Composite hydrogen-resistant coating on surface of high-strength steel and preparation method of composite hydrogen-resistant coating

By preparing an amorphous (AlCrZr)O coating on the surface of high-strength steel, and utilizing the difference in binding energy of Al, Cr, and Zr elements, a tortuous hydrogen diffusion path is constructed, which solves the hydrogen embrittlement problem of high-strength steel in a hydrogen environment, improves the hydrogen barrier efficiency and adhesion of the coating, and broadens the application range of the product.

CN119040828AActive Publication Date: 2024-11-29UNIV OF SCI & TECH BEIJING

Patent Information

Application Number
CN202411174317.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

High-strength steel is prone to hydrogen embrittlement in hydrogen environments. Traditional hydrogen barrier coatings suffer from insufficient adhesion, poor thermal stability, and high preparation costs, and their performance optimization is inadequate.

Method used

By utilizing the difference in binding energies between Al, Cr, and Zr and hydrogen, an amorphous (AlCrZr)O coating was prepared on the surface of high-strength steel using magnetron sputtering technology. This process constructed a tortuous hydrogen diffusion path and a high hydrogen diffusion barrier, forming a composite coating consisting of a transition layer and a hydrogen barrier layer.

Benefits of technology

It significantly improves the hydrogen embrittlement resistance of high-strength steel, enhances the adhesion and hydrogen barrier efficiency of the coating, broadens the application range and processability of the product, and meets the mechanical performance requirements of high-strength steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040828A_ABST
    Figure CN119040828A_ABST
Patent Text Reader

Abstract

The invention provides a high-strength steel surface composite hydrogen-resistant coating and a preparation method thereof. Belongs to the field of metal material surface modification, and the hardness of the high-strength steel is HV300-HV600, the tensile strength is 900-1200 MPa, the maximum thermal expansion coefficient can be (8-20) * 10 <-6 > / K, and the elastic modulus is 100-200 GPa. The composite hydrogen-resistant coating is composed of a transition layer and a hydrogen-resistant layer, the transition layer is composed of three elements of Al, Cr and Zr, the molar ratio of each element is not less than 30%, and the hydrogen-resistant layer is composed of oxides of Al, Cr and Zr and a part of unoxidized metal; the transition layer and the hydrogen blocking layer are of an amorphous structure. According to the coating, a material system with a zigzag hydrogen diffusion path and a high hydrogen diffusion barrier is constructed by utilizing the binding energy difference between three elements of Al, Cr and Zr and hydrogen. Through the magnetron sputtering technology, the (AlCrZr) O coating of an amorphous structure can be prepared on the surface of the high-strength steel, effective blocking and capturing of hydrogen atoms are achieved, and the hydrogen embrittlement resistance of the material is remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal material surface modification, and particularly relates to a high-strength steel surface composite hydrogen barrier coating and a preparation method thereof. Background Art

[0002] With the transformation of the global energy structure, the development and application of hydrogen energy as a clean and efficient energy form is receiving more and more attention. In the storage, transportation and application of hydrogen energy, metal materials, as key structural materials, are of vital importance for their safety and reliability. However, the hydrogen embrittlement of metal materials in a hydrogen environment, that is, hydrogen atoms penetrate into the metal lattice and cause the material to become embrittled, has become the main obstacle to its widespread application in the field of hydrogen energy.

[0003] Hydrogen embrittlement can lead to reduced plasticity and fracture toughness of metal materials, and even catastrophic failure in severe cases. In particular, the hydrogen embrittlement problem is particularly prominent in high-strength steel materials due to their wide application in hydrogen-related environments, such as hydrogen storage tanks for hydrogen fuel vehicles and pressure vessels at hydrogen refueling stations. Traditional solutions, such as material alloying and microstructure optimization, can improve the material's resistance to hydrogen embrittlement to a certain extent, but they are often difficult to meet the increasingly stringent application requirements.

[0004] In recent years, surface coating technology has attracted great attention from researchers as an effective means of material modification. By applying a hydrogen barrier coating on the surface of metal materials, the permeability of hydrogen can be effectively reduced, thereby slowing down or preventing the occurrence of hydrogen embrittlement. The hydrogen barrier coating forms a physical barrier, prolongs the diffusion path of hydrogen atoms in the material, increases the diffusion barrier, and thus reduces the concentration of hydrogen atoms inside the material, reducing the risk of hydrogen embrittlement.

