Method for improving metal micro-electroforming uniformity
By using photolithography in microelectroforming technology to prepare annular assisted cathode and optimize its position and shape, the problem of uneven thickness of the electroforming layer is solved, significantly improving the uniformity of metal microelectroforming and reducing subsequent processing steps and manufacturing costs.
Patent Information
- Application Number
- CN202310621278.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-29
- Publication Date
- 2024-11-29
AI Technical Summary
In the existing microelectroforming technology, the thickness unevenness of the electroforming layer results in the subsequent steps requiring grinding/polishing, extending the manufacturing cycle and increasing the manufacturing cost.
Based on photolithography technology, an annular auxiliary cathode is prepared to cover the uneven current density area. By setting conductive seed layers on different photoresist layers, the position and shape of the cathode and auxiliary cathode are optimized to improve the uniformity of metal microelectroforming.
Minimize the impact of uneven current density areas on the uniformity of plating, significantly improve the uniformity of metal microelectroforming, reduce the demand for subsequent processing steps, shorten the manufacturing cycle and reduce manufacturing costs.
Smart Images

Figure CN119040972A_ABST
Abstract
Description
Technical Field
[0001] This document relates to the field of micro-manufacturing technology, and in particular to a method for improving the uniformity of metal micro-electroforming. Background Art
[0002] In recent years, micro-electroforming based on UV (Ultraviolet Rays)-LIGA (Lithographie, Galvanoformung and Abformung, photolithography, electroforming and injection molding) technology has become one of the important technologies for manufacturing micro-metal devices in the field of micro-electromechanical system technology.
[0003] It combines photolithography and electrodeposition, and has the advantages of high precision, large processing size, and mass production.
[0004] However, the above solution will cause uneven thickness of the electroformed layer, so in the subsequent steps, post-processing (grinding / polishing) is required to ensure dimensional accuracy and surface quality, which prolongs the manufacturing cycle and increases the manufacturing cost. Summary of the invention
[0005] In view of the above analysis, the present application aims to propose a method for improving the uniformity of metal micro-electroforming based on an auxiliary cathode to improve the uniformity of metal micro-electroforming.
[0006] One or more embodiments of this specification provide a method for improving uniformity of metal micro-electroforming, including:
[0007] Based on the photolithography technology, an auxiliary cathode is prepared in the area with uneven current density according to the position of the cathode on the substrate;
[0008] The auxiliary cathode is annular, arranged around the cathode, and covers the current density non-uniform area. The current density non-uniform area reduces the plating uniformity of the electroforming area during metal micro-electroforming.
[0009] Furthermore, the shape of the annular cross section of the auxiliary cathode is adapted to the cross section shape of the cathode.
[0010] Further, based on the photolithography technology, a plurality of photoresist layers are formed on the substrate;
[0011] The auxiliary cathode and the cathode are located in different photoresist layers.
[0012] Furthermore, a conductive seed layer is arranged between the photoresist layer where the auxiliary cathode is located and the photoresist layer where the cathode is located.
[0013] Furthermore, the auxiliary cathode is prepared in the area with uneven current density based on the photolithography technology according to the position of the cathode on the substrate, including:
[0014] Based on the photolithography technology, a first photoresist layer is prepared on the substrate;
[0015] Based on photolithography technology, a cathode is arranged on the first photoresist layer;
[0016] Disposing a first conductive seed layer on the first photoresist layer and the cathode;
[0017] Disposing a second photoresist layer on the first conductive seed layer;
[0018] Determining the auxiliary cathode coverage area in the second photoresist layer;
[0019] The auxiliary cathode is disposed in the auxiliary cathode covering region.
[0020] Further, the step of providing a first conductive seed layer on the first photoresist layer comprises:
[0021] On the first photoresist layer, a second conductive seed layer covering the cathode is provided;
[0022] disposing a third photoresist layer on the second conductive seed layer;
[0023] The third photoresist layer and the second conductive seed layer covering the cathode are removed to obtain the first conductive seed layer.
