Lithium ion battery silicon-carbon negative electrode material and preparation method and application thereof

In the preparation of silicon carbon anode material for lithium-ion batteries, uniform deposition and carbon coating of silanes are used to utilize the thermal conductivity of porous carbon and the pore structure, the safety and deposition uniformity of the production process in the prior art are solved, and the problems of safety and deposition uniformity of the production process in the prior art are improved. Electrochemical and cyclic properties.

CN119040844APending Publication Date: 2024-11-29INNER MONGOLIA XINGYANG TECH CO LTD
View PDF 0 Cites 8 Cited by

Patent Information

Application Number
CN202411150452.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The production process of existing lithium-ion batteries has problems such as high cost, difficult to guarantee uniformity of crushing size, low first efficiency and poor circulation performance, and silane CVD deposition technology has safety risks and deposition inhomogeneity at high temperatures. question.

Method used

Using a preparation method of lithium-ion battery silicon carbon anode material, the silane deposition reaction is carried out by heating porous carbon under an inert atmosphere and passing silicon source gas into the CVD reactor after cooling, and repeated several times to ensure uniform deposition. Carbon coating is carried out under high temperature conditions, and the thermal conductivity of porous carbon and pore structure are used to achieve uniform diffusion and deposition of silane.

Benefits of technology

The uniform deposition of silane in porous carbon is achieved, the electrochemical performance is improved, the safety risk of high-temperature heating is avoided, the production cost is reduced, and the circulation performance and first-time efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040844A_ABST
    Figure CN119040844A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium ion battery silicon-carbon negative electrode material and a preparation method and application thereof, and belongs to the technical field of lithium ion battery materials. The method comprises the following steps: heating porous carbon in an inert atmosphere; cooling is performed; introducing mixed gas of silicon source gas and inert gas or silicon source gas to carry out silane deposition reaction on the porous carbon; heating the obtained product in a mixed atmosphere of inert gas and water vapor; cooling is performed; introducing mixed gas of silicon source gas and inert gas or silicon source gas to carry out silane deposition reaction on the cooled product; repeating the steps for multiple times; and introducing a carbon source gas under a high-temperature heating condition to carry out carbon coating on the surface of the product to obtain the product. Through multi-stage deposition, uniform deposition of silane in the porous carbon can be realized, so that better electrochemical performance is achieved. The deposition process is separated from the porous carbon heating process, and the silicon source gas is in contact with the heated porous carbon under the cold state condition, so that the production process is safer and more reliable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion battery materials, and more specifically to a lithium ion battery silicon-carbon negative electrode material and a preparation method and application thereof. Background Art

[0002] The main direction of lithium-ion battery development is to increase specific capacity and achieve rapid charge and discharge. Since silicon has a very high theoretical specific capacity, it has attracted widespread attention as an emerging material for lithium-ion battery negative electrodes. At present, there are silicon-carbon negative electrode products on the market, and there are three main production methods: nano-grinding method, silicon-oxygen method and silane CVD (chemical vapor deposition technology) deposition method. Although the current commercial production method can mass-produce silicon-carbon negative electrodes, there are still some problems that need to be solved.

[0003] Currently, commercial silicon-carbon negative electrode materials are mainly obtained by intensively crushing and mixing silicon and carbon materials, or by reducing silicon oxygen with lithium to obtain nano-scale silicon materials. These nano-silicon and carbon materials are combined to form silicon-carbon negative electrodes. However, there are still some problems with these technologies, such as high cost, difficulty in ensuring the uniformity of the size of the crushed silicon, low initial efficiency of the battery, and poor cycle performance.

[0004] The silicon-carbon negative electrode preparation technology that uses silane CVD deposition on porous carbon can disperse silicon in the porous carbon in a uniform nanostructured manner. Compared with silicon-carbon negative electrode materials prepared by traditional technology routes, it has the advantages of high specific capacity, high first efficiency and good cycle performance. It has received widespread attention and has been successfully commercialized.

[0005] However, this technology also has two problems. First, this technology requires silane to be deposited in porous carbon at high temperature, and the high temperature environment makes the use of silane very dangerous; second, the uniformity of silane deposition in porous carbon cannot be guaranteed. For a single porous carbon material, at the beginning of deposition, due to the high surface temperature of the porous carbon, a large amount of silicon is deposited on the surface, blocking the pores, resulting in the inability of silane or silicon radicals to effectively diffuse into the pores, resulting in uneven deposition.