[0005] Although a variety of hydrogen barrier coatings have been studied and applied, such as metal coatings, oxide coatings, carbide coatings, etc., they still have some problems in practical applications, such as insufficient bonding with the substrate material, poor thermal stability of the coating, high preparation cost, etc. In addition, the hydrogen barrier mechanism of existing coatings is not fully understood, and there is still much room for optimization and improvement of coating performance. Summary of the invention

[0006] In view of the deficiencies in the above-mentioned prior art, the present invention provides a composite hydrogen barrier coating on the surface of high-strength steel and a preparation method thereof. The coating utilizes the difference in binding energy between the three elements Al, Cr, and Zr and hydrogen to construct a material system with a tortuous hydrogen diffusion path and a high hydrogen diffusion barrier. By using magnetron sputtering technology, an (AlCrZr)O coating with an amorphous structure can be prepared on the surface of high-strength steel to effectively block and capture hydrogen atoms, significantly improving the material's resistance to hydrogen embrittlement.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows: a composite hydrogen barrier coating on the surface of a high-strength steel, wherein the hardness of the high-strength steel is HV300-HV600, the tensile strength is 900-1200MPa, and the thermal expansion coefficient can be up to (8-20)×10 -6 / K, and the elastic modulus is between 100-200GPa; the composite hydrogen barrier coating consists of a transition layer and a hydrogen barrier layer, the transition layer consists of three elements, Al, Cr, and Zr, and the molar ratio of each element is not less than 30%, and the hydrogen barrier layer consists of Al, Cr, Zr oxides and some unoxidized metals; the transition layer and the hydrogen barrier layer are amorphous structures.

[0008] Furthermore, the thickness of the transition layer is 20-30 μm; the thickness of the hydrogen barrier layer is 80-170 μm.

[0009] On the other hand, the present invention provides a method for preparing the above-mentioned composite hydrogen barrier coating, comprising: selecting high-strength steel and a target material, and pretreating the surface of the high-strength steel to be coated; and coating the surface to be coated by magnetron sputtering.

[0010] Furthermore, the target material includes an AlCr target and a Zr target.

[0011] Furthermore, the pretreatment includes: using 400# to 5000# SiC sandpaper to polish the surface of the high-strength steel to be coated step by step until there are no voids and large scratches on the surface, and then mirror polishing with diamond polishing paste. The surface roughness of the prepared product is less than 0.16μm. Finally, the sample is soaked and cleaned with deionized water, anhydrous ethanol and acetone in an ultrasonic cleaner for 10-30 minutes and then dried.

[0012] Furthermore, the magnetron sputtering process includes vacuuming, bias cleaning and coating; the vacuum degree after vacuuming is not greater than 2.0×10 -3 Pa.

[0013] Furthermore, the bias cleaning process is as follows: the substrate is heated at a preparation temperature of 180-220°C, and the vacuum degree in the chamber is not greater than 1.8×10 -3 When 0.040 ℃ and 0.080 ℃, the stop valve is opened, the limiting valve parameter is set to 100°, the argon flow rate is set to 30 sccm, the voltage is set to -900 V, and the pressure in the chamber is maintained above 1.0 Pa for bias cleaning. The cleaning time is not less than 10 min.

[0014] Furthermore, the coating process of the transition layer is as follows: the argon flow rate is set to 25-30sccm, the AlCr target power is 140-160W, the Zr target power is 90-110W, the chamber working pressure is 0.4-0.6Pa, the substrate rotation speed is 9-11r / min, the deposition temperature is 180-220°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100V, and the deposition time is 4-6min.

[0015] Furthermore, the coating process of the hydrogen barrier layer is as follows: the argon flow rate is set to 25-30 sccm, the AlCr target power is 140-160 W, the Zr target power is 90-110 W, the chamber working pressure is 0.4-0.6 Pa, the substrate rotation speed is 9-11 r / min, the deposition temperature is 180-220 ° C, the bias voltage of the magnetron sputtering equipment is adjusted to -100 V, the oxygen flow rate is adjusted to 7-8 sccm, the deposition time is 7-8 min, the oxygen flow rate is adjusted to 5-6 sccm, the deposition time is 5-6 min, the oxygen flow rate is adjusted to 2-3 sccm, and the deposition time is 16-18 min.

[0016] Furthermore, the coating process of the hydrogen barrier layer is as follows: the argon flow rate is set to 30 sccm, the AlCr target power is 150 W, the Zr target power is 100 W, the chamber working pressure is 0.5 Pa, the substrate rotation speed is 10 r / min, the deposition temperature is 200°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100 V, the oxygen flow rate is adjusted to 8 sccm, the deposition time is 7 min, the oxygen flow rate is adjusted to 5 sccm, the deposition time is 5 min, the oxygen flow rate is adjusted to 3 sccm, and the deposition time is 18 min.

[0017] Compared with the prior art, the technical solution provided by the present invention brings the following beneficial effects:

[0018] (1) The present invention uses three elements, Al, Cr, and Zr, which have significant differences in binding energy with hydrogen. This difference is the basis for constructing a tortuous hydrogen diffusion path and a high hydrogen diffusion barrier, which is crucial for slowing down the diffusion rate of hydrogen in the material. By magnetron sputtering technology, an AlCrZr coating with an amorphous structure can be prepared. The amorphous structure lacks grain boundaries, thereby reducing the rapid diffusion channel of hydrogen and further improving the hydrogen barrier efficiency of the coating. Compared with a single metal oxide coating, the AlCrZr series oxide coating not only improves the cohesion of the coating through the synergistic effect of multiple elements, but also enhances the coating's ability to adsorb and capture hydrogen, thereby performing better in inhibiting hydrogen penetration; while the high entropy alloy oxide coating has complex interactions between elements, difficult-to-control lattice distortion, and unpredictable hydrogen diffusion behavior caused by its multi-element composition, while the AlCrZr series medium entropy alloy oxide coating optimizes the interactions between elements and reduces unfavorable lattice distortion through a carefully designed element composition, thereby providing a more stable hydrogen diffusion path.

