Low-cost and high-toughness 16MnDR steel for rail transit locomotive parts and production method of low-cost and high-toughness 16MnDR steel

By optimizing the alloy composition and production process of 16MnDR steel, the problems of precious alloy use and high energy consumption in the existing technology are solved, and 16MnDR steel with low cost, high strength and high temperature impact toughness are achieved to meet the use of rail transit locomotive parts Require.

CN119040760APending Publication Date: 2024-11-29WUHU XINXING DUCTILE IRON PIPES
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411078959.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing 16MnDR steel production method adds precious alloys such as V, Ni, Nb, and Ti, which leads to an increase in cost, and high energy consumption during heating and rolling, which affects production efficiency, and unreasonable composition design leads to low ferrite grain size. , cannot meet the requirements for the use of rail transit locomotive parts.

Method used

The alloy composition design of low-cost, high-toughness 16MnDR steel includes C0.16-0.20%, Si0.25-0.45%, Mn1.35-1.50%, V0.025-0.040%, Nb0.010-0.020%, P≤ 0.015%, S≤0.010%, N0.0060-0.0080%, through the production methods of converter smelting, LF refining, RH vacuum treatment, continuous casting, heating, rolling and normalizing treatment, the addition of precious metals is avoided and the heating time is optimized. and temperature control to ensure high strength and low temperature impact toughness of steel.

Benefits of technology

It achieves low cost, high strength and high-temperature impact toughness, meets the requirements of rail transit locomotive parts, reduces production costs and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040760A_ABST
    Figure CN119040760A_ABST
Patent Text Reader

Abstract

The invention discloses low-cost high-toughness 16MnDR steel for rail transit locomotive parts and a production method of the 16MnDR steel. The 16MnDR steel comprises the following chemical components in percentage by weight: 0.16 to 0.20 percent of C, 0.25 to 0.45 percent of Si, 1.35 to 1.50 percent of Mn, 0.025 to 0.040 percent of V, 0.010 to 0.020 percent of Nb, less than or equal to 0.015 percent of P, less than or equal to 0.010 percent of S, 0.0060 to 0.0080 percent of N and the balance of Fe and inevitable impurities. The tensile strength of the 16MnDR steel is 480-600 MPa, the yield strength is larger than or equal to 350 MPa, and the ductility is larger than or equal to 25%. At the temperature of-40 DEG C, the longitudinal impact absorption energy KV2 is greater than or equal to 120J; the ferrite grain size grade of the normalized 16MnDR steel is more than 7.0 grade; the steel has the comprehensive properties of low cost, high strength, good low-temperature impact toughness and the like, can be used as steel for rail transit locomotive parts, and can completely meet the use requirements of customers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of steel, and in particular relates to a low-cost and high-toughness 16MnDR steel for rail transit locomotive parts and a production method thereof. Background Art

[0002] With the high-quality development of my country's economic construction, the development of low-cost, high-efficiency, conservation and long-life has become the development trend of my country's future manufacturing industry. 16MnDR products have been used not only as steel for low-temperature pressure vessels, but also for the production of chassis parts for rail transit locomotives and vehicles. After processing, they are used in nearly 40 kinds of automotive parts.

[0003] The production method of using 16MnDR steel plates to make low-temperature pressure vessels has been reported, but the production of 16MnDR steel bars for processing locomotive parts has rarely been reported. At the same time, the 16MnDR steel for rail transit requires the low-temperature impact energy of ≥80J at -40℃ and the ferrite grain size after normalizing ≥7.0. The current state of the art is to add a certain amount of V and add elements such as Ni, Nb, and Ti to refine the grains. For example, Chinese patent CN102605241A discloses a normalizing type 16MnDR low-temperature pressure vessel steel plate and a manufacturing method thereof, in which a large amount of vanadium-nitrogen alloy is added, and V is controlled at 0.050-0.070%; for example, Chinese patent CN110468326A discloses an ultra-thin specification 16MnDR steel plate for LNG storage tanks and a manufacturing method thereof, in which a large amount of Ni alloy is added, and Ni is controlled at 0.10-0.30%, etc., resulting in a higher Ni alloy cost; at the same time, other steel mills use a production process in which the billet is slowly cooled and then cold-fed into a furnace for heating and rolling in the production of this type of steel, which additionally increases energy consumption, affects production efficiency, and increases market costs. It can be seen that the existing production method of 16MnDR continuous casting round billet has the following defects: 1) The alloy composition design of this steel grade adds precious alloys such as V, Ni, Nb, Ti, and the alloy mass percentage is relatively large, resulting in an increase in cost; 2) The large-section 16MNDR round continuous casting billet is pile-cooled or slowly cooled in a pit before being sent for rolling. The cold billet needs a long heating time to be heated and rolled in the furnace. Generally, It takes 7 to 8 hours to heat the round billet in the steel rolling heating furnace, which increases gas consumption, resulting in increased gas costs and reduced production efficiency; 3) If the composition design is unreasonable, the heating rolling and normalizing processes are improper, resulting in low ferrite grain size and corresponding low strength indicators, which cannot meet customer requirements. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a low-cost and high-toughness 16MnDR steel for rail transit locomotive parts and a production method thereof. The 16MnDR steel has comprehensive properties such as low cost, high strength, and good low-temperature impact toughness. It can be used as steel for rail transit locomotive parts and can fully meet customer requirements.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A low-cost and high-toughness 16MnDR steel for rail transit locomotive parts comprises the following chemical components in weight percentage: C 0.16-0.20%, Si 0.25-0.45%, Mn 1.35-1.50%, V 0.025-0.040%, Nb 0.010-0.020%, P ≤ 0.015%, S ≤ 0.010%, N 0.0060-0.0080%, and the rest is Fe and unavoidable impurities.

