that the composition of the aluminum alloy liquid meets the composition requirements of the target aluminum alloy.
[0030] Furthermore, the refining agent in step three is composed of the following components in mass percentage: NaCl 35.12%, NaF 19.84%, TiCl3 16.51%, SrSO4 10.06%, KPO3 11.45%, and Na2B4O7 7.02%.
[0031] Since the surface of scrap aluminum is inevitably covered or adhered with paint, coatings, oil stains and water vapor, these coverings and water vapor enter the aluminum melting furnace with the scrap aluminum. After heating and melting, the aluminum alloy liquid is involved in the inclusions. After the water vapor decomposes, the aluminum alloy liquid absorbs hydrogen, making the aluminum alloy liquid contain a large amount of slag and hydrogen. If the slag and hydrogen removal treatment is not performed, the slag and hydrogen will remain in the aluminum alloy to form defects such as pores, inclusions and looseness, reducing the strength and plasticity of the aluminum alloy battery tray. Therefore, in order to obtain a high-strength and high-plasticity aluminum alloy battery tray, the aluminum alloy liquid must be refined, deslaged and dehydrogenated.
[0032] The deslagging and dehydrogenation effect of refining agent spray refining is closely related to the composition of the refining agent. The existing refining agent is mainly obtained by crushing and mixing fluoride salts and chloride salts, which leads to low deslagging and dehydrogenation efficiency of the refining agent, large emission of irritating smoke and single function, which makes it difficult to meet the needs of waste aluminum die-casting aluminum alloy battery trays. In order to improve the deslagging and dehydrogenation effect of powder spray refining, the present invention has developed a high-efficiency and environmentally friendly multifunctional powder refining agent, in which NaCl reacts with aluminum liquid to generate AlCl3 with a boiling point of only 180°C. AlCl3 bubbles adsorb and capture inclusions and hydrogen in the aluminum alloy liquid during the floating process, and then escape from the aluminum alloy liquid together, playing a role in deslagging and dehydrogenation. The main function of NaF is to destroy the aluminum oxide film by forming molten salt, dissolve inclusions such as aluminum oxide into the molten salt, increase the surface tension between the inclusions and the aluminum alloy liquid, promote the separation of inclusions such as aluminum oxide from the aluminum alloy liquid, and enhance the deslagging function of the refining agent. TiCl3 reacts with aluminum alloy liquid to generate AlCl3 bubbles, which absorb and capture inclusions and hydrogen in the aluminum alloy liquid during the floating process, enhancing the slag and hydrogen removal capabilities of the refining agent. The Ti element obtained by the reaction can enhance the effect on the grains of the aluminum alloy and improve the strength and plasticity of the aluminum alloy battery tray. SrSO4 reacts with aluminum alloy liquid to generate SO2 bubbles, which absorb and capture inclusions and hydrogen in the aluminum alloy liquid during the floating process, enhancing the slag and hydrogen removal capabilities of the refining agent. The Sr element obtained by the reaction can enhance the refinement and modification of the eutectic Si phase in the aluminum alloy and improve the strength and plasticity of the aluminum alloy battery tray. KPO3 reacts with aluminum alloy liquid to generate P elements, which can enhance the refinement and modification of the primary Si phase in the aluminum alloy and improve the strength, plasticity and wear resistance of the aluminum alloy battery tray. Na2B4O7 reacts with aluminum liquid to generate B elements, which can refine the coarse Fe-rich phase of the modified aluminum alloy, eliminate the harm of the coarse Fe-rich phase to the strength and plasticity of the aluminum alloy, and improve the strength and plasticity of the aluminum alloy battery tray.
[0033] Furthermore, the preparation method of the refining agent in step 3 comprises the following steps in sequence:
[0034] (1) According to the composition and mass percentage of the refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 with a purity of ≥99.8% are selected as raw materials for batching; (2) the ingredients are added into water at a temperature of 70° C. and stirred to dissolve into an aqueous solution, wherein the mass ratio of water to the ingredients is 1.2, and then the aqueous solution is heated to 100° C. to evaporate and obtain solid crystals; (3) the solid crystals are crushed into powders with a particle size of less than 2 mm, and the powders are dried and dehydrated at 160° C. for 4 hours to obtain the refining agent.