[0006] Therefore, how to develop a lithium-ion battery silicon-carbon negative electrode material with a safer production process and better electrochemical performance, as well as its preparation method and application is an urgent problem that technicians in this field need to solve. Summary of the invention

[0007] In view of this, the present invention provides a lithium ion battery silicon-carbon negative electrode material and a preparation method and application thereof.

[0008] In order to achieve the above object, the present invention adopts the following technical solution:

[0009] A method for preparing a lithium-ion battery silicon-carbon negative electrode material comprises the following steps:

[0010] (1) heating the porous carbon to a certain temperature under an inert atmosphere, and then taking the porous carbon out from the heating source under an inert atmosphere or a reducing atmosphere;

[0011] (2) placing the heated porous carbon in an inert atmosphere at room temperature and naturally cooling it to a certain temperature;

[0012] Alternatively, the heated porous carbon is placed in a CVD reactor, and an inert gas at room temperature is introduced to purge and cool the heated porous carbon, so that the heated porous carbon is cooled to a certain temperature;

[0013] (3) introducing a mixture of silicon source gas and inert gas into the CVD reactor, or introducing silicon source gas to purge the cooled porous carbon to perform a silane deposition reaction;

[0014] (4) heating the product obtained in step (3) to a certain temperature in a mixed atmosphere of an inert gas and water vapor, and then taking the product out from the heating source in an inert atmosphere or a reducing atmosphere;

[0015] (5) placing the heated product in an inert atmosphere at room temperature and naturally cooling it to a certain temperature;

[0016] Or the heated product is placed in a CVD reactor, and an inert gas at room temperature is introduced to purge and cool the heated product, and the heated product is cooled to a certain temperature;

[0017] (6) introducing a mixture of silicon source gas and inert gas into the CVD reactor, or introducing silicon source gas to purge the cooled product, to perform a silane deposition reaction;

[0018] (7) Repeat steps (4) to (6) multiple times;

[0019] (8) Introducing a carbon source gas into the CVD reactor under high temperature heating conditions to carbon-coat the surface of the product obtained in step (7) to obtain the above-mentioned lithium-ion battery silicon-carbon negative electrode material.

[0020] Furthermore, the porous carbon is a combination of one or more of activated carbon, mesoporous carbon, microporous carbon, carbon nanotubes, graphene, carbon nanofibers, porous ordered carbon, carbon black or metal organic frameworks, and the pore size of the porous carbon is in the range of 2-100 nm, the macropore ratio is less than 10%, and the pore volume is 0.5-2 cm 3 / g, with a specific surface area range of 5-3000m 2 / g.

[0021] The beneficial effects of adopting the above-mentioned further technical solution are as follows: the carbon material containing a rich pore structure is conducive to the diffusion of silicon or silicon radicals, and can make full use of the internal space of the porous carbon to achieve uniform and overall deposition in the porous carbon; the porous carbon has a high thermal conductivity, and its well-developed pore structure is conducive to rapid cooling after heating.

[0022] Furthermore, the inert atmosphere or inert gas is a combination of one or more of nitrogen, argon or helium;

[0023] The reducing atmosphere is a combination of one or more of hydrogen, carbon monoxide, hydrogen sulfide, methane or sulfur monoxide;

[0024] The silicon source gas is a combination of one or more of silane, trichlorosilane, dichlorosilane, chloromethyltrichlorosilane, trimethylchlorosilane, chloromethyltrichlorosilane, dichloromethyldichlorosilane, trichloromethylchlorosilane, trimethylchlorosilane, methyldichlorosilane, ethyldichlorosilane or propyldichlorosilane;

[0025] The carbon source gas is one or more of methane, ethane, ethylene, acetylene, propane, propylene, propyne, butane or isobutane.

[0026] Furthermore, in step (1), the porous carbon is heated to 400-1200°C, preferably 800°C-1000°C, under an inert atmosphere; in step (4), the product obtained in step (3) is heated to 400-1200°C, preferably 800°C-1000°C, under an inert atmosphere.

[0027] The beneficial effect of adopting the above further technical solution is that it avoids the risk of heating the silane in a high-temperature atmosphere in the conventional technology, and is safer.

[0028] Furthermore, in step (2), the heated porous carbon is cooled to 300-1000°C; and in step (5), the heated product is cooled to 300-1000°C.

[0029] The beneficial effect of adopting the above further technical solution is that it can achieve the effect of low external temperature and high internal temperature of the porous carbon particles, which is beneficial to the subsequent deposition reaction of the silicon source inside the porous carbon particles.

[0030] Furthermore, in step (2) or step (5), the cooling time is 0-1440 min, preferably 2-30 min.

