Method for preparing lead dioxide from lead-zinc-ammonia-chlorine complex system

Lead dioxide is prepared by electrolyzing the lead-zinc ammonium chlorine complex system in pure ammonium chloride solution, which solves the problems of high energy consumption and serious pollution in the existing technology, and achieves low-cost and environmentally friendly lead dioxide production and secondary production and development of low-cost and environmentally friendly lead dioxide Efficient recycling of resources.

CN119040908APending Publication Date: 2024-11-29HUNAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411101950.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing methods for preparing lead dioxide have high energy consumption and serious pollution, especially in pyrometallurgy and partial wet processes, which lead to environmental pollution and waste of resources.

Method used

The lead-zinc ammonia chlorine complex system is adopted. During the preparation of pure ammonium chloride solution and leaching, no ammonia water or ammonia gas is added. The electrolytic device is used to generate stable lead dioxide, and the selection of pure ammonium chloride solution is used. Simplify purification steps and reduce costs.

Benefits of technology

It has achieved the realization of saving material consumption, reducing energy consumption, simplifying process flow, reducing pollution, and improving the purity and morphological quality of lead dioxide, which is suitable for the recycling and recycling of secondary lead and zinc resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119040908A_ABST
    Figure CN119040908A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing lead dioxide from a lead-zinc-ammonia-chlorine complex system. The method comprises the following steps: obtaining a lead-zinc-containing material; ammonium chloride is added into water to prepare a pure ammonium chloride solution, ammonia water is not added and ammonia gas is not introduced in the preparation process of the pure ammonium chloride solution, the purity of ammonium chloride in the pure ammonium chloride solution is greater than 95%, and the concentration is 3.0-7.0 mol / L; the material containing lead and zinc is put into a pure ammonium chloride solution to be leached, leach liquor of the lead-zinc-ammonia-chlorine complex is obtained, ammonia water is not added in the leaching process, and ammonia gas is not introduced in the leaching process; and the leachate is put into an electrolysis device with the preset temperature and the preset current density kept for electrolysis, and lead dioxide is obtained on an anode plate of the electrolysis device. According to the embodiment of the invention, ammonia water does not need to be added and ammonia gas does not need to be introduced in the processes of preparing the pure ammonium chloride solution and leaching, and in the electrolytic process of the leachate, the performance of the leachate is stable, electrolyte precipitation and decomposition do not occur, and the material consumption is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of hydrometallurgy, and in particular to a method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system. Background Art

[0002] Lead, as a non-ferrous metal with good electrical and thermal conductivity, is widely used in the industrial field. With the gradual depletion of high-grade lead oxide and lead sulfide ores that are easy to beneficiate, the utilization of secondary lead-zinc materials is gradually gaining attention. There are many types of secondary lead-zinc materials, including arc furnace slag, fuming ash collected from fuming furnaces, discarded lead-acid batteries and waste lead-silver anodes. If secondary lead-zinc materials are not handled properly, they will cause serious environmental pollution and waste of resources.

[0003] Some companies use pyrometallurgy to prepare anodic lead dioxide from secondary lead-zinc materials. The pyrometallurgical method of preparing anodic lead dioxide from secondary lead-zinc materials has the problems of high energy consumption, large amounts of sulfur dioxide and volatile lead-containing smoke, which is not conducive to energy conservation, emission reduction and hazardous waste treatment. Compared with pyrometallurgy, most companies in the industrial field currently use hydrometallurgy to prepare anodic lead dioxide from secondary lead-zinc materials. The wet process includes solid-phase electrolysis, RSR and CX-EW processes. The solid-phase electrolysis method has high energy consumption and a long electrolysis time; the RSR and CX-EW processes deposit anodic lead dioxide in a lead fluoride silicate system. The system is extremely corrosive, and the wastewater contains a large amount of fluoride ions, which are difficult to handle and seriously pollute the environment.

[0004] In summary, the existing methods for preparing lead dioxide have the problems of high energy consumption and serious pollution. Summary of the invention

[0005] Therefore, in order to overcome some defects and shortcomings in the prior art, the embodiment of the present invention provides a method for preparing lead dioxide using a lead-zinc ammonia-chlorine complex system. In the process of preparing a pure ammonium chloride solution and in the leaching process, it is not necessary to add ammonia water or pass ammonia gas, and the leachate exists in a stable form during the electrolysis process, thereby saving material consumption and reducing costs.