[0035] The deslagging and dehydrogenation effect of the refining agent is also closely related to its preparation method. Existing refining agents are usually obtained by directly mixing chloride salts and fluoride salts after mechanical crushing. The components of this refining agent exist independently of each other, the melting point of the refining agent is high, and there is a lack of synergy between the components, resulting in low deslagging and dehydrogenation efficiency of the refining agent. The present invention breaks through the traditional preparation method and adopts a solution evaporation method to prepare the refining agent. Through solution evaporation, the components are re-solidified and recrystallized to form a eutectic with a lower melting point. For example, the melting point of NaCl is usually 801°C, and the melting point of NaF is usually 993°C. When the two form a NaCl·NaF eutectic, the melting point drops to 698°C, thereby greatly reducing the melting point of the refining agent, making the refining agent easier to dissolve in the aluminum alloy liquid, and playing a synergistic role during refining, which can significantly enhance the deslagging and dehydrogenation ability of the refining agent.
[0036] Furthermore, the carrier gas for the refining agent spray refining in step three is argon with a purity of ≥99.99%, the amount of the refining agent is 0.1-0.2% of the weight of the aluminum alloy liquid, the temperature of the aluminum alloy liquid during spray refining is 700-720°C, and the spray refining time is 15-20 minutes.
[0037] The refining agent spray refining adopts a powder spraying tank and a stainless steel pipe, and uses argon as a carrier to spray a solid powdered refining agent into the aluminum alloy liquid, so that the refining agent contacts and reacts with the aluminum alloy liquid, and then the inclusions and hydrogen in the aluminum alloy liquid are taken out of the aluminum alloy liquid. The deslagging and degassing effect of the refining agent spray refining is also related to the purity of the argon gas, the amount of the refining agent, the temperature of the aluminum alloy liquid during refining, and the spray refining time. The higher the purity of the argon gas, the greater the amount of the refining agent, the longer the spray refining time, the better the effect of deslagging and dehydrogenation, but the production cost will also increase accordingly. If the temperature of the aluminum alloy liquid is too high or the spray refining time is too long, the oxidation and burning of the aluminum alloy liquid will also increase. After the spray refining is completed, after the scum on the surface of the aluminum alloy liquid is removed, a covering agent should be sprinkled on the surface of the aluminum alloy liquid in time to avoid oxidation and burning of the aluminum alloy liquid and re-absorption of hydrogen. After sprinkling the covering agent, the aluminum alloy liquid needs to be left standing for a period of time so that inclusions and bubbles in the aluminum alloy liquid have sufficient time to escape. The standing time of the aluminum alloy liquid is not less than 30 minutes, and preferably the standing time of the aluminum alloy liquid is 30-40 minutes.
[0038] Furthermore, the mixed gas in step three is composed of argon gas with a purity of ≥99.99%, sulfur hexafluoride and carbon monoxide, the volume percentage of sulfur hexafluoride in the mixed gas is 9-11%, and the volume percentage of carbon monoxide is 3-5%.
[0039] Although the refining agent spray refining greatly reduces the slag hydrogen content of the aluminum alloy liquid, the aluminum alloy liquid still contains slag hydrogen because the refining agent spray refining can only remove part of the slag. In addition, although powder spray refining also has a dehydrogenation effect, the dehydrogenation effect is limited because the refining agent inevitably contains moisture, which will be brought into the powder spray refining, causing the aluminum alloy liquid to absorb hydrogen again, so that the dehydrogenation is always in a dynamic equilibrium process. It is difficult for powder spray refining to reduce the hydrogen content of the aluminum alloy liquid to below 0.2ml / 100gAl. Therefore, in order to obtain a highly clean aluminum alloy liquid, gas spray refining is also required to further reduce the slag hydrogen content in the aluminum alloy liquid.