[0031] Further, in step (3) or step (6), in the mixed gas of silicon source gas and inert gas, the molar ratio of silicon source gas to inert gas is (1-1000):(1-1000);

[0032] In step (3), the mass ratio of the mixed gas of the silicon source gas and the inert gas or the silicon source gas and the cooled porous carbon is (1-100):(1-10000);

[0033] In step (6), the mass ratio of the mixed gas of silicon source gas and inert gas or the silicon source gas and the cooled product is (1-100):(1-1000).

[0034] The beneficial effect of adopting the above further technical solution is that the room temperature silicon source is in contact with the heated porous carbon, and the heat of the heated porous carbon is used to provide energy for the silicon source to undergo CVD reaction in the porous carbon, which is safer and the silicon source deposition reaction is more uniform.

[0035] Furthermore, in step (4), in the mixed gas of inert gas and water vapor, the molar ratio of inert gas to water vapor is (1-100):(1-20), preferably (5-10):1.

[0036] The beneficial effect of adopting the above-mentioned further technical solution is as follows: after the porous carbon has undergone the previous heating and cooling, the internal structure has collapsed to a certain extent, and a part of the pores have been blocked. The small amount of water vapor contained in the secondary heating process can achieve a pore-forming effect in the porous carbon and regenerate certain pores, which is beneficial to the subsequent repeated silicon source CVD deposition reaction.

[0037] Further, in step (3) or step (6), the silane deposition reaction time is 0.1-500 min;

[0038] In step (8), the heating temperature is 400-900° C., the carbon coating time is 10-600 min, and the mass ratio of the carbon source gas to the product obtained in step (7) is (1-1000):(1-1000).

[0039] Furthermore, the above-mentioned CVD reactor is a moving fixed bed, fluidized bed, heat pipe, low pressure, atmospheric pressure, microwave assisted, plasma enhanced, rotating base, spray or light assisted CVD reactor.

[0040] The present invention also provides a lithium ion battery silicon-carbon negative electrode material prepared by the above method.

[0041] The present invention also provides an application of the above lithium ion battery silicon-carbon negative electrode material in a lithium ion battery.

[0042] Beneficial effects of the present invention: Through multi-stage deposition, uniform deposition of silane inside the porous carbon can be achieved, so that the prepared silicon-carbon negative electrode material can be uniformly deposited with silane from the inside to the outside, thereby having better electrochemical performance.

[0043] The deposition process is separated from the porous carbon heating process, and the silicon source gas contacts the heated porous carbon under cold conditions, thereby avoiding the danger caused by heating the silicon source gas and making the production process safer and more reliable.

[0044] In the present invention, the silane gas does not need to be heated for depositing silane, and the heat for silane CVD deposition is provided by the sensible heat of heating the porous carbon itself, thereby avoiding the risk of high-temperature combustion and explosion.

[0045] In the present invention, the porous carbon is heated, and after cooling for a period of time, due to the heat dissipation on the surface, the surface temperature of the porous carbon single particle is low and the internal temperature is high. Therefore, silane or silicon free radicals or silicon hydrogen free radicals can penetrate into the porous carbon for deposition. When repeated deposition is performed for subsequent times, as the cooling interval time is shortened each time, the high temperature area of ​​the single porous carbon gradually increases from the center of the sphere to the outside, so the effective area of ​​silicon deposition also covers the entire porous carbon sphere from the inside to the outside, thereby achieving uniform deposition. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 This is a schematic diagram of the preparation principle of the silicon-carbon negative electrode material for lithium-ion batteries of the present invention. DETAILED DESCRIPTION

[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] Example 1

[0049] The porous carbon used in Example 1 is activated carbon, and the pore size of the porous carbon is in the range of 2-100 nm, the macropore ratio is less than 10%, and the pore volume is 0.5-2 cm 3 / g, with a specific surface area range of 5-3000m 2 / g.

[0050] A method for preparing a lithium-ion battery silicon-carbon negative electrode material comprises the following steps:

[0051] (1) In a rotary kiln heating furnace, the porous carbon is heated to 1000° C. under nitrogen, and then the porous carbon is taken out of the rotary kiln heating furnace under nitrogen;

[0052] (2) placing the heated porous carbon in a nitrogen environment at room temperature and naturally cooling it to 600°C for 20 minutes;

[0053] (3) feeding the porous carbon into a fluidized bed reactor, introducing silane into the fluidized bed reactor to purge the cooled porous carbon, the mass ratio of silane to the cooled porous carbon being 5:1, and performing a silane deposition reaction, and the purge reaction time being 20 min;