[0024] Further, determining the auxiliary cathode coverage area in the second photoresist layer includes:
[0025] Determining the horizontal distance between the auxiliary cathode and the cathode according to a preset processing accuracy;
[0026] Determining the size of the auxiliary cathode according to the size of the second photoresist layer;
[0027] The auxiliary cathode coverage area is determined according to the horizontal distance between the auxiliary cathode and the cathode and the size of the auxiliary cathode.
[0028] Further, after the auxiliary cathode is arranged in the auxiliary cathode covering area, the method further comprises:
[0029] Performing metal micro-electroforming on the cathode and the auxiliary cathode simultaneously;
[0030] The first photoresist layer is removed.
[0031] Furthermore, the cross-sectional shape of the auxiliary cathode is any one of a circle, a triangle, a rectangle, a polygon and a polygon with a gear structure.
[0032] Compared with the prior art, this application can at least achieve the following technical effects:
[0033] By using an annular auxiliary cathode surrounding the cathode, the current density non-uniform area during electroforming can be covered to the maximum extent, thereby minimizing the impact of the current density non-uniform area on the uniformity of the coating, and ultimately improving the uniformity of metal micro-electroforming. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate one or more embodiments of this specification or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in this specification. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0035] Figure 1 A schematic diagram of the structure of a photoresist mold in the prior art provided for one or more embodiments of this specification;
[0036] Figure 2 A schematic diagram of a cathode and an auxiliary cathode formed by the same layer of photoresist provided in one or more embodiments of this specification;
[0037] Figure 3 A flow chart of a method for improving uniformity of metal micro-electroforming provided for one or more embodiments of this specification;
[0038] Figure 4 A schematic diagram of the structure of a photoresist mold after a cathode is disposed on a substrate provided in one or more embodiments of this specification;
[0039] Figure 5 A schematic diagram of the structure of a photoresist mold after generating a first conductive seed layer provided for one or more embodiments of this specification;
[0040] Figure 6 A schematic structural diagram of a photoresist mold after generating a second conductive seed layer provided for one or more embodiments of this specification;
[0041] Figure 7 A schematic structural diagram of a photoresist mold after a third photoresist layer is provided for one or more embodiments of this specification;
[0042] Figure 8 A schematic diagram of a process for generating an auxiliary cathode provided for one or more embodiments of this specification;
[0043] Fig. 9A schematic diagram of a process of forming a photoresist mold with a microstructure pattern, an auxiliary cathode pattern, and a peripheral conductive structure pattern provided for one or more embodiments of the present specification;
[0044] Fig.10 A top view of four basic microstructures with auxiliary cathodes provided for one or more embodiments of this specification;
[0045] Fig.11 Structural schematic diagrams of four basic microstructures provided for one or more embodiments of this specification;
[0046] Fig.12 A schematic diagram of a micro-gear structure provided for one or more embodiments of this specification;
[0047] Fig.13 A top view of a micro-gear structure with an auxiliary cathode provided for one or more embodiments of the present specification.
[0048] Description of reference numerals:
[0049] 1-substrate; 2-first negative photoresist; 3-mask with microstructure pattern and peripheral conductive structure pattern; 4-conductive seed layer; 5-second negative photoresist; 6-mask with microstructure pattern; 7-third negative photoresist; 8-mask with microstructure pattern, auxiliary cathode pattern and peripheral conductive structure pattern. DETAILED DESCRIPTION
[0050] In order to enable those skilled in the art to better understand the technical solutions in one or more embodiments of this specification, the following will be combined with the drawings in one or more embodiments of this specification to clearly and completely describe the technical solutions in one or more embodiments of this specification. Obviously, the described embodiments are only part of the embodiments of this specification, not all of the embodiments. Based on one or more embodiments of this specification, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of this document.