[0040] In the existing gas injection refining technology, inert gas nitrogen or argon, or a mixture of inert gas and chlorine, is usually injected into the aluminum alloy liquid. The relative molecular mass of nitrogen is 28.01 and the density is 1.25kg / m 3 The relative molecular mass of argon is 39.94 and the density is 1.78 kg / m 3 The relative molecular mass of chlorine is 70.91 and the density is 3.21kg / m 3 . Due to the small relative molecular mass and low density of nitrogen, argon and chlorine, the bubbles rise faster in the aluminum alloy liquid, and the contact time between the bubbles and the aluminum alloy liquid is shorter, which limits the time for the bubbles to capture and adsorb hydrogen and inclusions, greatly affecting the dehydrogenation and deslagging effect of gas injection refining. In addition, although the relative density of chlorine is relatively large, chlorine is a toxic gas with a strong pungent odor, which will not only corrode the smelting furnace and smelting tools, but also cause serious environmental pollution.
[0041] Aiming at the problems and shortcomings of the existing gas injection refining technology, in order to obtain a highly clean aluminum alloy liquid, the present invention injects a mixed gas consisting of argon with a purity of ≥99.99%, sulfur hexafluoride with a purity of ≥99.99% and carbon monoxide with a purity of ≥99.99% into the aluminum alloy liquid, wherein sulfur hexafluoride is a high-density, high-stability gas with a relative molecular mass of 146.05 and a density of 6.5kg / m 3 , and sulfur hexafluoride is non-toxic, non-flammable and non-corrosive. Adding 9-11% by volume of sulfur hexafluoride to the mixed gas can significantly slow down the floating speed of bubbles in the aluminum alloy liquid, increase the contact time between the bubbles and the aluminum alloy liquid, and enable the bubbles to capture and absorb more hydrogen and inclusions, thereby improving the dehydrogenation and deslagging effect of gas injection refining. Adding 3-5% by volume of carbon monoxide to the mixed gas is to use carbon monoxide to capture oxygen in the aluminum alloy liquid to form carbon dioxide, avoid oxygen and aluminum forming an aluminum oxide film on the bubble surface, enhance the ability of the bubbles to capture and absorb hydrogen and inclusions, and improve the deslagging and dehydrogenation effect of gas injection refining.
[0042] Furthermore, the amount of the mixed gas in step 3 is 2-3 cubic meters per ton of aluminum alloy liquid, and the pressure of the mixed gas is (0.3-0.5)×10 5 Pa, the temperature of the aluminum alloy liquid during spray refining is 700-720℃, and the spray refining time is 10-15 minutes.
[0043] The mixed gas spray refining adopts a stainless steel pipe or a degasser to spray the mixed gas into the aluminum alloy liquid, so that the mixed gas forms fine bubbles to contact and react with the aluminum alloy liquid, and the hydrogen and inclusions in the aluminum alloy liquid are brought out of the liquid surface by the floating of the bubbles. The dehydrogenation and slag removal effect of the mixed gas spray refining is also related to the amount of the mixed gas, the temperature of the aluminum alloy liquid and the spray refining time. The greater the amount of the mixed gas, the longer the spray refining time, the better the deslag and hydrogen removal effect of the spray refining, but the production cost will also increase accordingly. If the temperature of the aluminum alloy liquid is too high or the spray refining time is too long, the oxidation and burning of the aluminum alloy liquid will also increase. After the spray refining is completed, after removing the scum on the surface of the aluminum alloy liquid, a covering agent should be sprinkled on the surface of the aluminum alloy liquid in time to avoid oxidation and burning of the aluminum alloy liquid and hydrogen absorption. After the coating agent is applied, the aluminum alloy liquid needs to be left to stand for a period of time so that the bubbles in the aluminum alloy liquid have sufficient time to escape. The standing time of the aluminum alloy liquid cannot be less than 20 minutes. As a preferred embodiment, the standing time of the aluminum alloy liquid is 20-30 minutes. Through mixed gas spray refining, the hydrogen content of the aluminum alloy liquid can be reduced to less than 0.15ml / 100gAl, and the inclusion content can be reduced to 0.1mm 2 / kgAl or less, thereby greatly improving the cleanliness of the aluminum alloy liquid.
[0044] Furthermore, during the vacuum die-casting in step 4, the pouring temperature of the aluminum alloy liquid is 710-730°C, the mold temperature is 200-250°C, the vacuum degree is 200-300mbar, the filling speed is 20-25m / s, the boost pressure is 700-800bar, and the holding time is 15-20s.