[0007] Furthermore, it is preferred to include the following chemical compositions in weight percentage: C 0.17-0.19%, Si 0.25-0.30%, Mn 1.40-1.45%, V 0.025-0.30%, Nb 0.010-0.015%, P ≤ 0.012%, S ≤ 0.008%, N 0.0065-0.0075%, and the rest are Fe and unavoidable impurities.

[0008] The metallographic structure of the 16MnDR steel is ferrite and pearlite.

[0009] The 16MnDR steel has a tensile strength of 480-600MPa, a yield strength of ≥350MPa, and an elongation of ≥25%; at a temperature of -40°C, the longitudinal impact absorption energy KV2 is ≥120J; and the ferrite grain size of the 16MnDR steel after normalizing is above grade 7.0.

[0010] The present invention also provides a method for producing the low-cost and high-toughness 16MnDR steel for rail transit locomotive parts, which comprises the following steps: converter smelting→LF refining→RH vacuum treatment→continuous casting→heating→rolling→normalizing treatment.

[0011] Furthermore, in the converter smelting step, silicon manganese, low carbon ferromanganese, vanadium nitrogen alloy, aluminum blocks are added to the ladle when tapping steel, and aluminum wire is fed, and lime and slag-removing agent are added.

[0012] In the LF refining step, argon is blown throughout the refining process, and lime and slag-removing agent are added to control the basicity to be 4.0-6.0, S≤0.005%, and then the RH furnace can be put into vacuum.

[0013] In the RH vacuum treatment step, the holding time under the high vacuum degree of ≤100Pa is ≥12min; the lifting gas is ≥1000Nm 3 / min, pure calcium wire is fed before RH air-breaking soft blowing, and the effective soft blowing time after wire feeding is ≥15min; after the circulation is completed, the hydrogen content is controlled to be less than 1.5ppm.

[0014] In the continuous casting step, the molten steel is cast in a protective manner throughout the entire process, the temperature of the continuous casting tundish is 1525-1545°C, and the casting speed during the continuous casting process is 0.26-0.30 m / min, preferably 0.26 m / min, to ensure that the temperature of the ingot in the straightening section is ≥900°C, avoid the second type of brittle temperature range of 700-880°C, reduce the precipitation of particles such as A1N, V(C, N), and Nb(C, N) at the grain boundaries in this temperature range, reduce the plasticity of the steel, and avoid the generation of cracks. .

[0015] In the continuous casting step, the diameter of The temperature of the round billet entering the straightening section is between 915 and 930°C.

[0016] In the heating step, the ingot is hot loaded into the furnace, and the furnace temperature is controlled at above 600°C; the temperature of the preheating section of the heating furnace is 850-1100°C, the heating section is 1100-1200°C, the temperature of the soaking temperature is 1150-1200°C, and the billet is heated and kept in the furnace for 5-7 hours; water descaling is performed after leaving the heating furnace.

[0017] In the rolling step, the starting rolling temperature is 1080-1120°C. After blanking and continuous rolling, the rolled material needs to ensure that the final rolling temperature is ≥920°C for slow cooling in the pit.

[0018] In the normalizing step, the normalizing temperature is 900° C. to 920° C., and the holding time is d×1.5 min, wherein d is the diameter of the steel rod in mm.