[0051] Before micro-electroforming, a cathode needs to be set on the substrate, that is, a micro-electroforming area is formed between the substrate surface and the photoresist layer, such as Figure 1 As shown. Figure 1 The structure in the micro-electroforming is micro-electroforming. During micro-electroforming, the current density in the micro-electroforming area, especially the edge area, is uneven, while the current density in the middle area of the micro-electroforming is relatively uniform. Therefore, the uniformity of micro-electroforming is poor. The prior art usually determines an area on the photoresist near the cathode, which is used to set an auxiliary cathode to improve the uniformity of micro-electroforming. However, the above solution has two defects:
[0052] 1. When setting the structure of the existing auxiliary electrode, it is usually necessary to use a cathode product that is not made of photoresist alone, or to set it on one side of the cathode based on photolithography technology, which makes the existing auxiliary electrode have great limitations in improving the uniformity of micro-electroforming.
[0053] 2. When the existing auxiliary electrode is set, the cathode and the set auxiliary cathode are usually formed by the same layer of photoresist, such as Figure 2 As shown, the effect of the cathode and the auxiliary cathode being in different photoresist layers on the current density distribution is neglected.
[0054] In view of the above problems, the embodiment of the present application proposes a method for improving the uniformity of metal micro-electroforming. Based on the photolithography technology, an auxiliary cathode is prepared in the area of uneven current density according to the position of the cathode on the substrate. The auxiliary cathode is annular, arranged around the cathode, and covers the area of uneven current density. The area of uneven current density reduces the uniformity of the coating in the electroforming area during metal micro-electroforming.
[0055] The annular and surrounding cathode can make the auxiliary cathode cover the current density non-uniform area to the greatest extent. The auxiliary cathode is made based on photolithography technology, so that the user does not need to prepare the auxiliary cathode separately, but only needs to add the process of making the auxiliary cathode to the usual photolithography process. The auxiliary cathode thus made has better adaptability than the auxiliary cathode prepared separately.
[0056] Among them, the shape of the auxiliary cathode annular cross-section is adapted to the cathode cross-section shape. Specifically, the shape of the auxiliary cathode annular cross-section is the same as the cathode cross-section shape. For example, if the cathode cross-section shape is circular, then the cross-sectional shape of the auxiliary cathode is circular. Or the shape of the auxiliary cathode annular cross-section is similar to the cathode cross-sectional shape, for example, the cathode cross-sectional shape is a rounded sawtooth polygon, the auxiliary cathode cross-sectional shape is an acute sawtooth polygon, and the number of sides of the polygon is the same. It should be noted that in order to better achieve the adaptation of the shape of the auxiliary cathode annular cross-section to the cathode cross-sectional shape, in an embodiment of the present application, the cross-sectional shape of the auxiliary cathode is any one of a circle, a triangle, a rectangle, a polygon and a polygon with a gear structure.
[0057] In order to address defect 2, preferably, based on photolithography technology, multiple photoresist layers are formed on the substrate; the auxiliary cathode and the cathode are located in different photoresist layers. In the embodiment of the present application, the increase in the thickness of the photoresist can reduce the difference in current density between the edge area of the micro-electroforming and the middle area of the micro-electroforming. Based on this, a new photoresist layer is set on the photoresist layer corresponding to the cathode, and the newly set photoresist layer is used to set the auxiliary cathode. The above method is equivalent to increasing the thickness of the photoresist layer where the cathode is located. Increasing the thickness of the photoresist layer where the cathode is located changes the distribution of current density in the micro-electroforming area. At the same time, based on the conductive properties of the photoresist, the auxiliary cathode and the cathode are in a conductive state during electroforming. Therefore, during electroforming, the entire cathode is equivalent to Figure 1 The middle area of micro-electroforming, and the auxiliary cathode is equivalent to Figure 1 The edge area of the micro-electroforming process is made to make the current density of the cathode relatively uniform. In addition, the auxiliary cathode on the cathode photoresist layer can be removed, so the auxiliary cathode will not affect the structure of the casting after micro-electroforming.