[0045] During vacuum die casting, the pouring temperature of aluminum alloy cannot be lower than 710℃, the mold temperature cannot be lower than 200℃, the vacuum degree cannot be less than 200mbar, the filling speed cannot be lower than 20m / s, and the boost pressure cannot be lower than 700bar, otherwise it may cause incomplete filling of aluminum alloy battery tray and surface cold shut defects, and it is impossible to obtain a dense aluminum alloy battery tray. However, the pouring temperature of aluminum alloy and the mold temperature cannot be too high, otherwise it is easy to cause the aluminum alloy liquid to cool and solidify for too long in the mold, resulting in shrinkage cracks and reducing production efficiency.
[0046] Furthermore, the trimming of the aluminum alloy battery tray blank described in step five refers to cutting off the die-casting head and flash of the aluminum alloy battery tray to obtain an aluminum alloy battery tray with a complete shape. The sandblasting is to put the aluminum alloy battery tray blank into a sandblasting machine, and use fine steel balls to grind the surface of the aluminum alloy battery tray to remove defects such as die-casting flow lines on the surface to obtain an aluminum alloy battery tray with uniform surface roughness. The CNC processing is to use a CNC machine tool to drill holes, tap screw holes and turn and mill the aluminum alloy battery tray to obtain a finished aluminum alloy battery tray. The trimming, sandblasting and CNC processing of the aluminum alloy battery tray blank are relatively mature production processes, and the equipment used is also conventional equipment. Therefore, the trimming, sandblasting and CNC processing of the aluminum alloy battery tray blank will not be repeated or described in detail.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] (1) The present invention realizes the die-casting production of aluminum alloy battery trays for electric vehicles. Compared with traditional welded aluminum alloy battery trays, the present invention shortens the production process of aluminum alloy battery trays and reduces the production steps, which is beneficial to improving the production efficiency of aluminum alloy trays and reducing the production cost of aluminum alloy trays.
[0049] (2) The present invention realizes the use of waste aluminum to die-cast aluminum alloy battery trays. Compared with the traditional use of original aluminum ingots to die-cast aluminum alloy trays, the present invention does not need to add too many alloy elements, which not only improves the use value of waste aluminum, but also helps to reduce the production cost of aluminum alloy battery trays.
[0050] (3) The present invention greatly improves the strength and plasticity of the aluminum alloy battery tray by optimizing the design of the component composition of the aluminum alloy and through refining, purification and refinement and modification. In the non-heat-treated state, the tensile strength of the aluminum alloy battery tray body sample is not less than 350MPa, the yield strength is not less than 300MPa, and the elongation after fracture is not less than 10%, thereby improving the structural strength and reliability of the aluminum alloy battery tray.
[0051] (4) The present invention also develops a highly efficient, environmentally friendly, multifunctional powder refining agent, which overcomes the problems of low degassing and slag removal efficiency and single function of traditional refining agents. It can not only greatly improve the cleanliness of aluminum alloy liquid, but also refine and modify the aluminum alloy, thereby improving the strength and plasticity of the aluminum alloy battery tray. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 This is the optical microscope microstructure of the aluminum alloy battery tray of Example 1 of the present invention.
[0053] Figure 2 This is the scanning electron microscope microstructure of the aluminum alloy battery tray of Example 1 of the present invention.
[0054] Figure 3 This is the optical microscope microstructure of the aluminum alloy battery tray of comparative example 4.