[0019] The components of the 16MnDR steel for low-cost and high-toughness rail transit locomotive parts provided by the present invention have the following functions and controls:

[0020] C: It is an essential element to ensure the strength of 16MnDR steel. C and Fe form a cementite structure of Fe3C in steel. Therefore, C can effectively improve the strength of steel and reduce alloy cost. However, too high C content affects the ductility and toughness of steel and reduces low-temperature impact toughness. The present invention controls the carbon content to 0.16-0.20%, preferably 0.17-0.19%.

[0021] Si: It is a deoxidizing element and improves the strength of steel in the form of solid solution strengthening, but a high Si content will cause a decrease in toughness. The Si content of the present invention is controlled to be 0.25-0.45%, preferably 0.25-0.30%.

[0022] Mn: is a solid solution strengthening element, which can improve the yield strength and tensile strength of steel, and also improve the hardenability of steel. A higher manganese content reduces the welding performance of steel and increases the alloy cost. In the present invention, the Mn content is controlled at 1.35-1.50%, preferably 1.40-1.45%.

[0023] V: V is easy to combine with C and V elements in steel to form V (C / N) precipitates, which play a role of precipitation strengthening. At the same time, it can prevent the growth of austenite and ferrite grains to refine the grains. However, vanadium-nitrogen alloy is a precious metal. Adding too much will cause excess performance and cost waste. In the present invention, the content of V element is controlled at 0.025-0.040%, preferably 0.025-0.030%.

[0024] Nb: Niobium plays a major role in fine grain strengthening and dispersion strengthening in steel. A trace amount of niobium can generate stable carbides and carbonitrides with carbon and nitrogen in steel, and can also disperse carbides to form fine grain steel, thereby improving the toughness of steel. In the present invention, the Nb element content is controlled to be 0.010-0.020%, preferably 0.010-0.015%.

[0025] N: an austenite-forming element, which can combine with V to form fine dispersed vanadium nitride precipitation, which can refine the grains and strengthen the steel, thereby improving the strength. However, excessive N content can easily increase the brittleness of the steel. In the present invention, the N content is controlled within the range of N0.0060 to 0.0080%, preferably N0.0065 to 0.0075%.

[0026] P and S are harmful impurity elements in steel, which are easy to form defects such as segregation and inclusion. As impurity elements, they will have an adverse effect on the toughness of the steel plate, especially the toughness of the core and the toughness of the welding heat-affected zone, and their content should be reduced as much as possible. The present invention controls P≤0.012% and S≤0.008%.

[0027] The invention adopts reasonable alloy component design, adopts niobium-vanadium composite and increases carbon content, designs carbon content to be 0.17-0.19%, improves strength of steel under the premise of ensuring certain plasticity, and is conducive to reducing alloy cost; at the same time, the addition of Ni and Ti elements is cancelled, and V and Nb contents are designed to be lower than the level of the same industry, V is designed to be 0.025-0.040%, and Nb is designed to be 0.010-0.020%; the N content in the steel is increased, and the N content is controlled to be 60-80ppm, so as to ensure precipitation strengthening of V (C, N) and fine grain strengthening of Nb (C, N), thereby jointly improving mechanical properties of steel and reducing alloy cost.

[0028] In the production method of 16MnDR steel for rail transit locomotive parts with low cost and high toughness provided by the present invention, in the continuous casting step, low superheat and a certain pulling speed casting are adopted to ensure that the temperature of the billet entering the pulling and straightening section is ≥900°C, avoid the second type of brittle temperature range of 700-880°C, reduce the precipitation of particles such as A1N, V (C, N), Nb (C, N) and the like at the grain boundaries in the temperature range, and reduce the plasticity of the steel, which can effectively avoid the generation of billet cracks, avoid surface cracks of rolled materials, and improve the quality and yield rate of rolled materials; the billet hot delivery and hot loading rolling technology is adopted, which effectively reduces the heating time of the billet and saves fuel. Gas consumption is reduced, and energy consumption costs are reduced. At the same time, this type of steel contains crack-sensitive elements V and Nb. Hot charging can reduce the initiation of cracks in the casting caused by the rapid increase in furnace temperature after cold charging into the furnace. The hot charging process uses high-temperature heating to better shape and reshape the grains of the steel billet, so it has higher strength and toughness than the cold charging process. The use of a suitable normalizing heat treatment process can make the steel completely austenitized and obtain more fine-grained structure. The 16MnDR steel produced by this method has excellent comprehensive properties such as low cost, high strength, high and low temperature impact toughness, and is a steel for rail transit locomotive parts. The product fully meets customer requirements.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The low-cost and high-toughness 16MnDR steel for rail transit locomotive parts provided by the present invention has a low-temperature impact toughness of more than 120J at -40°C, which is much higher than the customer's standard requirement of ≥80J, and the strength index is better than the standard GB3531-2014 requirement.