[0006] The present invention provides a method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system, comprising:

[0007] Obtaining lead-zinc-containing materials;

[0008] Adding ammonium chloride to water to prepare a pure ammonium chloride solution, wherein no ammonia water is added and no ammonia gas is introduced during the preparation of the pure ammonium chloride solution, the purity of ammonium chloride in the pure ammonium chloride solution is greater than 95%, and the concentration of the ammonium chloride is 3.0-7.0 mol / L;

[0009] The lead-zinc-containing material is placed in the pure ammonium chloride solution for leaching to obtain a leachate, wherein no ammonia water is added and no ammonia gas is introduced during the leaching process;

[0010] The leaching solution is placed in an electrolysis device maintained at a preset temperature and a preset current density for electrolysis, and lead dioxide is obtained on the anode plate of the electrolysis device;

[0011] The preset temperature is 70-90°C, and the preset current density is 200-500A / m 2 .

[0012] In one embodiment of the present invention, the obtaining of the lead-zinc-containing material specifically comprises: fuming and reducing the smelting slag in the closed blast furnace in a fuming furnace to obtain fumed ash; and obtaining the fumed ash to obtain the lead-zinc-containing material.

[0013] In one embodiment of the present invention, the lead content in the leaching solution is greater than or equal to 0.1 mol / L.

[0014] In one embodiment of the present invention, the distance between the cathode plate and the anode plate of the electrolysis device is 3 to 5 cm.

[0015] In one embodiment of the present invention, the anode plate is a ruthenium-coated titanium mesh, a graphite plate, a titanium plate or a stainless steel plate; the cathode plate is a titanium plate, an aluminum plate or a stainless steel plate.

[0016] In one embodiment of the present invention, after leaching the lead-zinc material into the pure ammonium chloride solution to obtain a leachate, the method further comprises: adding an electrodeposition additive to the leachate and completely dissolving the electrodeposition additive to obtain a post-reaction leachate; and placing the post-reaction leachate into the electrolysis device for electrolysis to obtain the lead dioxide.

[0017] In one embodiment of the present invention, the type of the electrodeposition additive is bone glue, and the concentration range of the electrodeposition additive is 5 to 50 mg / L.

[0018] In one embodiment of the present invention, the leachate includes iron ions. After leaching the lead-containing material into the pure ammonium chloride solution to obtain the leachate, the method further includes: purifying the leachate to obtain a purified leachate; and placing the leachate into the electrolysis device for electrolysis to obtain the lead dioxide.

[0019] In one embodiment of the present invention, the method further comprises: stripping and cleaning the lead dioxide to obtain cleaned lead dioxide.

[0020] In one embodiment of the present invention, the electrolysis device is a polyvinyl chloride electrolysis cell.

[0021] It can be seen from the above that the above technical solution has at least one or more of the following beneficial effects:

[0022] (1) In the process of preparing the pure ammonium chloride solution and the leaching process of the embodiment of the present invention, it is not necessary to add ammonia water or pass ammonia gas, and the performance of the leachate is stable during the electrolysis process, and no electrolyte precipitation and decomposition occur, thereby saving material consumption and reducing costs.

[0023] (2) By placing the leachate in an electrolytic device for electrolysis, the electrolytic device can control the temperature of the leachate so that the temperature of the leachate is moderate; in addition, the pH of the leachate is nearly neutral, which has the advantage of not being easy to corrode equipment. Furthermore, due to the strong selectivity of the pure ammonium chloride solution, the leachate can be directly put into electrolysis without going through a complicated purification step. This method has the advantages of simple and controllable operation, low cost and environmental friendliness, and the purity and macroscopic morphology of the lead dioxide product can meet the basic requirements of industrial production.

[0024] (3) The embodiment of the present invention uses pure ammonium chloride solution, which can give play to the selective advantage of zinc and ammonia chloride, lead and chlorine forming complexes, ensure that zinc and lead ions exist stably in the form of complexes during the electrolysis process, avoid the problems of zinc and lead ion hydrolysis in the leachate, the influence of organic matter on the morphology of the anode product, and the easy peeling of the anode product layer. At the same time, it solves the problem that the metal lead is difficult to recover after the secondary lead and zinc resources are leached with pure ammonium chloride. This method is particularly suitable for the recovery and treatment of valuable metals in the leachate of secondary lead and zinc resources. Secondly, adding ammonia water or ammonium chloride to the waste electrolyte can achieve recycling, achieving the goals of efficient production and energy conservation and emission reduction. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The specific implementation modes of the present invention will be described in detail below with reference to the accompanying drawings.