[0019] (2) The coating provided by the present application utilizes the difference in binding energy between the three elements Al, Cr, and Zr and hydrogen to construct a material system with a tortuous hydrogen diffusion path and a high hydrogen diffusion barrier. Through magnetron sputtering technology, an (AlCrZr)O coating with an amorphous structure can be prepared on the surface of high-strength steel to effectively block and capture hydrogen atoms, significantly improving the material's resistance to hydrogen embrittlement.

[0020] (3) With respect to the high-strength steel of the prior art, the high-strength steel has the following physical properties: hardness of HV300-HV600, tensile strength of 900-1200 MPa, and thermal expansion coefficient of up to (8-20)×10 -6 / K, due to the high mechanical performance indicators, it is difficult to directly plate the coating through the technical solutions disclosed in the prior art, and in order to meet the subsequent processing requirements, a certain degree of processing is required after the coating is plated. The composite hydrogen barrier coating prepared by the technical solution of the present application can meet the requirement that when the thickness of the high-strength steel is within 5mm, the minimum bending radius is 2cm, and no cracks will be generated between the coating and the surface of the high-strength steel, which greatly broadens the scope of application and machinability of subsequent products. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0022] Figure 1This is a SEM image of the surface morphology of the composite hydrogen barrier coating provided in Example 1 of the present invention, where a is the coating surface and b is the cross section;

[0023] Figure 2 XPS fine spectrum of the composite hydrogen barrier coating provided in an embodiment of the present invention;

[0024] Figure 3 This is the hydrogen permeation curve of the composite hydrogen barrier coating provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0025] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. The specific implementation of the present invention is not limited to the specific embodiments given here, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the disclosed specific embodiments.

[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and do not limit the present invention.

[0027] An embodiment of the present invention provides a composite hydrogen barrier coating on the surface of a high-strength steel, wherein the hardness of the high-strength steel is HV300-HV600, the tensile strength is 900-1200MPa, the thermal expansion coefficient can be up to (8-20)×10-6 / K, and the elastic modulus is between 100-200GPa; the composite hydrogen barrier coating is composed of a transition layer and a hydrogen barrier layer, the transition layer is composed of three elements of Al, Cr, and Zr, and the molar ratio of each element is not less than 30%, and the hydrogen barrier layer is composed of Al, Cr, Zr oxides and some unoxidized metals; the transition layer and the hydrogen barrier layer are amorphous structures.

[0028] Firstly, the three elements Al, Cr and Zr used in the present invention have significant differences in binding energy with hydrogen. This difference is the basis for constructing a tortuous hydrogen diffusion path and a high hydrogen diffusion barrier, which is crucial for slowing down the diffusion rate of hydrogen in the material. By magnetron sputtering technology, an AlCrZr coating with an amorphous structure can be prepared. The amorphous structure lacks grain boundaries, thereby reducing the rapid diffusion channel of hydrogen and further improving the hydrogen barrier efficiency of the coating. Compared with a single metal oxide coating, the AlCrZr-based oxide coating not only improves the coating's cohesion through the synergistic effect of multiple elements, but also enhances the coating's ability to adsorb and capture hydrogen, thereby performing better in inhibiting hydrogen penetration; while the high-entropy alloy oxide coating, due to its multi-element composition, has problems such as complex interactions between elements, difficult-to-control lattice distortion, and unpredictable hydrogen diffusion behavior caused by this, while the AlCrZr-based medium-entropy alloy oxide coating optimizes the interactions between elements through a carefully designed element composition, reduces unfavorable lattice distortion, and thus provides a more stable hydrogen diffusion path; secondly, the coating provided in the present application utilizes the difference in binding energy between the three elements Al, Cr, and Zr and hydrogen to construct a material system with a tortuous hydrogen diffusion path and a high hydrogen diffusion barrier. Through magnetron sputtering technology, an (AlCrZr)O coating with an amorphous structure can be prepared on the surface of high-strength steel to effectively block and capture hydrogen atoms, significantly improving the material's resistance to hydrogen embrittlement. Again, for the high-strength steel in the prior art, the high-strength steel has the following physical properties: hardness of HV300-HV600, tensile strength of 900-1200MPa, and thermal expansion coefficient of up to (8-20)×10 -6 / K, due to the high mechanical performance indicators, it is difficult to directly plate the coating through the technical solutions disclosed in the prior art, and in order to meet the subsequent processing requirements, a certain degree of processing is required after the coating is plated. The composite hydrogen barrier coating prepared by the technical solution of the present application can meet the requirement that when the thickness of the high-strength steel is within 5mm, the minimum bending radius is 2cm, and no cracks will be generated between the coating and the surface of the high-strength steel, which greatly broadens the scope of application and machinability of subsequent products.

[0029] It should be noted that the high-strength steel in the present invention is 12Cr2Mo1R steel or 17-4PH.