[0031] The present invention adopts the design of carbon-enhanced niobium-vanadium composite composition combined with the hot charging furnace rolling technology of red hot steel billet, cancels the addition of precious alloys such as Ni and Ti, appropriately adds Nb to increase the impact toughness, and increases the nitrogen content, thereby reducing the mass percentage of manganese and vanadium components in the steel, ensuring the strength and plasticity of the steel, while reducing energy consumption costs. The 16MnDR steel for rail transit locomotive parts produced by the invention technology has high strength and good plasticity, saves production costs, and improves the economic benefits of the enterprise. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 is the metallographic structure diagram of 16MnDR steel in Example 1;

[0033] Figure 2 This is the crack morphology of the rolled material of 16MnDR steel in Comparative Example 4. DETAILED DESCRIPTION

[0034] The invention provides a low-cost and high-toughness 16MnDR steel for rail transit locomotive parts, comprising the following chemical components in weight percentage: C 0.16-0.20%, Si 0.25-0.45%, Mn 1.35-1.50%, V 0.025-0.040%, Nb 0.010-0.020%, P ≤ 0.015%, S ≤ 0.010%, N 0.0060-0.080%, and the rest is Fe and inevitable impurities.

[0035] The production method of the low-cost and high-toughness 16MnDR steel for rail transit locomotive parts is as follows: converter smelting→LF refining→RH vacuum treatment→continuous casting→heating→rolling→normalizing treatment.

[0036] In the converter smelting step, silicon manganese, low carbon ferromanganese, vanadium nitrogen alloy, aluminum blocks are added to the ladle when tapping steel, and aluminum wire is fed, and lime and slag-removing agent are added.

[0037] In the LF refining step, argon is blown throughout the refining process, lime and slag-removing agent are added to control the basicity at 4.0-6.0, and S≤0.005% is maintained after the refining is completed before the RH furnace is put into vacuum.

[0038] In the RH vacuum treatment step, the holding time under the high vacuum degree of ≤100Pa is ≥12min; the lifting gas is ≥1000Nm 3 / min, pure calcium wire is fed before RH air-breaking soft blowing, and the effective soft blowing time after wire feeding is ≥15min; after the circulation is completed, the hydrogen content is controlled to be less than 1.5ppm.

[0039] In the continuous casting step, the molten steel is cast in a protected manner throughout the entire process, the temperature of the continuous casting tundish is 1525-1545° C., and the casting speed during the continuous casting process is 0.26-0.30 m / min, preferably 0.26 m / min.

[0040] In the continuous casting step, the diameter of Round billet.

[0041] In the heating step, the ingot is hot loaded into the furnace, and the furnace temperature is controlled at above 600°C; the temperature of the preheating section of the heating furnace is 850-1100°C, the heating section is 1100-1200°C, the temperature of the soaking temperature is 1150-1200°C, and the billet is heated and kept in the furnace for 5-7 hours; water descaling is performed after leaving the heating furnace.

[0042] In the rolling step, the starting rolling temperature is 1080-1120°C. After blanking and continuous rolling, the rolled material needs to ensure that the final rolling temperature is ≥920°C for slow cooling in the pit.

[0043] In the normalizing step, the normalizing temperature is 900° C. to 920° C., and the holding time is d×1.5 min / mm, where d is the thickness of the steel bar in mm.

[0044] The present invention is described in detail below with reference to the embodiments.

[0045] The chemical composition and weight percentage of the 16MnDR steel in each embodiment and comparative example are shown in Table 1.

[0046] Table 1

[0047]

[0048]

[0049] The production method of 16MnDR steel in each embodiment and comparative example is as follows:

[0050] Example 1

[0051] A method for producing low-cost and high-toughness 16MnDR steel for rail transit locomotive parts comprises the following steps:

[0052] (1) Converter smelting: silicon-manganese alloy, low-carbon ferromanganese, ferrosilicon, vanadium-nitrogen alloy, ferroniobium alloy, and aluminum alloy are used for deoxidation and alloying. The converter tapping temperature is 1600°C. When one-third of the steel is tapped, silicon-manganese alloy, low-carbon ferromanganese, vanadium-nitrogen alloy, 50 kg of aluminum blocks / furnace are added to the ladle, and aluminum wire is fed: 200 m / furnace, lime 400 kg / furnace, and 100 kg of slag agent / furnace. All alloys and slag are added when two-thirds of the steel is tapped. The argon blowing flow rate at the bottom of the ladle is 120 NL / min, and the stirring time is 8 min to ensure that the alloy elements in the molten steel in the ladle are melted evenly and the molten steel surface is quickly slag-formed for deoxidation and absorption of inclusions.