[0026] Figure 1 A schematic flow chart of a method for preparing lead dioxide from a lead-zinc-ammonia-chlorine complex system provided in an embodiment of the present invention.

[0027] Figure 2 for Figure 1 Specific flow chart of step S10 in FIG.

[0028] Figure 3 for Figure 1 The flowchart of the additional steps after step S40 is shown.

[0029] Figure 4 for Figure 1 The flowchart of the additional steps after step S30 is shown.

[0030] Figure 5 for Figure 1 The flowchart of another additional step after step S30 is shown.

[0031] Figure 6 A schematic block diagram of the system structure of a method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system provided in an embodiment of the present invention.

[0032] Figure 7 This is a schematic diagram of a macroscopic photograph of electrolysis products on the anode plate of an embodiment of the present invention.

[0033] Figure 8 It is a schematic diagram of the X-ray diffraction (XRD) characterization results of the product on the anode plate of an embodiment of the present invention.

[0034] Fig. 9 A schematic block diagram of a specific process of a method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0035] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0036] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative work should fall within the scope of protection of the present invention.

[0037] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0038] It should also be noted that the division of multiple embodiments in the present invention is only for the convenience of description and should not constitute a special limitation. The features in various embodiments can be combined and referenced to each other without contradiction.

[0039] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system. The method for preparing lead dioxide using a lead-chlorine-ammonia complex system includes, for example:

[0040] S10: Obtain lead-zinc containing materials.

[0041] Specifically, the lead-zinc-containing material can be obtained from the smelting slag of a smelter, for example. The lead-zinc-containing material is, for example, a solid substance containing lead such as fumed fly ash or a lead-containing secondary material.

[0042] S20: adding ammonium chloride into water to prepare a pure ammonium chloride solution. In the process of preparing the pure ammonium chloride solution, no ammonia water is added and no ammonia gas is introduced. The purity of ammonium chloride in the pure ammonium chloride solution is greater than 95%, and the concentration of ammonium chloride is 3.0-7.0 mol / L.

[0043] S30: Leaching the lead-zinc material into a pure ammonium chloride solution to obtain a leachate. No ammonia water is added and no ammonia gas is introduced during the leaching process. The lead content in the leachate is greater than or equal to 0.1 mol / L.

[0044] S40: The leaching solution is placed in an electrolysis device maintained at a preset temperature and a preset current density for electrolysis, and lead dioxide is obtained on the anode plate of the electrolysis device. The preset temperature is 70-90°C, and the preset current density is 200-500A / m 2 .

[0045] In step S20, the concentration of ammonium chloride may be 3.0 mol / L, 5.0 mol / L, or 7.0 mol / L.

[0046] In step S40, the preset temperature may be 70°C, 80°C or 90°C; the preset current density may be 200A / m 2 or 300A / m 2 or 400A / m 2 or 500A / m 2 .

[0047] In the prior art, both pyrometallurgy and hydrometallurgy processes for preparing lead dioxide have the problem of high energy consumption. In the process of preparing pure ammonium chloride solution and the leaching process in the embodiment of the present invention, it is not necessary to add ammonia water or introduce ammonia gas, and the leachate exists in a stable form during the electrolysis process. The leachate can be directly used as an electrolyte for electrolysis, and then lead dioxide is obtained on the anode plate. It can be seen that the present application can omit the purification step in the prior art, save the purification device, and reduce the cost of the entire system structure; secondly, in the electrodeposition mode using voltage to control current, the potential of a single electrolysis system (a pair of anode and cathode plates, a DC power supply and a tank of electrolyte) is controlled to be 2.20V to achieve the preparation of lead dioxide. The lower current density and potential control conditions can reduce the use of electric energy, thereby reducing energy consumption. This method can save material consumption, thereby reducing costs.

[0048] like Figure 2 As shown, in a preferred implementation of this embodiment, step S10 specifically includes the following steps:

[0049] S11: reducing and fuming the smelting slag in the closed blast furnace in a fuming furnace to obtain fumed ash.

[0050] S12: Obtain smoke ash to obtain a lead-zinc-containing material.