[0058] Preferably, in order to enhance the coordination effect between the cathode and the auxiliary cathode, a conductive seed layer is provided between the photoresist layer where the auxiliary cathode is located and the photoresist layer where the cathode is located. By providing the conductive seed layer, the conductive connectivity between the auxiliary cathode and the cathode is enhanced, thereby changing the distribution area of the current density, and further improving the uniformity of micro-electroforming.
[0059] The production of the auxiliary cathode specifically includes the following steps: Figure 3 As shown:
[0060] Step 1: Based on photolithography technology, prepare a first photoresist layer on a substrate.
[0061] Step 2: Based on the photolithography technology, a cathode is arranged on the first photoresist layer.
[0062] In the present application example, the structure obtained in step 2 is as follows Figure 4 As shown. The specific process is: spin-coat the first negative photoresist 2 (this photoresist forms the first photoresist layer) on the conductive substrate 1, perform pre-baking, and use a mask 3 with a microstructure pattern and a peripheral conductive structure pattern for exposure, wherein the microstructure is the device structure to be electroformed, and the peripheral conductive structure is located at the periphery of the mask, which plays the role of conducting the cathode structure and the auxiliary cathode layer in the subsequent electroforming process. After exposure, post-baking and development are performed to obtain a photoresist mold with a microstructure. Considering the adhesion of the photoresist to the substrate, a hardening operation can be performed. It should be noted that based on the micro-electroforming process, the microstructure is called a cathode.
[0063] Step 3: Dispose a first conductive seed layer on the first photoresist layer and the cathode.
[0064] In the present embodiment, the structure obtained in step 3 is as follows Figure 5 As shown. Wherein, 4 is a conductive seed layer. The specific process is:
[0065] Step 31: Dispose a second conductive seed layer covering the cathode on the first photoresist layer.
[0066] In the embodiment of the present application, a conductive seed layer 4 is prepared on the surface of the photoresist mold with a cathode, and the obtained structure is as follows: Figure 6 At this time, the conductive seed layer 4 covers the cathode. In order to distinguish it from the final structure, Figure 6 The conductive seed layer 4 in the embodiment is recorded as the second conductive seed layer. Figure 5 The conductive seed layer 4 in the embodiment is recorded as the first conductive seed layer.
[0067] Step 32: Dispose a third photoresist layer on the second conductive seed layer.
[0068] In the embodiment of the present application, a second negative photoresist 5 (the photoresist is used to obtain a third photoresist layer) is spin-coated on the surface with the entire seed layer, pre-baked, and exposed using a mask 6 with a microstructure pattern. Figure 7 shown.
[0069] Step 33: remove the third photoresist layer and the second conductive seed layer covering the cathode to obtain a first conductive seed layer.
[0070] In the embodiment of the present application, after exposure, post-baking and development are performed to obtain a photoresist film that does not shield only the sidewalls of the microstructure and the inside of the microstructure grooves. Afterwards, etching is performed to remove the seed layer on the sidewalls of the photoresist mold and the inside of the microstructure grooves and the second negative photoresist to obtain Figure 5 The structure shown.
[0071] Step 4: Dispose a second photoresist layer on the first conductive seed layer.
[0072] In the embodiments of the present application, Figure 8 As shown, a third negative photoresist 7 (the photoresist is used to obtain a second photoresist layer) is spin-coated on the surface of the seed layer substrate with the auxiliary cathode layer.
[0073] Step 5: Determine the auxiliary cathode coverage area in the second photoresist layer.
[0074] In the embodiments of the present application, Figure 8 As shown, pre-baking is performed, and exposure is performed using a mask 8 with a microstructure pattern, an auxiliary cathode pattern and a peripheral conductive structure pattern. That is, the auxiliary cathode coverage area is determined using the microstructure pattern, the auxiliary cathode pattern and the peripheral conductive structure pattern in the mask.