[0053] (2) LF refining: argon is blown throughout the process, and the argon volume is controlled at 90L / min. After the refining, the outlet S is 0.004%; the LF furnace maintains white slag operation, and the slag basicity is controlled at 4.0. After the refining is completed, Ar is blown and stirred for soft blowing for 10 minutes, and then it is hoisted to RH for high vacuum degassing and inclusion removal treatment.

[0054] (3) RH vacuum treatment: maintain the high vacuum degree of ≤100Pa for 12min; increase the gas flow rate to 1100Nm 3 / min, the effective soft blowing time of molten steel after breaking the air is 15min; after the circulation is completed, the hydrogen fixing operation is carried out, and the continuous casting process can only be carried out when the mass percentage of hydrogen is ≤1.5ppm.

[0055] (4) During the round billet continuous casting step, the molten steel is protected throughout the casting process, the pouring temperature of the tundish is controlled at 1525°C, and a constant pulling speed of 0.26 m / min is adopted for pouring. The temperature of the billet entering the straightening section is 916°C. The billet is hot rolled using a conveyor roller, and the billet temperature entering the heating furnace is 650°C.

[0056] (5) Heating: The preheating temperature of the heating furnace is 995°C, the heating temperature is 1140°C, and the average heating temperature is 1150°C. The insulation time in the furnace is 6 hours. After leaving the heating furnace, high-pressure water is used to descale the surface iron oxide. The pressure of the dephosphorization water is set at 20 MPa.

[0057] (6) Rolling: The rolling temperature is 1080℃. The round billet is opened into a rectangular billet of 300*310mm. The compression ratio of the opening process is 3.038, and then rolled into a rectangular billet by a continuous rolling mill. The final rolling temperature of the round bars is 930℃, and then they are slowly cooled in the pit.

[0058] (7) Normalizing treatment: The normalizing temperature is 900℃, and the steel is kept at this temperature for 360 minutes before being air-cooled.

[0059] Example 2

[0060] A method for producing low-cost and high-toughness 16MnDR steel for rail transit locomotive parts comprises the following steps:

[0061] (1) Converter smelting: silicon-manganese alloy, low-carbon ferromanganese, ferrosilicon, vanadium-nitrogen alloy, ferroniobium alloy, and aluminum alloy are used for deoxidation and alloying. The converter tapping temperature is 1610°C. When one-third of the steel is tapped, silicon-manganese alloy, low-carbon ferromanganese, vanadium-nitrogen alloy, 50 kg of aluminum blocks / furnace are added to the ladle, and aluminum wire is fed: 200 m / furnace, lime is 400 kg / furnace, and slag agent is 100 kg / furnace. All alloys and slag are added when two-thirds of the steel is tapped. The argon blowing flow rate at the bottom of the ladle is 130 NL / min, and the stirring time is 6 min to ensure that the alloy elements in the molten steel in the ladle are melted evenly and the molten steel surface is quickly slag-formed for deoxidation and absorption of inclusions.

[0062] (2) LF refining: argon blowing throughout the process, the argon volume is controlled at 100L / min, and the outlet S is 0.003% at the end of refining; the LF furnace maintains white slag operation, and the slag basicity is controlled at 5.0. After the refining is completed, Ar blowing is required, stirring and soft blowing for 14 minutes, and then it is hoisted to RH for high vacuum degassing and inclusion removal treatment.

[0063] (3) RH vacuum treatment: maintain the high vacuum degree of ≤100Pa for 12min; increase the gas flow rate to 1200Nm 3 / min, the effective soft blowing time of molten steel after breaking the air is 18min; after the circulation is completed, the hydrogen fixing operation is carried out, and the continuous casting process can only be carried out when the mass percentage of hydrogen is ≤1.5ppm.

[0064] (4) During the round billet continuous casting step, the molten steel is protected throughout the casting process, the pouring temperature of the tundish is controlled at 1530°C, and a constant pulling speed of 0.27 m / min is adopted for pouring. The temperature of the billet entering the straightening section is 930°C. The billet is hot rolled using a conveyor roller, and the billet temperature entering the heating furnace is 610°C.