[0051] In this embodiment, the lead-zinc-containing material is, for example, smelting slag in a closed blast furnace of a lead-zinc smelter, which is reduced and fumed to obtain fumed ash in a fuming furnace, thereby realizing the secondary utilization of lead-zinc smelting waste slag.

[0052] Furthermore, this embodiment uses the fumed fly ash obtained by reducing and volatilizing the smelting slag in the closed blast furnace of the lead-zinc smelter as the lead-zinc material for illustration. For example, the lead-zinc material in this embodiment is a solid. When the lead-zinc material is placed in a pure ammonium chloride solution for leaching, the lead-zinc material will become an ionic form, that is, a leachate is obtained. The leachate is, for example, a complex containing zinc, lead and ammonia chloride. The composition and chemical formula of the complex may include the following categories: zinc-ammonia complex, such as Zn(NH3) 2+ 、Zn(NH3)2 2+ 、Zn(NH3)3 2+ and Zn(NH3)4 2+ ; Zinc-chloride complex, such as ZnCl + 、ZnCl 2(aq) 、ZnCl3 - and ZnCl4 2- ; Lead-chloride complexes, such as PbCl + 、PbCl 2(aq) and PbCl3 -; Zinc-ammonia-chlorine ternary complex, for example Zn(NH3)2Cl 2(aq) and Zn(NH3)2Cl3 - For example, ammonia and chloride are free ammonia and chloride ions in solution, and their chemical formulas are NH 3(aq) and Cl - In this embodiment, by using pure ammonium chloride solution, the selectivity advantage of zinc-lead and ammonia-chloride forming a complex can be brought into play, ensuring that zinc-lead ions exist stably in the form of a complex during the electrolysis process.

[0053] The electrolysis device in this embodiment is, for example, a polyvinyl chloride (PVC) electrolytic cell. An anode plate and a cathode plate are provided in the electrolysis device, and lead dioxide is generated on the anode plate. The anode plate is, for example, a conductive material such as a ruthenium-coated titanium mesh, a graphite plate, a titanium plate, a stainless steel plate, etc. The components of the anode plate do not contain lead and zinc, and its oxidation reaction potential should be higher than the precipitation potential of lead dioxide, so as to prevent the anode or the lead and zinc in the anode from dissolving and contaminating the leachate. The cathode plate is, for example, a conductive material that does not react with the electrolyte, such as a titanium plate, an aluminum plate or a stainless steel plate. The pole distance between the cathode plate and the anode plate is, for example, 3 to 5 cm, and the pole distance between the cathode plate and the anode plate is, for example, 4 cm as the best.

[0054] In this embodiment, the leachate is an electrolyte. The leachate is placed in an electrolysis device, and the anode plate and the cathode plate are connected to a DC circuit. The leachate is electrolyzed under high temperature conditions by controlling the electrolysis device. For example, the temperature of the leachate is controlled to be 70-90°C and the current density is 300-500A / m 2 , thus, the divalent lead ions in the lead-chlorine complex will undergo oxidation reaction on the surface of the anode plate, and the reaction equation is as follows:

[0055] Pb 2+ +2H2O-2e=PbO2+4H +

[0056] In this way, lead dioxide can be produced on the anode plates.

[0057] In addition, it is worth mentioning that since the oxidation reaction on the anode plate will generate hydrogen ions, as the electrolysis process continues, the electrolyzed solution (i.e., the leachate) will be acidic. Therefore, if the method for preparing lead dioxide from the lead-zinc ammonia-chlorine complex system provided in this embodiment requires a long preparation time, that is, a long electrolysis process, a small amount of ammonia water needs to be added to the leachate so that the leachate can remain neutral and not easily corrode the equipment. Adding a small amount of ammonia water can not only replenish the consumed ammonium ions, but also adjust the pH value of the leachate.

[0058] like Figure 7 and Figure 8As shown, the morphology of lead dioxide prepared by this method is different from the plate-like and volcanic morphologies prepared by the lead methanesulfonate system and the xylitol system. The morphology of the lead dioxide product is a standard reddish-brown coating, which has good adsorption on the surface of the anode plate and does not fall off during the process of taking out the anode plate. Secondly, from the perspective of the distribution and intensity correspondence of the miscellaneous peaks in the XRD spectrum, except for the undetectable tiny miscellaneous peaks in the sample, the other main peaks, whether in position or intensity, perfectly correspond to the standard card characteristic peaks of lead dioxide, confirming that the oxidation reaction of lead ions occurred at the anode to generate lead dioxide.