[0054] (4) heating the product obtained in step (3) to 900° C. in a mixed atmosphere of nitrogen and water vapor, wherein the molar ratio of nitrogen to water vapor is 3:1, and then taking the product out of the rotary kiln heating furnace under nitrogen or a reducing atmosphere;

[0055] (5) The heated product is placed in a nitrogen environment at room temperature and naturally cooled to 600°C for 15 minutes;

[0056] (6) introducing silane into the fluidized bed reactor to purge the cooled product, the ratio of silane to the cooled product being 5:1, and performing a silane deposition reaction, and the purge reaction time being 20 min;

[0057] (7) Repeat steps (4) to (6) 4 times;

[0058] (8) Under high temperature heating conditions, methane is introduced into the fluidized bed reactor to carbon-coat the surface of the product obtained in step (7); the heating temperature is 650° C., the carbon coating time is 120 min, and the mass ratio of the carbon source gas to the product obtained in step (7) is 1:200, thereby obtaining a silicon-carbon negative electrode material for a lithium-ion battery.

[0059] The performance of the obtained silicon-carbon negative electrode lithium-ion negative electrode battery material: first reversible specific capacity = 1910 mAh.g, first coulomb efficiency: 93.2%, capacity retention rate after 100 cycles: 83.2%, capacity retention rate after 300 cycles: 72.4%

[0060] Example 2

[0061] The same as Example 1, except that in step (1), the porous carbon is heated to 1100° C. under nitrogen, and then the porous carbon is taken out from the rotary kiln heating furnace under nitrogen.

[0062] The performance of the obtained silicon-carbon negative electrode lithium ion negative electrode battery material: first reversible specific capacity = 1810 mAh.g, first coulomb efficiency: 92.2%, capacity retention rate after 100 cycles: 85.9%, capacity retention rate after 300 cycles: 76.8%.

[0063] Example 3

[0064] The same as Example 1, except that in step (1), the porous carbon is heated to 800° C. under nitrogen, and the porous carbon is taken out from the rotary kiln heating furnace under nitrogen.

[0065] The performance of the obtained silicon-carbon negative electrode lithium-ion negative electrode battery material: first reversible specific capacity = 1101.4 mAh.g, first coulomb efficiency: 83.1, capacity retention rate after 100 cycles: 78.6, capacity retention rate after 300 cycles: 67.2%

[0066] Comparative Example 1

[0067] The same as Example 1, except that in step (1), the porous carbon is heated to 300° C. under nitrogen, and the porous carbon is taken out from the rotary kiln heating furnace under nitrogen.

[0068] The performance of the obtained silicon-carbon negative electrode lithium-ion negative electrode battery material: first reversible specific capacity = 130 mAh.g, first coulomb efficiency: 23.1%, capacity retention rate after 100 cycles: 53.7%, capacity retention rate after 300 cycles: 12.3%.

[0069] Comparative Example 2

[0070] The same as Example 1, except that in step (1), the porous carbon is heated to 1400° C. under nitrogen, and the porous carbon is taken out from the rotary kiln heating furnace under nitrogen.

[0071] The performance of the obtained silicon-carbon negative electrode lithium-ion negative electrode battery material: first reversible specific capacity = 946.1 mAh.g, first coulomb efficiency: 81.9%, capacity retention rate after 100 cycles: 53.7%, capacity retention rate after 300 cycles: 68.3%.

[0072] like Figure 1 As shown, after a single porous carbon is heated and cooled for a certain period of time, the external temperature is low and the internal temperature is high. In the figure, the red color represents the internal high-temperature area, so after the room-temperature silane is introduced, the silane CVD reaction mainly occurs in the internal high-temperature area; after the porous carbon is heated and cooled for the second time, the internal high-temperature area increases due to the shortened cooling interval, so the secondary silane CVD reaction area increases; and so on, after multiple reactions, the internal reaction area gradually expands outward, and finally the overall reaction is achieved.