[0055] Figure 4 This is the scanning electron microscope microstructure of the aluminum alloy battery tray of comparative example 4. DETAILED DESCRIPTION
[0056] The technical solution of the present invention is described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0057] Embodiment 1:
[0058] The aluminum alloy battery tray is composed of the following components in mass percentage: Si 11.86%, Cu 2.04%, Zn 1.79%, Mn 0.73%, Ti 0.05%, Sr 0.004%, P 0.002%, Fe ≤ 0.2%, the balance is Al and other inevitable impurity elements, the individual content of other impurity elements is ≤ 0.05%, and the total amount of other impurity elements is ≤ 0.2%. The die-casting production method includes the following steps in sequence: Step 1: sorting and pre-treating the scrap aluminum to remove the iron, rubber, plastic, wood, stone, mud and other inclusions carried or embedded, and then heating the scrap aluminum at 740 ° C to melt it into aluminum alloy liquid; Step 2: online detection and adjustment of the composition of the aluminum alloy liquid to make the composition of the aluminum alloy liquid meet the target The composition of the aluminum alloy; Step 3: Use argon gas with a purity of 99.99% and a refining agent of 0.15% by weight of the aluminum alloy liquid to spray and refine the aluminum alloy liquid at 710°C for 17 minutes, and then use a mixed gas composed of argon gas with a purity of 99.99%, sulfur hexafluoride and carbon monoxide to spray and refine the aluminum alloy liquid at 710°C for 12 minutes, the volume percentage of sulfur hexafluoride in the mixed gas is 10%, the volume percentage of carbon monoxide is 4%, the amount of the mixed gas is 2.5 cubic meters / ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.4×10 5 Pa; Step 4: Under the conditions of aluminum alloy liquid pouring temperature of 720°C, mold temperature of 230°C, vacuum degree of 250mbar, filling speed of 23m / s, boost pressure of 750bar and holding time of 18s, the aluminum alloy liquid is vacuum die-cast into an aluminum alloy battery tray blank; Step 5: Cut the excess, sandblast and CNC process the aluminum alloy battery tray blank to obtain the aluminum alloy battery tray.
[0059] Embodiment 2:
[0060] The aluminum alloy battery tray is composed of the following components in mass percentage: Si 12.1%, Cu1.8%, Zn 2.0%, Mn 0.6%, Ti 0.06%, Sr 0.003%, P 0.003%, Fe≤0.2%, the balance is Al and other inevitable impurity elements, the individual content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.2%. The die-casting production method includes the following steps in sequence: Step 1: sorting and pre-treating the scrap aluminum to remove the iron, rubber, plastic, wood, stone, mud and other inclusions carried or embedded, and then heating the scrap aluminum at 760°C to melt it into aluminum alloy liquid; Step 2: online detection and adjustment of the composition of the aluminum alloy liquid to make the composition of the aluminum alloy liquid meet the target The composition of the standard aluminum alloy; Step 3: Use argon with a purity of 99.99% and a refining agent of 0.2% by weight of the aluminum alloy liquid to spray and refine the aluminum alloy liquid at 700°C for 20 minutes, and then use a mixed gas composed of argon with a purity of 99.99%, sulfur hexafluoride and carbon monoxide to spray and refine the aluminum alloy liquid at 700°C for 15 minutes, the volume percentage of sulfur hexafluoride in the mixed gas is 11%, the volume percentage of carbon monoxide is 3%, the amount of the mixed gas is 3 cubic meters / ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.3×10 5 Pa; Step 4: Under the conditions of aluminum alloy liquid pouring temperature of 710°C, mold temperature of 250°C, vacuum degree of 200mbar, filling speed of 25m / s, boost pressure of 700bar and holding time of 20s, the aluminum alloy liquid is vacuum die-cast into an aluminum alloy battery tray blank; Step 5: Cut the excess, sandblast and CNC process the aluminum alloy battery tray blank to obtain the aluminum alloy battery tray.
[0061] Embodiment 3:
[0062] The aluminum alloy battery tray is composed of the following components in mass percentage: Si 11.6%, Cu2.2%, Zn 1.5%, Mn 0.8%, Ti 0.04%, Sr 0.005%, P 0.001%, Fe≤0.2%, the balance is Al and other inevitable impurity elements, the individual content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.2%. The die-casting production method comprises the following steps in sequence: Step 1: sorting and pre-treating the scrap aluminum to remove the iron, rubber, plastic, wood, stone, mud and other inclusions carried or embedded, and then heating the scrap aluminum at 720°C to melt it into aluminum alloy liquid; Step 2: online detection and adjustment of the composition of the aluminum alloy liquid to make the composition of the aluminum alloy liquid meet the requirements. The composition of the target aluminum alloy; Step 3: Use argon with a purity of 99.99% and a refining agent of 0.1% by weight of the aluminum alloy liquid to spray and refine the aluminum alloy liquid at 720°C for 15 minutes, and then use a mixed gas composed of argon with a purity of 99.99%, sulfur hexafluoride and carbon monoxide to spray and refine the aluminum alloy liquid at 720°C for 10 minutes, the volume percentage of sulfur hexafluoride in the mixed gas is 9%, the volume percentage of carbon monoxide is 5%, the amount of the mixed gas is 2 cubic meters / ton of aluminum alloy liquid, and the pressure of the mixed gas is 0.5×10 5 Pa; Step 4: Under the conditions of aluminum alloy liquid pouring temperature of 730°C, mold temperature of 200°C, vacuum degree of 300mbar, filling speed of 20m / s, boost pressure of 800bar and holding time of 15s, the aluminum alloy liquid is vacuum die-cast into an aluminum alloy battery tray blank; Step 5: Cut the excess, sandblast and CNC process the aluminum alloy battery tray blank to obtain the aluminum alloy battery tray.