[0059] In this embodiment, the leachate is placed in an electrolysis device for electrolysis. The electrolysis device can control the temperature of the leachate to make the temperature of the leachate moderate. In addition, the pH of the leachate is nearly neutral, which has the advantage of not easily corroding equipment. In addition, due to the strong selectivity of the pure ammonium chloride solution, the leachate can be directly put into electrolysis without going through complicated purification steps. The method has the advantages of simple and controllable operation, low cost and environmental friendliness, and the purity and macroscopic morphology of the lead dioxide product can meet the basic requirements of industrial production.

[0060] like Figure 3 As shown, the method for preparing lead dioxide by a lead-zinc-ammonia-chlorine complex system also includes:

[0061] S50: stripping and cleaning the lead dioxide to obtain cleaned lead dioxide.

[0062] Specifically, the lead dioxide is stripped and cleaned after electrolysis to remove a small amount of solute precipitated when the lead dioxide is taken out, thereby preventing the purity of the lead dioxide from being affected. Optionally, in this embodiment, the purity of the lead dioxide is greater than 90%.

[0063] like Figure 4 As shown, after step S30, the method for preparing lead dioxide by a lead-zinc-ammonia-chlorine complex system further includes:

[0064] S60: adding an electrodeposition additive to the leaching solution and completely dissolving the electrodeposition additive to obtain a reacted leaching solution.

[0065] S70: placing the leaching solution after the reaction into an electrolysis device for electrolysis to obtain lead dioxide.

[0066] In step S60, the type of the electrodeposition additive is, for example, bone glue, and the concentration range of the electrodeposition additive is 5 mg / L to 50 mg / L; the optimal concentration of the electrodeposition additive is 10 mg / L.

[0067] Specifically, in this embodiment, the electrodeposition additive is, for example, bone glue. Bone glue is a protein organic substance made by hydrolyzing, extracting and drying collagen contained in animal bones, tendons or hooves. The main component of bone glue is the amino acid component in collagen protein, and its molecular formula can be expressed as H2NCH2RCOOH. The amino acid component in collagen protein includes acidic amino acids glutamic acid (Glutamic acid, HOOC-(CH2) 2- ) and basic amino acids such as arginine (Arginine, HN=C(NH2)-NH-(CH2) 3- ), Lysine (Lysine, H2N-(CH2) 4- ) and the sulfur-containing amino acid methionine (Methionine, CH3-S-(CH2) 2- )wait.

[0068] In this embodiment, bone glue, as a commonly used electrodeposition additive, has the effects of smoothing the surface, inhibiting the side effects of impurity ions, and smoothing the product morphology. Although the raw material reagent prepared by the leachate of this embodiment has a high purity, it still contains a small amount of impurities. Therefore, by adding bone glue to the leachate, the influence of impurities can be suppressed and the morphology of the electrodeposition product, i.e., lead dioxide, can be smoothed.

[0069] like Figure 5 and Figure 6 As shown, after step S30, the method further includes:

[0070] S80: purifying the leachate to obtain a purified leachate.

[0071] S90: placing the purified leaching solution into an electrolysis device for electrolysis to obtain lead dioxide.

[0072] Optionally, the leachate includes, for example, iron ions. For example, in the process of leaching the lead-zinc material into a pure ammonium chloride solution, a small amount of iron may be leached, and the iron ions can be purified from the leachate in the manner of this embodiment; in other embodiments, the leachate may be electrolyzed directly without purification, because trivalent iron ions will not discharge on the anode surface to increase the valence, but divalent iron ions will be oxidized to trivalent iron ions near the anode and exist in the solution or precipitate at the cathode. Of course, if no iron ions are generated during the leaching process, the electrolysis effect is better and the energy consumption is lower.