[0065] (5) Heating: The preheating temperature of the heating furnace is 900°C, the heating temperature is 1160°C, and the average heating temperature is 1180°C. The insulation time in the furnace is 6 hours. After leaving the heating furnace, high-pressure water is used to descale the surface iron oxide. The pressure of the dephosphorization water is set at 20Mpa.

[0066] (6) Rolling: The rolling temperature is 1090℃. The round billet is opened into a rectangular billet of 300*310mm. The compression ratio of the opening process is 3.038, and then rolled into a rectangular billet by a continuous rolling mill. The final rolling temperature of the round bars is 930℃, and then they are slowly cooled in the pit.

[0067] (7) Normalizing treatment: The normalizing temperature is 910℃, and the holding time is 345min before air cooling.

[0068] Example 3

[0069] A method for producing low-cost and high-toughness 16MnDR steel for rail transit locomotive parts comprises the following steps:

[0070] (1) Converter smelting: silicon-manganese alloy, low-carbon ferromanganese, ferrosilicon, vanadium-nitrogen alloy, ferroniobium alloy, and aluminum alloy are used for deoxidation and alloying. The converter tapping temperature is 1620°C. When one-third of the steel is tapped, silicon-manganese alloy, low-carbon ferromanganese, vanadium-nitrogen alloy, 50 kg of aluminum blocks / furnace are added to the ladle, and aluminum wire is fed: 200 m / furnace, lime 400 kg / furnace, and 100 kg of slag agent / furnace. All alloys and slag are added when two-thirds of the steel is tapped. The argon blowing flow rate at the bottom of the ladle is 140 NL / min, and the stirring time is 8 min to ensure that the alloy elements in the molten steel in the ladle are melted evenly and the molten steel surface is quickly slag-formed for deoxidation and absorption of inclusions.

[0071] (2) LF refining: argon is blown throughout the process, and the argon volume is controlled at 110L / min. After the refining, the outlet S is 0.002%; the LF furnace maintains white slag operation, and the slag basicity is controlled at 6.0. After the refining is completed, Ar is blown and stirred for soft blowing for 10 minutes, and then it is hoisted to RH for high vacuum degassing and inclusion removal treatment.

[0072] (3) RH vacuum treatment: maintain a high vacuum of ≤100Pa for 15min; increase the gas flow rate to 1000Nm 3 / min, the effective soft blowing time of the molten steel after breaking the air is 20min; after the circulation is completed, the hydrogen fixing operation is carried out, and the continuous casting process can only be carried out when the mass percentage of hydrogen is ≤1.5ppm.

[0073] (4) During the round billet continuous casting step, the molten steel is protected throughout the casting process, the pouring temperature of the tundish is controlled at 1535°C, and a constant pulling speed of 0.28 m / min is adopted for pouring. The temperature of the billet entering the straightening section is 912°C. The billet is hot rolled using a conveyor roller, and the billet temperature entering the heating furnace is 615°C.

[0074] (5) Heating: The preheating temperature of the heating furnace is 1000°C, the heating temperature is 1145°C, and the average temperature is 1200°C. The insulation time in the furnace is 6 hours. After leaving the heating furnace, high-pressure water is used to descale the surface iron oxide. The pressure of the dephosphorization water is set at 20 MPa.

[0075] (6) Rolling: The rolling temperature is 1110°C. The round billet is opened into a rectangular billet of 300*310mm. The compression ratio of the opening process is 3.038, and then rolled into a rectangular billet by a continuous rolling mill. The final rolling temperature of the round bars is 930℃, and then they are slowly cooled in the pit.

[0076] (7) Normalizing treatment: The normalizing temperature is 920℃, the holding time is 330min, and the steel is air-cooled after being taken out of the furnace.

[0077] Example 4

[0078] A method for producing low-cost and high-toughness 16MnDR steel for rail transit locomotive parts comprises the following steps:

[0079] (1) Converter smelting: silicon-manganese alloy, low-carbon ferromanganese, ferrosilicon, vanadium-nitrogen alloy, ferroniobium alloy, and aluminum alloy are used for deoxidation and alloying. The converter tapping temperature is 1620°C. When one-third of the steel is tapped, silicon-manganese alloy, low-carbon ferromanganese, vanadium-nitrogen alloy, 50 kg of aluminum blocks / furnace are added to the ladle, and aluminum wire is fed: 200 m / furnace, lime 400 kg / furnace, and 100 kg of slag agent / furnace. All alloys and slag are added when two-thirds of the steel is tapped. The argon blowing flow rate at the bottom of the ladle is 125 NL / min, and the stirring time is 7 minutes to ensure that the alloy elements in the molten steel in the ladle are melted evenly and the molten steel surface is quickly slag-formed for deoxidation and absorption of inclusions.