[0030] Specifically, the thickness of the transition layer is 20-30μm; the thickness of the hydrogen barrier layer is 80-170μm. The hydrogen barrier layer should not be too thin. Although it increases the manufacturing efficiency, the hydrogen barrier performance is weakened. It should be pointed out that there is no redundant transition distance between the hydrogen barrier layer and the transition layer, which is easy to cause cracks between the hydrogen barrier layer and the high-strength steel substrate or the transition layer during the subsequent bending process. However, the hydrogen barrier coating should not be too thick. Too thick increases the preparation time, and since the hydrogen barrier layer is a metal oxide layer, the brittleness increases the probability of cracks on the outer surface of the coating. The transition layer is used to coordinate the deformation of the hydrogen barrier layer and the high-strength steel substrate at different temperatures to prevent the deformation between the two from being inconsistent and causing cracks at the interface. Compared with (AlCrZr)O, AlCrZr is more tightly bonded to the high-strength steel substrate. Therefore, when the transition layer is set to 20-30μm, it can not only meet the above conditions, but also reduce the thickness of the transition layer, avoiding the composite hydrogen barrier coating from being too thick and affecting the bending performance indicators of the prepared product.

[0031] The present invention also provides a method for preparing the above-mentioned composite hydrogen barrier coating, comprising:

[0032] S1 selects high-strength steel and a target material, and pre-treats the surface of the high-strength steel to be coated.

[0033] Specifically, for illustration, in the present invention, the high-strength steel is selected from 12Cr2Mo1R and 17-4PH, and the components of the 12Cr2Mo1R steel and their mass percentages are as follows: C: 0.14%, Si: 0.12%, Mn: 0.57%, P: 0.01%, Cr: 2.64%, Ni: 0.02%, Co: 3.67%, Nb: 0.01%, Al: 0.07%.

[0034] The components of the 17-4PH and their mass percentages are as follows: C: 0.03%, Si: 0.56%, Mn: 0.51%, P: 0.02%, Cr: 16.75%, Ni: 3.99%, Cu: 3.67%, Nb: 0.28%.

[0035] The target material is a 99.99% pure metal AlCr composite target (φ76.2×5mm 3 ) and a Zr target with a purity of 99.99% (φ76.2×5mm 3 ).

[0036] The pretreatment includes: using 400# to 5000# SiC sandpaper to grind the surface of the 12Cr2Mo1R steel to be coated step by step until there are no cavities and large scratches on the surface, and then using diamond polishing paste to perform mirror polishing. The surface roughness of the prepared product is less than 0.16μm. Finally, using an ultrasonic cleaner to soak and clean the sample with deionized water, anhydrous ethanol and acetone in turn for 10-30 minutes and then drying.

[0037] S2 uses magnetron sputtering to coat the surface to be coated.

[0038] The magnetron sputtering process includes vacuuming, bias cleaning, plating a transition layer and plating a hydrogen barrier layer; the vacuum degree after vacuuming is not greater than 2.0×10 -3 Pa.

[0039] The bias cleaning process is as follows: setting the preparation temperature to 180-220°C to heat the substrate, and when the vacuum degree in the chamber is not greater than 1.8×10 -3 When the pressure is 0.04 Pa, open the stop valve, set the flow limit valve parameter to 100°, set the argon flow rate to 30 sccm, set the voltage to -900 V, keep the pressure in the chamber above 1.0 Pa for bias cleaning, and the cleaning time is not less than 10 minutes. Ensure that the contaminants on the substrate surface can be removed, the substrate surface can be activated, and the adhesion of the coating can be guaranteed.

[0040] The coating process of the transition layer is as follows: the argon flow rate is set to 25-30sccm, the AlCr target power is 140-160W, the Zr target power is 90-110W, the chamber working pressure is 0.4-0.6Pa, the substrate rotation speed is 9-11r / min, the deposition temperature is 180-220°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100V, and the deposition time is 4-6min.

[0041] The coating process of the hydrogen barrier layer is as follows: the argon flow rate is set to 25-30 sccm, the AlCr target power is 140-160W, the Zr target power is 90-110W, the chamber working pressure is 0.4-0.6Pa, the substrate rotation speed is 9-11r / min, the deposition temperature is 180-220°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100V, the oxygen flow rate is adjusted to 7-8sccm, the deposition time is 7-8min, the oxygen flow rate is adjusted to 5-6sccm, the deposition time is 5-6min, the oxygen flow rate is adjusted to 2-3sccm, and the deposition time is 16-18min.

[0042] Preferably, the coating process of the hydrogen barrier layer is: setting the argon flow rate to 30 sccm, the AlCr target power to 150 W, the Zr target power to 100 W, the chamber working pressure to 0.5 Pa, the substrate rotation speed to 10 r / min, the deposition temperature to 200°C, adjusting the bias voltage of the magnetron sputtering equipment to -100 V, adjusting the oxygen flow rate to 8 sccm, the deposition time to 7 min, adjusting the oxygen flow rate to 5 sccm, the deposition time to 5 min, adjusting the oxygen flow rate to 3 sccm, and the deposition time to 18 min.