[0063] The refining agent described in Examples 1-3 of the present invention is composed of the following components in mass percentage: NaCl 35.12%, NaF 19.84%, TiCl3 16.51%, SrSO4 10.06%, KPO3 11.45%, and Na2B4O7 7.02%. The preparation method of the refining agent comprises the following steps in sequence: (1) according to the composition and mass percentage of the refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 with a purity of ≥99.8% are selected as raw materials for batching; (2) the ingredients are added into water at a temperature of 70°C and stirred to dissolve into an aqueous solution, the mass ratio of water to the ingredients being 1.2, and then the aqueous solution is heated to 100°C to evaporate to obtain a solid crystal; (3) the solid crystal is crushed into a powder with a particle size of less than 2 mm, and the powder is dried and dehydrated at 160°C for 4 hours to obtain the refining agent.
[0064] Comparative Example 1:
[0065] The component composition and die-casting production method of the aluminum alloy battery tray in this comparative example are the same as those in Example 1, except that the aluminum alloy battery tray is composed of the following components in mass percentage: Si11.86%, Cu 1.52%, Zn 1.79%, Mn0.73%, Ti 0.05%, Sr 0.004%, P0.002%, Fe≤0.2%, and the remainder is Al and other unavoidable impurity elements, the individual content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.2%.
[0066] Comparative Example 2:
[0067] The component composition and die-casting production method of the aluminum alloy battery tray in this comparative example are the same as those in Example 1, except that the aluminum alloy battery tray is composed of the following components in mass percentage: Si11.86%, Cu 2.04%, Zn 1.79%, Mn0.73%, Ti 0.02%, Sr 0.004%, P0.002%, Fe≤0.2%, and the balance is Al and other unavoidable impurity elements, the individual content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.2%.
[0068] Comparative Example 3:
[0069] The component composition and die-casting production method of the aluminum alloy battery tray in this comparative example are the same as those in Example 1, except that the aluminum alloy battery tray is composed of the following components in mass percentage: Si11.86%, Cu 2.04%, Zn 1.79%, Mn0.73%, Ti 0.05%, Sr 0.001%, P0.002%, Fe≤0.2%, and the balance is Al and other unavoidable impurity elements, the individual content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.2%.
[0070] Comparative Example 4:
[0071] The component composition and die-casting production method of the aluminum alloy battery tray in this comparative example are the same as those in Example 1, except that the refining agent used is an existing conventional refining agent, which is composed of the following components in mass percentage: NaCl 36.13%, KCl 15.42%, CaF2 16.84%, NaF19.24%, C2Cl6 12.37%, and the refining agent is obtained by directly crushing and mixing the raw materials after drying and dehydration.
[0072] Comparative Example 5:
[0073] The component composition and die-casting production method of the aluminum alloy battery tray in this comparative example are the same as those in Example 1, except that in step five, a mixed gas composed of argon, sulfur hexafluoride and carbon monoxide is not used, but argon with a purity of 99.99% is used to spray and refine the aluminum alloy liquid.