[0075] In the embodiment of the present application, the mask is prepared in advance, so it is necessary to predetermine the auxiliary cathode coverage area according to the process conditions. Specifically, according to the preset processing accuracy, the horizontal distance between the auxiliary cathode and the cathode is determined. According to the size of the second photoresist layer, the size of the auxiliary cathode is determined. According to the horizontal distance between the auxiliary cathode and the cathode and the size of the auxiliary cathode, the auxiliary cathode coverage area is determined.
[0076] It should be noted that the horizontal distance between the auxiliary cathode and the cathode is the thickness of the photoresist between the cathode and the auxiliary cathode. The smaller the thickness, the better, but the specific value of the thickness is affected by the processing accuracy. For example, the tolerance of the processing equipment is 5nm. Obviously, if the thickness is less than 5nm, it will cause a large error, so the optimal thickness value should be the tolerance of the processing equipment. The auxiliary cathode is annular, so the size of the auxiliary cathode is the annular width. Since the auxiliary cathode is to stabilize the current density, the longer the annular width, the larger the range of influence of the auxiliary cathode, and the better the effect of stabilizing the current density. The maximum limit of the annular width is that the outer ring contour line of the annular ring coincides with the edge of the second photoresist layer. Therefore, in order to ensure the micro-electroforming effect, the size of the auxiliary cathode needs to be determined according to the size of the second photoresist layer. When the horizontal distance between the auxiliary cathode and the cathode and the annular width are determined, the auxiliary cathode coverage area is determined.
[0077] Step 6: Arrange an auxiliary cathode in the auxiliary cathode coverage area.
[0078] In the embodiment of the present application, after exposure, post-baking and development are performed to obtain a double-layer photoresist mold having a cathode layer and an auxiliary cathode layer, such as Fig. 9 As shown. Considering the adhesion between the photoresist and the underlying material, a hardening operation can be performed. In order to ensure that the residual photoresist in the cathode groove and the auxiliary cathode groove is completely removed, plasma etching can be used for removal. Among them, the blank area of the second photoresist layer formed by the third negative photoresist 7 is the groove of the auxiliary cathode.
[0079] Preferably, the sum of the thicknesses of the first photoresist layer and the first conductive seed layer is determined according to the current density non-uniform area to control the vertical distance between the auxiliary cathode and the cathode, thereby controlling the current density area affected by the auxiliary cathode.
[0080] In the embodiment of the present application, the metal micro-electroforming process of the present application is:
[0081] Performing metal micro-electroforming on the cathode and the auxiliary cathode simultaneously;
[0082] The first photoresist layer is removed.
[0083] It can be seen from the above steps that the present application adds the process of constructing an auxiliary cathode to the process before metal micro-electroforming, so the above method can be applied to various types of metal micro-electroforming.
[0084] In order to illustrate the feasibility of the above embodiments of the present application, the present application takes four basic microstructures and microgears as examples and gives the following specific examples:
[0085] like Figure 10-13As shown, the basic unit size L of the four basic microstructures (circle, square, equilateral triangle, and regular hexagon) is 100μm, the diameter D of the micro gear is 960μm, the number of teeth is 10, and the module is 0.08mm. The outer contour of the auxiliary cathode structure of these five microstructures is exactly the same as the outer contour of the microstructure. The horizontal spacing G between the two is 10μm, and the width W of the auxiliary cathode structure is 40μm. The first negative photoresist and the third negative photoresist use SU-82025 with a thickness of 20μm, and the second negative photoresist uses L300 with a thickness of 3μm. The electroforming material is nickel, and the current density is 1A / dm 2 The electroforming time is 30 minutes. Compared with the microstructures electroformed without adding an auxiliary cathode, the casting uniformity of the four basic microstructures of circle, square, equilateral triangle, regular hexagon and the micro-gear structure prepared by the present invention are improved by 190.63%, 116.74%, 80.43%, 164.30% and 101.15% respectively.