[0043] The above preparation method can prepare the composite hydrogen barrier coating with a surface (AlCrZr)O in which the metal atoms are oxidized to the extent that Al and Zr are completely oxidized, Cr is oxidized by more than 70%, and the oxygen ion content is at least 75%.

[0044] In the embodiment of the present invention, the performance of the prepared composite hydrogen barrier coating is tested, including:

[0045] Penetration current density: Tested in accordance with the national standard “Determination of hydrogen permeability of metallic materials Part 1: Steady-state current method” (GB / T 35439.1-2017).

[0046] In order to further illustrate the present invention, a wide temperature range multiphase low expansion lightweight aluminum-based composite material provided by the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0047] Example 1

[0048] The embodiment of the present invention prepares a composite hydrogen barrier coating on the surface of high-strength steel, and the preparation method thereof includes:

[0049] S1 selects high-strength steel and a target material, and pre-treats the surface of the high-strength steel to be coated.

[0050] 12Cr2Mo1R steel and target material are used to polish and clean the surface of the 12Cr2Mo1R steel to be coated.

[0051] S2 uses magnetron sputtering to coat the surface to be coated.

[0052] Turn on the magnetron sputtering equipment, place the substrate material on the sample stage of the substrate stage, close the chamber door and evacuate the chamber to a vacuum degree of 2.0×10 -3 Below Pa.

[0053] The bias cleaning process is as follows: 12Cr2Mo1R steel is heated and bias cleaned. The preparation temperature is set to 200°C and the 12Cr2Mo1R steel is heated. When the predetermined temperature is reached and the vacuum degree in the chamber is 1.8×10 -3When 0.04°C / 6.08°C is reached, the stop valve is opened, the flow limiting valve parameter is set to 100° (the adjustment range is 0-1000°), the argon flow rate is set to 30 sccm, and the voltage is set to -900 V to keep the pressure in the chamber above 1.0 Pa for bias cleaning. The surface of 12Cr2Mo1R steel is first bombarded with Ar+ particles for 10 minutes to ensure that the contaminants on the surface of 12Cr2Mo1R steel can be removed, the surface of 12Cr2Mo1R steel can be activated, and the adhesion of the coating can be guaranteed.

[0054] The coating process of the transition layer is as follows: the argon flow rate is set to 30 sccm, the AlCr target power is 150 W, the Zr target power is 100 W, the chamber working pressure is 0.5 Pa, the substrate rotation speed is 10 r / min, the deposition temperature is 200°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100 V, the deposition time is 5 min, and the thickness of the prepared transition layer is 24 μm.

[0055] The coating process of the hydrogen barrier layer is as follows: set the argon flow rate to 30sccm, the AlCr target power to 150W, the Zr target power to 100W, the chamber working pressure to 0.5Pa, the substrate speed to 10r / min, the deposition temperature to 200°C, adjust the bias voltage of the magnetron sputtering device to -100V, adjust the oxygen flow rate to 8sccm, the deposition time to 7min, adjust the oxygen flow rate to 5sccm, the deposition time to 5min, adjust the oxygen flow rate to 3sccm, and the deposition time to 18min. The morphology of the prepared composite hydrogen barrier coating is shown in the figure. Figure 1 As shown in Figs. a and 1b, the thickness of the prepared hydrogen barrier layer is 124 μm. In summary, the total thickness of the composite hydrogen barrier coating is 148 μm.

[0056] The prepared coating has an amorphous structure, such as Figure 2 The present invention performs XPS detection on different oxygen flow rates, and it can be seen that on the surface of the composite hydrogen barrier coating (AlCrZr)O, part of the Cr is not completely oxidized, and the oxygen ion content is 77.5%; Figure 3 As shown in the figure, under different oxygen flow rates at the end of the preparation process, the minimum permeation current density is obtained when the oxygen flow rate is 3 sccm, and the permeation current density is: 0.21 μA·cm -2 ; Through testing, when the thickness of high-strength steel is 5mm, the minimum bending radius is 2cm, and there is no crack at the interface between the composite hydrogen barrier coating and the 12Cr2Mo1R steel substrate.

[0057] Example 2

[0058] The embodiment of the present invention prepares a composite hydrogen barrier coating on the surface of high-strength steel, and the preparation method thereof includes:

[0059] S1 selects high-strength steel and a target material, and pre-treats the surface of the high-strength steel to be coated.

[0060] 12Cr2Mo1R steel and target material are used to polish and clean the surface of the 12Cr2Mo1R steel to be coated.

[0061] S2 uses magnetron sputtering to coat the surface to be coated.

[0062] Turn on the magnetron sputtering equipment, place the substrate material on the sample stage of the substrate stage, close the chamber door and evacuate the chamber to a vacuum degree of 2.0×10 -3 Below Pa.