[0073] like Fig. 9As shown, the method for preparing lead dioxide from a lead-zinc ammonia-chlorine complex system also includes, for example: obtaining a waste electrolyte in an electrolysis device, adding ammonia water or ammonium chloride to the waste electrolyte to obtain a mixed solution. For example, the leachate is electrolyzed in the electrolysis device, and not only the lead-chlorine complex ions undergo an oxidation reaction on the anode plate to produce solid lead dioxide, but also the ammonium ions in the solution undergo an oxidation reaction to produce gaseous nitrogen (reaction: 2NH4 + -6e=N2(g)+8H + ), since the liquid used in leaching is only pure ammonium chloride solution, the ammonium radicals in the leaching solution are consumed after electrolysis, and thus, after the lead dioxide is collected, the ammonium radical concentration and acidity in the waste electrolyte generated will be reduced. At this time, ammonia water is added to the waste electrolyte. Since ammonia water is an ammonia-containing reagent that does not contain other impurities, it can effectively supplement the ammonium radicals and adjust the pH value of the mixed solution. Therefore, after adding ammonia water to the waste electrolyte, the ammonium radical ions can be effectively supplemented. Thus, the obtained mixed solution contains sufficient ammonium radical ions, and the pH value of the mixed solution is nearly neutral. This method allows the waste electrolyte to be recycled, thereby saving materials and avoiding the pollution to the environment caused by improper treatment of the waste electrolyte, thereby improving the environmental protection effect. Of course, in this embodiment, ammonium chloride can also be directly added to the waste electrolyte.

[0074] like Fig. 9 As shown, a specific example is given by reducing and volatilizing the smelting slag in a closed blast furnace to obtain fumed ash as a lead-zinc material. Specifically, the slag (i.e., smelting slag) in the closed blast furnace is fumed (i.e., reduced and volatilized) in a fuming furnace to obtain fumed ash, and then the fumed ash is placed in a pure ammonium chloride solution for leaching to obtain a leachate. At this time, there may be a small amount of leached iron in the leachate, so the leachate can be purified to remove a small amount of iron that may be present in the leachate to obtain an iron-free leachate, and then the leachate is placed in an electrolysis device for electrolysis, and lead dioxide can be generated on the anode plate. Optionally, the lead-zinc material can also be a secondary material containing lead (or lead-zinc) or other materials containing lead-zinc oxides that can be leached by a pure ammonium chloride solution, which is not limited here.

[0075] Furthermore, in addition to the solid lead dioxide generated on the anode plate, gaseous nitrogen and hydrogen ions are also produced, so that the ammonium ion concentration and pH value of the remaining leachate, that is, the waste electrolyte, are reduced. Therefore, ammonium chloride or ammonia water can be added to the waste electrolyte to form a mixed solution, provide ammonium ions and adjust the pH value of the solution so that the solution can be reused.

[0076] Furthermore, if Figure 4As shown, when the slag in the closed blast furnace is fumed in a fuming furnace, dusty SO2 flue gas will also be generated. The dusty SO2 flue gas is dust-collected and purified to obtain SO2 flue gas. In this embodiment, the SO2 flue gas can be used to make acid to produce sulfuric acid. After the dust-containing SO2 flue gas is dust-collected and purified, other substances except the SO2 flue gas are collected to obtain a small amount of lead-zinc-containing material, because during the fuming process, a small amount of lead and zinc metal vapor will enter the pipeline with the sulfur dioxide flue gas, and react under the action of air and sulfur dioxide to form a complex substance, but because the main metal elements of the substance are lead and zinc, a small amount of lead-zinc-containing material can be obtained. This method can make full use of the dusty SO2 flue gas generated when the slag in the closed blast furnace is fumed in a fuming furnace, thereby avoiding the pollution of the environment caused by improper treatment of the SO2 flue gas, thereby improving the environmental protection effect. Specific embodiments

[0078] The smelting slag in the closed blast furnace of a lead-zinc smelter was reduced and volatilized to obtain fumed ash. The fumed ash was leached with pure ammonium chloride solution to obtain a leachate. 500 mL of the leachate was placed in a beaker. The lead ion content in the leachate was about 21 g / L. A gelatin additive was added thereto at a concentration of 10 mg / L and the gelatin additive was completely dissolved to obtain a post-reaction leachate. The post-reaction leachate was placed in an electrolytic device, and then the anode plate and the cathode plate were connected to a DC circuit. The temperature of the post-reaction leachate was maintained at 80°C by the control of the electrolytic device, the distance between the anode plate and the cathode plate was controlled at 4 cm, and the current density was 400 A / m 2 , which can be used to produce lead dioxide on the anode plate.