[0074] Verification example:
[0075] The hydrogen content and slag content of the aluminum alloy liquid before die casting of Examples 1-3 and Comparative Examples 1-5 were detected by using a HDA-V hydrogen meter and an Analyze PoDFA slag meter. The results are shown in Table 1. As can be seen from Table 1, the hydrogen content of the aluminum alloy liquid before die casting of Examples 1-3 and Comparative Examples 1-3 is less than 0.14 ml / 100 gAl, and the slag content is less than 0.08 mm 2 / kgAl. Comparative Example 4 uses commercially available conventional refining agent for refining by spraying, and Comparative Example 5 does not use mixed gas for refining by spraying, resulting in a relatively high gas slag content in the aluminum alloy liquid. By comparison, it can be seen that the use of the technical solution of the present invention can significantly reduce the gas slag content of the aluminum alloy liquid before die casting and improve the cleanliness of the die-cast aluminum alloy battery tray.
[0076] Table 1 Hydrogen content and slag content of aluminum alloy liquid
[0077]
[0078] Samples were taken from the die-cast aluminum alloy battery trays obtained in Example 1 and Comparative Example 4. After the samples were ground, polished and corroded, the microstructures of the samples were observed using an optical microscope and a scanning electron microscope, respectively. Figure 1 and Figure 2 Optical microscope and scanning electron microscope microstructures of the die-cast aluminum alloy battery tray of Example 1, respectively. Figure 3 and Figure 4 The optical microscope and scanning electron microscope microstructures of the die-cast aluminum alloy battery tray of comparative example 4 are shown respectively. Figure 1 and Figure 2 It can be seen that, since Example 1 uses a multifunctional powder refining agent for refining, the refining agent has a refining and modification function, so that the grain structure of the die-cast aluminum alloy battery tray is fine and uniform, and there are no coarse dendritic α-Al grains, coarse needle-like Si phases and Fe-rich phases. Figure 3 and Figure 4 It can be seen that since comparative example 4 uses conventional refining agents, which have no refining and modification function, the grain structure of the die-cast aluminum alloy battery tray is relatively coarse, with the presence of some coarse dendritic α-Al grains and coarse needle-like Si phases and Fe-rich phases.
[0079] Samples were taken from the die-cast aluminum alloy battery trays obtained in Examples 1-3 and Comparative Examples 1-5, and the room temperature tensile mechanical properties of the aluminum alloy samples in the non-heat-treated state were tested. The results are shown in Table 2. As can be seen from Table 2, the tensile strength of the aluminum alloy battery trays of Examples 1-3 is not less than 350MPa, the yield strength is not less than 300MPa, and the elongation after fracture is not less than 10%, which has the advantages of high strength and good plasticity. Due to the insufficient Cu content in the aluminum alloy of Comparative Example 1, the insufficient Ti content in the aluminum alloy of Comparative Example 2, and the insufficient Sr content in the aluminum alloy of Comparative Example 3, Comparative Example 4 uses commercially available conventional refining agents for spray refining, and Comparative Example 5 does not use mixed gas spray refining. Due to the high gas slag content of the aluminum alloy liquid, the tensile strength of the aluminum alloy battery trays of Comparative Examples 1-5 is lower than 335MPa, the yield strength is lower than 285MPa, and the elongation after fracture of the aluminum alloy battery trays of Comparative Examples 4 and 5 is lower than 8%.
[0080] Table 2 Tensile mechanical properties of die-cast aluminum alloy
[0081]
[0082]
Claims
1. An aluminum alloy battery tray for electric vehicles, characterized in that: The aluminum alloy battery tray consists of the following components in percentage by mass: Composition: Si 11.6-12.1%, Cu 1.8-2.2%, Zn 1.5-2.0%, Mn 0.6-0.8%, Ti 0.04-0.06%, Sr 0.003-0.005%, P0.001-0.003%, Fe≤0.2%, the balance is Al and other unavoidable impurity elements, the single content of other impurity elements is ≤0.05%, and the total amount of other impurity elements is ≤0.2%.
2. A die-casting production method for an aluminum alloy battery tray for an electric vehicle as claimed in claim 1, characterized in that: The following steps are included in sequence: Step 1: sorting and pre-treating the scrap aluminum, and then heating and melting it into aluminum alloy liquid; Step 2: Online detection and adjustment of the composition of aluminum alloy liquid; Step 3: performing refining agent injection refining and mixed gas injection refining on the aluminum alloy liquid in sequence; Step 4: vacuum die-casting the aluminum alloy liquid into an aluminum alloy battery tray blank; Step 5: The aluminum alloy battery tray blank is cut, sandblasted and polished, and CNC-processed to obtain the aluminum alloy battery tray.