[0080] (2) LF refining: argon was blown throughout the process, and the argon volume was controlled at 105 L / min, S 0.005%; the LF furnace was kept in white slag operation, and the slag basicity was controlled at 6.0. After the refining was completed, Ar was blown and stirred for 11 minutes, and then hoisted to RH for high vacuum degassing and inclusion removal.

[0081] (3) RH vacuum treatment: maintain the high vacuum degree of ≤100Pa for 12min; increase the gas flow rate to 1100Nm 3 / min, the effective soft blowing time of the molten steel after breaking the air is 19min; after the circulation is completed, the hydrogen fixing operation is carried out, and the hydrogen mass percentage content is ≤1.5ppm before it can be transferred to the continuous casting process.

[0082] (4) During the round billet continuous casting step, the molten steel is protected throughout the casting process, the pouring temperature of the tundish is controlled at 1545°C, and a constant pulling speed of 0.26 m / min is adopted for casting. The temperature of the billet entering the straightening section is 928°C. The billet is hot rolled using a conveyor roller, and the billet temperature entering the heating furnace is 608°C.

[0083] (5) Heating: The preheating section temperature of the heating furnace is 900°C, the heating section temperature is 1150°C, the average temperature is 1175°C, and the insulation time in the furnace is 6 hours. After leaving the heating furnace, high-pressure water is used to descale the surface iron oxide. The pressure of the dephosphorization water is set at 20Mpa.

[0084] (6) Rolling: The rolling temperature is 1115°C. The round billet is opened into a rectangular billet of 300*310mm. The compression ratio of the opening process is 3.038, and then rolled into a rectangular billet by a continuous rolling mill. The round bars are rolled at a final temperature of 920°C and then slowly cooled in a pit.

[0085] (7) Normalizing treatment: Normalizing temperature is 905℃, keep warm for 375min, and then air cool after being taken out of the furnace.

[0086] Comparative Example 1

[0087] The other parts are the same as Example 4, except that the carbon component of the alloying components in the smelting process is adjusted to outside the design range of the present invention, and the carbon mass percentage is reduced to 0.14%. The obtained metallographic structure is ferrite and pearlite, but the yield strength is low.

[0088] Comparative Example 2

[0089] The rest is the same as Example 4, except that niobium-iron alloy is not added to the alloying components in the smelting process. The obtained metallographic structure is ferrite and pearlite, and the grain size grade is level 6, which does not meet the standard requirement of grain size ≥ level 7. The V-shaped longitudinal impact absorption energy KV2 in a low temperature environment of -40°C is 70J, which is lower than the KV2≥80J required by the protocol standard.

[0090] Comparative Example 3

[0091] The rest is the same as Example 1, except that vanadium-nitrogen alloy is replaced by ferrovanadium alloy during alloying in the smelting process, and the mass percentage of nitrogen is 0.0040%. The obtained metallographic structure is ferrite and pearlite, and the grain size grade is 7.0, which just meets the standard requirement of grain size ≥ 7, but the yield strength of 320 MPa does not meet the standard requirement, and the V-shaped longitudinal impact absorption energy KV2 in a low temperature environment of -40°C is 75J, which is lower than the KV2≥80J required by the protocol standard.

[0092] Comparative Example 4

[0093] The other parts are the same as in Example 3, except that the continuous casting speed is adjusted to 0.24 m / min, and the straightening temperature in the straightening zone is 870°C. Surface cracks appear on the surface of the ingot, and correspondingly, fine cracks appear on the surface of the rolled product. Figure 2 The yield strength and metallographic structure of the product meet the standard requirements.

[0094] Comparative Example 5

[0095] The rest is the same as Example 2, except that the cold steel billet after slow cooling is charged into the furnace for heating and rolling. The heating and holding time after entering the furnace is 7.5h. The metallographic structure obtained by heating is coarse ferrite and pearlite, and the grain size grade is 6.0. The corresponding mechanical property yield strength is 335MPa, which is lower than the standard requirement of 350MPa or more. The V-shaped longitudinal impact absorption energy KV2 in a low temperature environment of -40℃ is 85J, which just meets the protocol standard requirement of KV2≥80J.

[0096] Comparative Example 6

[0097] The rest is the same as Example 1, except that the holding time of the normalizing treatment is adjusted to 250 min. The obtained metallographic structure is ferrite and pearlite and a small amount of segregation bands. The grain size grade is 6.5. The corresponding mechanical property yield strength is 325 MPa, which is lower than the standard requirement of 350 MPa or more. The V-shaped longitudinal impact absorption energy KV2 in a low temperature environment of -40°C is 68 J, which is lower than the KV2≥80 J required by the protocol standard.