[0063] The bias cleaning process is as follows: 12Cr2Mo1R steel is heated and bias cleaned. The preparation temperature is set to 200°C and the 12Cr2Mo1R steel is heated. When the predetermined temperature is reached and the vacuum degree in the chamber is 1.8×10 -3 When 0.04°C / 6.08°C is reached, the stop valve is opened, the flow limiting valve parameter is set to 100° (the adjustment range is 0-1000°), the argon flow rate is set to 30 sccm, and the voltage is set to -900 V to keep the pressure in the chamber above 1.0 Pa for bias cleaning. The surface of 12Cr2Mo1R steel is first bombarded with Ar+ particles for 10 minutes to ensure that the contaminants on the surface of 12Cr2Mo1R steel can be removed, the surface of 12Cr2Mo1R steel can be activated, and the adhesion of the coating can be guaranteed.

[0064] The coating process of the transition layer is as follows: the argon flow rate is set to 25 sccm, the AlCr target power is 140 W, the Zr target power is 90 W, the chamber working pressure is 0.4 Pa, the substrate rotation speed is 9 r / min, the deposition temperature is 180°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100 V, the deposition time is 4 min, and the thickness of the prepared transition layer is 20 μm.

[0065] The coating process of the hydrogen barrier layer is as follows: set the argon flow rate to 25sccm, the AlCr target power to 140W, the Zr target power to 90W, the chamber working pressure to 0.4Pa, the substrate speed to 9r / min, the deposition temperature to 180°C, adjust the bias voltage of the magnetron sputtering equipment to -100V, adjust the oxygen flow rate to 7sccm, the deposition time to 7min, adjust the oxygen flow rate to 5sccm, the deposition time to 5min, adjust the oxygen flow rate to 2sccm, and the deposition time to 16min. The thickness of the prepared hydrogen barrier layer is 80μm. In summary, the total thickness of the composite hydrogen barrier coating is 100μm.

[0066] The prepared coating has an amorphous structure. The surface of the composite hydrogen barrier coating is (AlCrZr)O. Some Cr is not completely oxidized. The oxidation degree of Cr is 77% and the oxygen ion content is 80%. The permeation current density of the sample is measured to be: 0.31μA·cm -2; Through testing, when the thickness of high-strength steel is 5mm, the minimum bending radius is 2cm, and there is no crack at the interface between the composite hydrogen barrier coating and the 12Cr2Mo1R steel substrate.

[0067] Example 3

[0068] The embodiment of the present invention prepares a composite hydrogen barrier coating on the surface of high-strength steel, and the preparation method thereof includes:

[0069] S1 selects high-strength steel and a target material, and pre-treats the surface of the high-strength steel to be coated.

[0070] 12Cr2Mo1R steel and target material are used to polish and clean the surface of the 12Cr2Mo1R steel to be coated.

[0071] S2 uses magnetron sputtering to coat the surface to be coated.

[0072] Turn on the magnetron sputtering equipment, place the substrate material on the sample stage of the substrate stage, close the chamber door and evacuate the chamber to a vacuum degree of 2.0×10 -3 Below Pa.

[0073] The bias cleaning process is as follows: 12Cr2Mo1R steel is heated and bias cleaned. The preparation temperature is set to 200°C and the 12Cr2Mo1R steel is heated. When the predetermined temperature is reached and the vacuum degree in the chamber is 1.8×10 -3 When 0.04°C / 6.08°C is reached, the stop valve is opened, the flow limiting valve parameter is set to 100° (the adjustment range is 0-1000°), the argon flow rate is set to 30 sccm, and the voltage is set to -900 V to keep the pressure in the chamber above 1.0 Pa for bias cleaning. The surface of 12Cr2Mo1R steel is first bombarded with Ar+ particles for 10 minutes to ensure that the contaminants on the surface of 12Cr2Mo1R steel can be removed, the surface of 12Cr2Mo1R steel can be activated, and the adhesion of the coating can be guaranteed.

[0074] The coating process of the transition layer is as follows: the argon flow rate is set to 30 sccm, the AlCr target power is 160 W, the Zr target power is 110 W, the chamber working pressure is 0.6 Pa, the substrate rotation speed is 11 r / min, the deposition temperature is 220°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100 V, the deposition time is 6 min, and the thickness of the prepared transition layer is 30 μm.

[0075] The coating process of the hydrogen barrier layer is as follows: set the argon flow rate to 30sccm, the AlCr target power to 160W, the Zr target power to 110W, the chamber working pressure to 0.6Pa, the substrate rotation speed to 11r / min, the deposition temperature to 220°C, adjust the bias voltage of the magnetron sputtering equipment to -100V, adjust the oxygen flow rate to 8sccm, the deposition time to 8min, adjust the oxygen flow rate to 6sccm, the deposition time to 6min, adjust the oxygen flow rate to 3sccm, and the deposition time to 18min. The thickness of the prepared hydrogen barrier layer is 170μm. In summary, the total thickness of the composite hydrogen barrier coating is 200μm. In summary, the total thickness of the composite hydrogen barrier coating is 200μm.

[0076] The prepared coating has an amorphous structure. The surface of the composite hydrogen barrier coating is (AlCrZr)O. Some Cr is not completely oxidized. The oxidation degree of Cr is 74% and the oxygen ion content is 75%. The permeation current density of the sample is measured to be: 0.53μA·cm -2 ; Through testing, when the thickness of high-strength steel is 5mm, the minimum bending radius is 2cm, and there is no crack at the interface between the composite hydrogen barrier coating and the 12Cr2Mo1R steel substrate.