3. The die-casting production method of the aluminum alloy battery tray for electric vehicles according to claim 2 is characterized in that: The waste aluminum described in step 1 includes shavings, flash, unqualified die-cast aluminum alloy parts and recycled waste die-cast aluminum alloy parts generated in the production of die-cast aluminum alloy.
4. The die-casting production method of the aluminum alloy battery tray for electric vehicles according to claim 2 is characterized in that: The pretreatment of the scrap aluminum in step 1 is to remove the iron, rubber, plastic, wood, stone, mud and other impurities carried or embedded in the scrap aluminum by manual or mechanical means to obtain scrap aluminum that can be recycled.
5. The die-casting production method of the aluminum alloy battery tray for electric vehicles according to claim 2 is characterized in that: In step 1, heating and melting the waste aluminum into aluminum alloy liquid is to put the waste aluminum into an aluminum melting furnace and heat it at 720-760° C. to melt it into aluminum alloy liquid.
6. The die-casting production method of the aluminum alloy battery tray for electric vehicles according to claim 2 is characterized in that: The online detection of the composition of the aluminum alloy liquid in step 2 is to cast the aluminum alloy liquid into an aluminum alloy sample, and use a desktop direct-reading spectrometer or a handheld spectrometer to detect the composition of the aluminum alloy sample on-site. The online adjustment of the composition of the aluminum alloy liquid includes adding pure metal or alloy to increase the content of elements in the aluminum alloy liquid and adding aluminum ingots to dilute the content of elements in the aluminum alloy liquid.
7. The die-casting production method of the aluminum alloy battery tray for electric vehicles according to claim 2 is characterized in that: The refining agent in step 3 is composed of the following components in mass percentage: NaCl 35.12%, NaF 19.84%, TiCl3 16.51%, SrSO4 10.06%, KPO3 11.45%, and Na2B4O7 7.02%. The preparation method of the refining agent comprises the following steps in sequence: (1) according to the composition and mass percentage of the refining agent, NaCl, NaF, TiCl3, SrSO4, KPO3, and Na2B4O7 with a purity of ≥99.8% are selected as raw materials for batching; (2) the ingredients are added into water at a temperature of 70°C and stirred to dissolve into an aqueous solution, the mass ratio of water to ingredients being 1.2, and then the aqueous solution is heated to 100°C to evaporate to obtain solid crystals; (3) the solid crystals are crushed into powders with a particle size of less than 2 mm, and the powders are dried and dehydrated at 160°C for 4 hours to obtain the refining agent.
8. The die-casting production method of the aluminum alloy battery tray for electric vehicles according to claim 2 is characterized in that: The carrier gas for the refining agent spray refining in step 3 is argon with a purity of ≥99.99%, the amount of the refining agent is 0.1-0.2% of the weight of the aluminum alloy liquid, the temperature of the aluminum alloy liquid during spray refining is 700-720°C, and the spray refining time is 15-20 minutes.
9. The die-casting production method of the aluminum alloy battery tray for electric vehicles according to claim 2, characterized in that: The mixed gas in step 3 is composed of argon with a purity of ≥99.99%, sulfur hexafluoride and carbon monoxide, the volume percentage of sulfur hexafluoride in the mixed gas is 9-11%, the volume percentage of carbon monoxide is 3-5%, the amount of the mixed gas is 2-3 cubic meters / ton of aluminum alloy liquid, and the pressure of the mixed gas is (0.3-0.5)×10 5 Pa, the temperature of the aluminum alloy liquid during spray refining is 700-720℃, and the spray refining time is 10-15 minutes.
10. The die-casting production method of the aluminum alloy battery tray for electric vehicles according to claim 2, characterized in that: During the vacuum die casting in step 4, the pouring temperature of the aluminum alloy liquid is 710-730°C, the mold temperature is 200-250°C, the vacuum degree is 200-300mbar, the filling speed is 20-25m / s, the boost pressure is 700-800bar, and the holding time is 15-20s.