[0073] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a lithium-ion battery silicon-carbon negative electrode material, characterized in that: The following steps are involved: (1) heating the porous carbon to a certain temperature under an inert atmosphere, and then taking the porous carbon out from the heating source under an inert atmosphere or a reducing atmosphere; (2) placing the heated porous carbon in an inert atmosphere at room temperature and naturally cooling it to a certain temperature; Alternatively, the heated porous carbon is placed in a CVD reactor, and an inert gas at room temperature is introduced to purge and cool the heated porous carbon, so that the heated porous carbon is cooled to a certain temperature; (3) introducing a mixture of silicon source gas and inert gas into the CVD reactor, or introducing silicon source gas to purge the cooled porous carbon to perform a silane deposition reaction; (4) heating the product obtained in step (3) to a certain temperature in a mixed atmosphere of an inert gas and water vapor, and then taking the product out from the heating source in an inert atmosphere or a reducing atmosphere; (5) placing the heated product in an inert atmosphere at room temperature and naturally cooling it to a certain temperature; Or the heated product is placed in a CVD reactor, and an inert gas at room temperature is introduced to purge and cool the heated product, and the heated product is cooled to a certain temperature; (6) introducing a mixture of silicon source gas and inert gas into the CVD reactor, or introducing silicon source gas to purge the cooled product, to perform a silane deposition reaction; (7) Repeat steps (4) to (6) multiple times; (8) Introducing a carbon source gas into the CVD reactor under high temperature heating conditions to carbon-coat the surface of the product obtained in step (7) to obtain the lithium-ion battery silicon-carbon negative electrode material.

2. The method for preparing a silicon-carbon negative electrode material for a lithium-ion battery according to claim 1, characterized in that: The porous carbon is a combination of one or more of activated carbon, mesoporous carbon, microporous carbon, carbon nanotubes, graphene, carbon nanofibers, porous ordered carbon, carbon black or metal organic frameworks. The porous carbon has a pore size range of 2-100 nm, a macropore ratio of <10%, and a pore volume of 0.5-2 cm 3 / g, with a specific surface area range of 5-3000m 2 / g.

3. The method for preparing a lithium-ion battery silicon-carbon negative electrode material according to claim 1, characterized in that: The inert atmosphere or inert gas is a combination of one or more of nitrogen, argon or helium; The reducing atmosphere is a combination of one or more of hydrogen, carbon monoxide, hydrogen sulfide, methane or sulfur monoxide; The silicon source gas is a combination of one or more of silane, trichlorosilane, dichlorosilane, chloromethyltrichlorosilane, trimethylchlorosilane, chloromethyltrichlorosilane, dichloromethyldichlorosilane, trichloromethylchlorosilane, trimethylchlorosilane, methyldichlorosilane, ethyldichlorosilane or propyldichlorosilane; The carbon source gas is one or more of methane, ethane, ethylene, acetylene, propane, propylene, propyne, butane or isobutane.

4. The method for preparing a lithium-ion battery silicon-carbon negative electrode material according to claim 1, characterized in that: In step (1), the porous carbon is heated to 400-1200° C. in an inert atmosphere; in step (4), the product obtained in step (3) is heated to 400-1200° C. in an inert atmosphere.

5. The method for preparing a lithium-ion battery silicon-carbon negative electrode material according to claim 1, characterized in that: In step (2), the heated porous carbon is cooled to 300-1000°C; in step (5), the heated product is cooled to 300-1000°C.

6. The method for preparing a lithium-ion battery silicon-carbon negative electrode material according to claim 1, characterized in that: In step (3) or step (6), in the mixed gas of silicon source gas and inert gas, the molar ratio of silicon source gas to inert gas is (1-1000):(1-1000); In step (3), the mass ratio of the mixed gas of the silicon source gas and the inert gas or the silicon source gas and the cooled porous carbon is (1-100):(1-10000); In step (6), the mass ratio of the mixed gas of silicon source gas and inert gas or the silicon source gas and the cooled product is (1-100):(1-1000).

7. The method for preparing a lithium-ion battery silicon-carbon negative electrode material according to claim 1, characterized in that: In step (4), in the mixed gas of inert gas and water vapor, the molar ratio of inert gas to water vapor is (1-100):(1-20).

8. The method for preparing a lithium-ion battery silicon-carbon negative electrode material according to claim 1, characterized in that: The silane deposition reaction time in step (3) or step (6) is 0.1-500 min; In step (8), the heating temperature is 400-900° C., the carbon coating time is 10-600 min, and the mass ratio of the carbon source gas to the product obtained in step (7) is (1-1000):(1-1000).

9. A lithium-ion battery silicon-carbon negative electrode material prepared by the method according to any one of claims 1 to 8.

10. Use of the lithium-ion battery silicon-carbon negative electrode material according to claim 9 in a lithium-ion battery.

Citation Information

Cited By

  • Silicon-carbon negative electrode material and preparation method and application thereof

    CN119481024A

  • Spherical porous carbon material as well as preparation method and application thereof

    CN119774607A

  • Bimetal-nitrogen site anchored silicon-carbon composite material and preparation method thereof

    CN119932518A

  • Carbon source mixed gas CVD coated silicon carbon negative electrode material, preparation method and lithium ion battery

    CN120261549A

  • Preparation method of porous carbon-silicon composite negative electrode material of lithium battery and lithium battery

    CN120432517A