[0098] The properties of the 16MnDR steels produced in the above embodiments and comparative examples are shown in Table 2.

[0099] Table 2

[0100]

[0101] As can be seen from the above, the low-cost and high-toughness 16MnDR steel for rail transit locomotive parts produced by the present invention has measured yield strength (Rel), tensile strength (Rm), elongation after fracture (Ag), and -40°C low-temperature impact energy (KV2) that all meet the use requirements. The process of the present invention is simple to operate, the production cost is low, and the product has the characteristics of good matching of strength, low-temperature impact resistance and toughness.

[0102] The above-mentioned reference embodiments provide a detailed description of a low-cost and high-toughness 16MnDR steel for rail transit locomotive parts and its production method, which is illustrative rather than restrictive. Several embodiments can be listed according to the limited scope. Therefore, changes and modifications without departing from the overall concept of the present invention should fall within the scope of protection of the present invention.

Claims

1. A low-cost and high-toughness 16MnDR steel for rail transit locomotive parts, characterized in that: The invention comprises the following chemical components in weight percentage: C 0.16-0.20%, Si 0.25-0.45%, Mn 1.35-1.50%, V 0.025-0.040%, Nb 0.010-0.020%, P ≤ 0.015%, S ≤ 0.010%, N 0.0060-0.0080%, and the rest are Fe and unavoidable impurities.

2. The low-cost and high-toughness 16MnDR steel for rail transit locomotive parts according to claim 1 is characterized in that: The chemical composition includes the following weight percentages: C0.17-0.19%, Si0.25-0.30%, Mn1.40-1.45%, V0.025-0.30%, Nb0.010-0.015%, P≤0.012%, S≤0.008%, N0.0065~0.0075%, the rest is Fe and inevitable impurities.

3. The low-cost and high-toughness 16MnDR steel for rail transit locomotive parts according to claim 1 is characterized in that: The metallographic structure of the 16MnDR steel is ferrite and pearlite.

4. The low-cost and high-toughness 16MnDR steel for rail transit locomotive parts according to claim 1 is characterized in that: The 16MnDR steel has a tensile strength of 480-600MPa, a yield strength of ≥350MPa, and an elongation of ≥25%; at a temperature of -40°C, the longitudinal impact absorption energy KV2 is ≥120J; and the ferrite grain size of the 16MnDR steel after normalizing is above grade 7.

0.

5. The method for producing low-cost and high-toughness 16MnDR steel for rail transit locomotive parts according to any one of claims 1 to 4, characterized in that: The production method comprises the following steps: converter smelting→LF refining→RH vacuum treatment→continuous casting→heating→rolling→normalizing treatment.

6. The production method according to claim 5, characterized in that In the RH vacuum treatment step, the holding time under the high vacuum degree of ≤100Pa is ≥12min; the lifting gas is ≥1000Nm 3 / min, pure calcium wire is fed before RH air-breaking soft blowing, and the effective soft blowing time after wire feeding is ≥15min; after the circulation is completed, the hydrogen content is controlled to be less than 1.5ppm.

7. The production method according to claim 5, characterized in that: In the continuous casting step, the molten steel is cast in a protected manner throughout the entire process, the temperature of the continuous casting tundish is 1525-1545° C., and the casting speed during the continuous casting process is 0.26-0.30 m / min.

8. The production method according to claim 5, characterized in that: In the heating step, the billet is hot loaded into the furnace, and the temperature of the furnace is controlled to be above 600°C; the temperature of the preheating section of the heating furnace is 850-1100°C, the heating section is 1100-1200°C, the temperature of the soaking temperature is 1150-1200°C, and the billet is heated and kept in the furnace for 5-7h; After leaving the heating furnace, water descaling is carried out.

9. The production method according to claim 5, characterized in that: In the rolling step, the starting rolling temperature is 1080-1120°C. After blanking and continuous rolling, the rolled material needs to ensure that the final rolling temperature is ≥920°C for slow cooling in the pit.

10. The production method according to claim 5, characterized in that: In the normalizing step, the normalizing temperature is 900° C. to 920° C., and the holding time is d×1.5 min, wherein d is the diameter of the steel rod in mm.

Citation Information

Patent Citations

  • Normalizing type 16MnDR low temperature pressure vessel steel plate and manufacturing method thereof

    CN102605241A

  • Ultrathin 16MnDR steel plate for LNG storage tank and manufacturing method thereof

    CN110468326A