[0077] Example 4

[0078] The embodiment of the present invention prepares a composite hydrogen barrier coating on the surface of high-strength steel, and the preparation method thereof includes:

[0079] S1 selects high-strength steel and a target material, and pre-treats the surface of the high-strength steel to be coated.

[0080] Using 17-4PH steel and target material, the surface of 17-4PH steel to be coated is polished and cleaned.

[0081] S2 uses magnetron sputtering to coat the surface to be coated.

[0082] Turn on the magnetron sputtering equipment, place the base material on the sample table of the substrate table, close the chamber door and evacuate the chamber to a vacuum degree below 2.0×10-3Pa.

[0083] The bias cleaning process is as follows: heat and bias clean the 17-4PH steel, set the preparation temperature to 200°C and start heating the 17-4PH steel. When the predetermined temperature is reached and the vacuum degree in the chamber is 1.8×10-3Pa, open the stop valve, set the limiting valve parameter to 100° (the adjustment range is 0-1000°), set the argon flow rate to 30sccm, set the voltage to -900V, and keep the pressure in the chamber above 1.0Pa for bias cleaning. First, bombard the surface of the 17-4PH steel with Ar+ particles for 10 minutes to ensure that the contaminants on the surface of the 17-4PH steel can be removed, the surface of the 17-4PH steel can be activated, and the adhesion of the coating can be guaranteed.

[0084] The coating process of the transition layer is as follows: the argon flow rate is set to 30 sccm, the AlCr target power is 150 W, the Zr target power is 100 W, the chamber working pressure is 0.5 Pa, the substrate rotation speed is 10 r / min, the deposition temperature is 200°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100 V, the deposition time is 5 min, and the thickness of the prepared transition layer is 23.8 μm.

[0085] The coating process of the hydrogen barrier layer is as follows: set the argon flow rate to 30sccm, the AlCr target power to 150W, the Zr target power to 100W, the chamber working pressure to 0.5Pa, the substrate speed to 10r / min, the deposition temperature to 200°C, adjust the bias voltage of the magnetron sputtering equipment to -100V, adjust the oxygen flow rate to 8sccm, the deposition time to 7min, adjust the oxygen flow rate to 5sccm, the deposition time to 5min, adjust the oxygen flow rate to 3sccm, and the deposition time to 18min. The thickness of the prepared hydrogen barrier layer is 122μm. In summary, the total thickness of the composite hydrogen barrier coating is 145.8μm.

[0086] The prepared coating has an amorphous structure. The surface of the composite hydrogen barrier coating is (AlCrZr)O. Some Cr is not completely oxidized. The oxidation degree of Cr is 76.0%, and the oxygen ion content is 77.5%. The permeation current density of the sample is measured to be: 0.27μA·cm -2 ; Through testing, when the thickness of high-strength steel is 5mm, the minimum bending radius is 2cm, and there is no crack at the interface between the composite hydrogen barrier coating and the 17-4PH steel substrate.

[0087] Comparative Example 1

[0088] Different from Example 1, in step S2 of this comparative example, the deposition time of the transition layer is 17 min, and the thickness of the prepared transition layer is 18 μm.

[0089] The prepared coating has an amorphous structure; through testing, it was found that cracks existed in the composite hydrogen barrier coating when the thickness of the high-strength steel was 5 mm and the bending radius was 15 cm.

[0090] Comparative Example 2

[0091] Different from Example 1, in step S2 of this comparative example, the deposition time of the transition layer is 20 min, and the thickness of the prepared transition layer is 34 μm.

[0092] The prepared coating has an amorphous structure; through testing, it was found that when the thickness of the high-strength steel was 5 mm and the bending radius was 15 cm, cracks existed on the outer surface of the composite hydrogen barrier coating.

[0093] Comparative Example 3

[0094] Different from Example 1, in step S2 of this comparative example, an oxygen flow rate of 8 sccm and a deposition time of 30 min are used.

[0095] The prepared coating has an amorphous structure; through testing, when the thickness of the high-strength steel is 5 mm and the bending radius is 20 cm, cracks exist between the hydrogen barrier layer and the transition layer, Al, Cr and Zr are not completely oxidized, and the oxygen ion content is 60%.

[0096] Comparative Example 4

[0097] Different from Example 1, in step S2 of this comparative example, an oxygen flow rate of 3 sccm and a deposition time of 30 min are used.

[0098] The prepared coating has an amorphous structure; through testing, it was found that when the thickness of the high-strength steel was 5 mm and the bending radius was 25 cm, cracks existed between the hydrogen barrier layer and the transition layer.

[0099] Comparative Example 5

[0100] Different from Example 1, in step S2 of this comparative example, the oxygen flow rate is adjusted to 8 sccm and the deposition time is 7 min, and the oxygen flow rate is adjusted to 3 sccm and the deposition time is 23 min.