[0086] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, commodity or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, commodity or device. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the process, method, commodity or device including the elements.
[0087] One or more embodiments of the present specification may be described in the general context of computer-executable instructions executed by a computer, such as program modules. Generally, program modules include routines, programs, objects, components, data structures, etc. that perform specific tasks or implement specific abstract data types. One or more embodiments of the present specification may also be practiced in distributed computing environments where tasks are performed by remote processing devices connected through a communication network. In a distributed computing environment, program modules may be located in local and remote computer storage media, including storage devices.
[0088] Each embodiment in this specification is described in a progressive manner, and the same or similar parts between the embodiments can be referred to each other, and each embodiment focuses on the differences from other embodiments. In particular, for the system embodiment, since it is basically similar to the method embodiment, the description is relatively simple, and the relevant parts can be referred to the partial description of the method embodiment.
[0089] The above description is only an embodiment of this document and is not intended to limit this document. For those skilled in the art, this document may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of this document should be included in the scope of the claims of this document.
Claims
1. A method for improving the uniformity of metal micro-electroforming, characterized in that: include: Based on the photolithography technology, an auxiliary cathode is prepared in the area with uneven current density according to the position of the cathode on the substrate; The auxiliary cathode is annular, arranged around the cathode, and covers the current density non-uniform area. The current density non-uniform area reduces the plating uniformity of the electroforming area during metal micro-electroforming.
2. The method according to claim 1, characterized in that The shape of the annular cross section of the auxiliary cathode is adapted to the cross section shape of the cathode.
3. The method according to claim 1, characterized in that Based on photolithography technology, forming a plurality of photoresist layers on the substrate; The auxiliary cathode and the cathode are located in different photoresist layers.
4. The method according to claim 3, characterized in that A conductive seed layer is arranged between the photoresist layer where the auxiliary cathode is located and the photoresist layer where the cathode is located.
5. The method according to claim 1, characterized in that The method is based on photolithography technology and according to the position of the cathode on the substrate, in the area with uneven current density, to prepare an auxiliary cathode, comprising: Based on the photolithography technology, a first photoresist layer is prepared on the substrate; Based on photolithography technology, a cathode is arranged on the first photoresist layer; Disposing a first conductive seed layer on the first photoresist layer and the cathode; Disposing a second photoresist layer on the first conductive seed layer; Determining the auxiliary cathode coverage area in the second photoresist layer; The auxiliary cathode is disposed in the auxiliary cathode covering region.
6. The method according to claim 5, characterized in that The step of disposing a first conductive seed layer on the first photoresist layer comprises: On the first photoresist layer, a second conductive seed layer covering the cathode is provided; Disposing a third photoresist layer on the second conductive seed layer; The third photoresist layer and the second conductive seed layer covering the cathode are removed to obtain the first conductive seed layer.
7. The method according to claim 5, characterized in that The step of determining the auxiliary cathode coverage area in the second photoresist layer comprises: Determining the horizontal distance between the auxiliary cathode and the cathode according to a preset processing accuracy; Determining the size of the auxiliary cathode according to the size of the second photoresist layer; The auxiliary cathode coverage area is determined according to the horizontal distance between the auxiliary cathode and the cathode and the size of the auxiliary cathode.
8. The method according to claim 5, characterized in that The method further comprises: The sum of the thicknesses of the first photoresist layer and the first conductive seed layer is determined according to the current density non-uniform area.
9. The method according to claim 5, characterized in that After the auxiliary cathode is disposed in the auxiliary cathode covering region, the method further comprises: Performing metal micro-electroforming on the cathode and the auxiliary cathode simultaneously; The first photoresist layer is removed.
10. The method according to any one of claims 1 to 9, characterized in that: The cross-sectional shape of the auxiliary cathode is any one of a circle, a triangle, a rectangle, a polygon and a polygon with a gear structure.