[0079] In the process of preparing the pure ammonium chloride solution and the leaching process of the embodiment of the present invention, it is not necessary to add ammonia water or pass ammonia gas, and the leachate exists in a stable form during the electrolysis process, thereby saving material consumption and reducing costs. Secondly, by placing the leachate in an electrolysis device for electrolysis, the electrolysis device can control the temperature of the leachate so that the temperature of the leachate is moderate; in addition, the pH value of the leachate can be maintained in a near-neutral state, which has the advantage of not being easy to corrode the equipment. In addition, due to the strong selectivity of the pure ammonium chloride solution, the leachate can be directly put into electrolysis without going through complicated purification steps. The method has the advantages of simple and controllable operation, low cost and environmental friendliness, and the purity and macroscopic morphology of the lead dioxide product can meet the basic requirements of industrial production.

[0080] Furthermore, the embodiment of the present invention uses pure ammonium chloride solution, which can give play to the selectivity advantage of zinc, lead and chlorine forming a complex, ensuring that zinc and lead ions are stably present in the form of a complex during the electrolysis process, avoiding the hydrolysis of zinc and lead ions in the leachate, the influence of organic matter on the morphology of the anode product, and the easy peeling of the anode product layer. The problem that the secondary lead-zinc resources are difficult to recover after leaching with pure ammonium chloride is solved. This method is particularly suitable for the recovery and treatment of valuable metals in the leachate of secondary lead-zinc resources. Secondly, adding ammonia water or ammonium chloride to the waste electrolyte can achieve recycling, achieving the goal of efficient production and energy conservation and emission reduction.

[0081] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system, characterized in that: include: Obtaining lead-zinc-containing materials; Adding ammonium chloride to water to prepare a pure ammonium chloride solution, wherein no ammonia water is added and no ammonia gas is introduced during the preparation of the pure ammonium chloride solution, the purity of ammonium chloride in the pure ammonium chloride solution is greater than 95%, and the concentration of the ammonium chloride is 3.0-7.0 mol / L; The lead-zinc-containing material is placed in the pure ammonium chloride solution for leaching to obtain a leachate, wherein no ammonia water is added and no ammonia gas is introduced during the leaching process; The leaching solution is placed in an electrolysis device maintained at a preset temperature and a preset current density for electrolysis, and lead dioxide is obtained on the anode plate of the electrolysis device; wherein the preset temperature is 70 to 90° C., and the preset current density is 200 to 500 A / m 2 .

2. The method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system as claimed in claim 1, characterized in that: The obtaining of the lead-zinc-containing material specifically comprises: The smelting slag in the closed blast furnace is fumed and reduced in a fuming furnace to obtain fumed ash; The fumed ash is obtained to obtain the lead-zinc-containing material.

3. The method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system as claimed in claim 1, characterized in that: The lead content in the leaching solution is greater than or equal to 0.1 mol / L.

4. The method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system as claimed in claim 1, characterized in that: The distance between the cathode plate and the anode plate of the electrolysis device is 3 to 5 cm.

5. The method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system as claimed in claim 4, characterized in that: The anode plate is a ruthenium-coated titanium mesh, a graphite plate, a titanium plate or a stainless steel plate; the cathode plate is a titanium plate, an aluminum plate or a stainless steel plate.

6. The method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system as claimed in claim 1, characterized in that: After leaching the lead-zinc material into the pure ammonium chloride solution to obtain a leachate, the method further comprises: Adding an electrodeposition additive to the leaching solution and completely dissolving the electrodeposition additive to obtain a reacted leaching solution; The post-reaction leaching solution is placed in the electrolysis device for electrolysis to obtain the lead dioxide.

7. The method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system as claimed in claim 6, characterized in that: The type of the electrodeposition additive is bone glue, and the concentration range of the electrodeposition additive is 5-50 mg / L.

8. The method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system as claimed in claim 1, characterized in that: The leachate includes iron ions. After the lead-containing material is placed in the pure ammonium chloride solution for leaching to obtain the leachate, the method further includes: Purifying the leachate to obtain a purified leachate; The purified leaching solution is placed in the electrolysis device for electrolysis to obtain the lead dioxide.

9. The method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system as claimed in claim 1, characterized in that: The method further comprises: The lead dioxide is stripped and cleaned to obtain cleaned lead dioxide.

10. The method for preparing lead dioxide using a lead-zinc-ammonia-chlorine complex system according to any one of claims 1 to 9, characterized in that: The electrolysis device is a polyvinyl chloride electrolysis cell.