[0101] The prepared coating has an amorphous structure; through testing, it was found that when the thickness of the high-strength steel was 5 mm and the bending radius was 10 cm, cracks existed between the hydrogen barrier layer and the transition layer.

[0102] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A composite hydrogen barrier coating on the surface of high-strength steel, characterized in that: The hardness of the high-strength steel is HV300-HV600, the tensile strength is 900-1200MPa, and the thermal expansion coefficient can be up to (8-20)×10 -6 / K, elastic modulus between 100-200GPa; The composite hydrogen barrier coating is composed of a transition layer and a hydrogen barrier layer, wherein the transition layer is composed of three elements, Al, Cr, and Zr, and the molar ratio of each element is not less than 30%, and the hydrogen barrier layer is composed of Al, Cr, Zr oxides and part of unoxidized metal; The transition layer and the hydrogen barrier layer are amorphous structures.

2. The composite hydrogen barrier coating according to claim 1, characterized in that: The thickness of the transition layer is 20-30 μm; the thickness of the hydrogen barrier layer is 80-170 μm.

3. A method for preparing a composite hydrogen barrier coating as claimed in claim 1 or 2, characterized in that: include: Selecting high-strength steel and a target material, and pretreating the surface of the high-strength steel to be coated; The surface to be coated is coated by magnetron sputtering.

4. The preparation method according to claim 3, characterized in that: The target materials include AlCr target and Zr target.

5. The preparation method according to claim 3, characterized in that: The pretreatment includes: using 400# to 5000# SiC sandpaper to grind the surface of the high-strength steel to be coated step by step until there are no cavities and large scratches on the surface, and then using diamond polishing paste to perform mirror polishing. The surface roughness of the prepared product is less than 0.16μm. Finally, using an ultrasonic cleaner to soak and clean the sample with deionized water, anhydrous ethanol and acetone in turn for 10-30 minutes and then drying.

6. The preparation method according to claim 3, characterized in that: The magnetron sputtering process includes vacuuming, bias cleaning, plating a transition layer and plating a hydrogen barrier layer; The vacuum degree after vacuuming is not greater than 2.0×10 -3 Pa.

7. The preparation method according to claim 6, characterized in that: The bias cleaning process is as follows: setting the preparation temperature to 180-220°C to heat the substrate, and when the vacuum degree in the chamber is not greater than 1.8×10 -3 When 0.040 ℃ and 0.080 ℃, the stop valve is opened, the limiting valve parameter is set to 100°, the argon flow rate is set to 30 sccm, the voltage is set to -900 V, and the pressure in the chamber is maintained above 1.0 Pa for bias cleaning. The cleaning time is not less than 10 min.

8. The preparation method according to claim 6, characterized in that: The coating process of the transition layer is as follows: the argon flow rate is set to 25-30sccm, the AlCr target power is 140-160W, the Zr target power is 90-110W, the chamber working pressure is 0.4-0.6Pa, the substrate rotation speed is 9-11r / min, the deposition temperature is 180-220°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100V, and the deposition time is 4-6min.

9. The preparation method according to claim 6, characterized in that: The coating process of the hydrogen barrier layer is as follows: the argon flow rate is set to 25-30 sccm, the AlCr target power is 140-160W, the Zr target power is 90-110W, the chamber working pressure is 0.4-0.6Pa, the substrate rotation speed is 9-11r / min, the deposition temperature is 180-220°C, the bias voltage of the magnetron sputtering equipment is adjusted to -100V, the oxygen flow rate is adjusted to 7-8sccm, the deposition time is 7-8min, the oxygen flow rate is adjusted to 5-6sccm, the deposition time is 5-6min, the oxygen flow rate is adjusted to 2-3sccm, and the deposition time is 16-18min.

10. The preparation method according to claim 9, characterized in that: The coating process of the hydrogen barrier layer is as follows: setting the argon flow rate to 30 sccm, the AlCr target power to 150 W, the Zr target power to 100 W, the chamber working pressure to 0.5 Pa, the substrate rotation speed to 10 r / min, the deposition temperature to 200°C, adjusting the bias voltage of the magnetron sputtering equipment to -100 V, adjusting the oxygen flow rate to 8 sccm, the deposition time to 7 min, adjusting the oxygen flow rate to 5 sccm, the deposition time to 5 min, adjusting the oxygen flow rate to 3 sccm, and the deposition time to 18 min.

Citation Information

Patent Citations

  • M / MOx composite hydrogen resistance coating and preparation method thereof

    CN105729934A

  • Iron-aluminum alloy bonding layer / zirconia layer composite hydrogen-retardant coating and preparation method thereof

    CN109023363A

  • Compound hydrogen-resistant coating and production method thereof

    CN113122842A

  • Anti-corrosion and anti-hydrogen permeation coating and preparation method thereof

    CN114686810A

  • Anti-corrosion and anti-hydrogen permeation coating and preparation method thereof

    CN114686814A

Cited By

  • Steel surface hydrogen-resistant wear-resistant coating and preparation method thereof

    CN121874721A

  • Composite hydrogen-resistant coating of high-strength maraging stainless steel and preparation method of composite hydrogen-resistant coating