Composite nanofiber membrane, preparation method thereof and flexible piezoelectric device
By preparing composite nanofiber membranes, the combination of barium titanate nanoflower powder and polydopamine and P(VDF-TrFE) nanoparticles was solved, and the problem of single stress conduction mode and low piezoelectric output of flexible piezoelectric devices was achieved, achieving high efficiency Mechanical enhancement and surface modification improve the output voltage and usability of piezoelectric devices.
Patent Information
- Application Number
- CN202411171135.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing flexible piezoelectric devices have a single stress conduction mode and relatively low piezoelectric output, making it difficult to achieve efficient skin fit and mechanical enhancement.
Using the preparation method of composite nanofiber membrane, BTO@PDA nanoflower/P(VDF-TrFE) composite is prepared by combining barium titanate nanoflower powder with polydopamine and P(VDF-TrFE) nanoparticles. Nanofiber membranes achieve mechanical enhancement and surface modification and improve piezoelectric output.
The output voltage of piezoelectric devices is significantly improved to reach up to 90V, enhancing the mechanical properties and skin fit characteristics of flexible piezoelectric devices, and improving the usability and sensitivity of piezoelectric devices.
Smart Images

Figure CN119041097A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nano functional materials, and more specifically, relates to a composite nano fiber membrane and a preparation method thereof, and a flexible piezoelectric device. Background Art
[0002] In recent years, flexible piezoelectric materials have played an important role in the development of flexible electronics. Flexible piezoelectric materials based on PVDF (polyvinylidene fluoride) and its copolymers have shown high usability. They can be used as pressure sensors to collect information about human motion, or as energy devices to collect energy from human motion, get rid of the dependence of electronic devices on batteries, and develop the next generation of integrated electronic devices. Traditional piezoelectric pressure sensors are mainly constructed using piezoelectric ceramic sheets, which inevitably lead to insurmountable problems such as fragility and difficulty in skin application, which hinders the application of wearable pressure sensors.
[0003] In order to meet the above challenges, polymer-based piezoelectric sensors have received great attention. PVDF is a piezoelectric polymer with good flexibility. PVDF and its copolymers have good flexibility and skin-fitting properties, but compared with piezoelectric ceramics, PVDF and its copolymers have weak piezoelectric output and sensor sensitivity. In current research, doping piezoelectric ceramics or other nanoparticles in PVDF and its copolymers to enhance the piezoelectric output of PVDF has become the main research method.
[0004] At present, research mainly focuses on the use of spherical nanoparticle fillers, which have a single stress conduction mode and relatively low piezoelectric output. For example, a flexible piezoelectric device composed of spherical BTO and PVDF described in Chinese patent CN201911342594.3 has a maximum output of only 14V. Summary of the invention
[0005] Based on the technical problems existing in the prior art, the present invention provides a composite nanofiber membrane and a preparation method thereof and a flexible piezoelectric device, aiming to solve the technical problems of the existing flexible piezoelectric devices having a single stress conduction mode and relatively low piezoelectric output.
[0006] To achieve the above object, according to a first aspect of the present invention, a method for preparing a composite nanofiber membrane is provided, comprising the following steps:
[0007] Step S1, dissolving tetrabutyl titanate in an alcohol solvent to obtain a tetrabutyl titanate solution;
[0008] Step S2, sterilizing the tetrabutyl titanate solution at high temperature, washing and drying to obtain titanium-containing powder;
[0009] Step S3, calcining the titanium-containing powder at high temperature, washing and drying to obtain flower-shaped anatase titanium dioxide powder;
[0010] Step S4, mixing the flower-shaped anatase titanium dioxide powder and barium hydroxide into deionized water, stirring evenly with a magnetic stirrer, and then performing ultrasonic treatment to obtain a titanium-containing mixed solution;
[0011] Step S5, calcining the titanium-containing mixed solution at high temperature to obtain barium titanate nanoflower powder;
[0012] Step S6, mixing the barium titanate nanoflower powder and the dopamine hydrochloride powder, adding Tris-HCl to dissolve, performing magnetic stirring, and centrifuging and washing to obtain BTO@PDA nanoflower powder;
[0013] Step S7, adding P(VDF-TrFE) nanoparticles into DMF, and preparing P(VDF-TrFE) electrospinning solution after magnetic stirring;
[0014] Step S8, adding BTO@PDA nanoflower powder to the P(VDF-TrFE) electrospinning solution, stirring evenly, and using electrospinning technology to prepare a composite nanofiber membrane.
[0015] Optionally, the alcohol solvent is a mixed solvent of any one of ethanol, deionized water, methanol, isopropanol and glycerol.
[0016] Optionally, the alcohol solvent is a mixed solvent of ethanol and glycerol, the added amount of ethanol is 10ml-50ml, the added amount of glycerol is 5ml-15ml, and the added amount of tetrabutyl titanate is 1g-3g.
[0017] Optionally, in step S2, the tetrabutyl titanate solution is sterilized at high temperature, washed and then dried to obtain a titanium-containing powder, and the tetrabutyl titanate solution is heated in an autoclave at a heating temperature of 180° C. for 24 hours. The filling factor of the autoclave is 0.4, the washing centrifuge speed is 5000 rpm, and the washing times are 5 times.
[0018] Optionally, in step S3, the titanium-containing powder is calcined at high temperature, washed and then dried to obtain a flower-shaped anatase titanium dioxide powder, and the titanium-containing powder is calcined at high temperature in an autoclave, the high temperature calcination temperature is 450°C, the calcination time is 3 hours, the washing centrifuge speed is 5000 rpm, and the washing times are 5 times.
[0019] Optionally, in step S4, the flower-shaped anatase titanium dioxide powder and barium hydroxide are mixed and added to deionized water, magnetically stirred and ultrasonically treated to obtain a titanium-containing mixed solution, the amount of the flower-shaped anatase titanium dioxide powder added is 0.1g to 0.2g, the amount of barium hydroxide added is 0.5g to 0.7g, the amount of deionized water added is 40ml, the magnetic stirring frequency is 500 times / minute, and the stirring time is 1 hour.
[0020] Optionally, the concentration of barium titanate nanoflower powder in the prepared dissolving solution is 10 g / L, and the concentration of dopamine hydrochloride is 0.1 mol / L.
[0021] Optionally, the amount of P(VDF-TrFE) nanoparticles added is 0.1 g to 3 g, and the amount of DMF added is 2 ml to 18 ml.
[0022] According to a second aspect of the present invention, there is provided a composite nanofiber membrane, which is prepared by the above-mentioned preparation method.
[0023] According to a third aspect of the present invention, a flexible piezoelectric device is provided, which includes the composite nanofiber membrane prepared as described above, wherein aluminum-platinum electrodes are provided on the upper and lower sides of the composite nanofiber membrane respectively, and a flexible piezoelectric device is obtained after packaging.
[0024] Compared with the prior art, the composite nanofiber membrane and the preparation method thereof and the flexible piezoelectric device provided by the present invention have the following beneficial effects:
[0025] (1) The BTO nanoflowers prepared by the present invention have good morphology, obvious petal structure, excellent mechanical reinforcement properties, and significant effect on improving the output of piezoelectric devices;
[0026] (2) The BTO@polydopamine (PDA) nanoflowers prepared in the present invention have good morphology, a coated shell structure, and excellent filler surface modification effect, and have a significant effect on improving the output of piezoelectric devices.
[0027] (3) The BTO@PDA nanoflower / P(VDF-TrFE) composite nanofiber membrane prepared by the present invention has good morphology, obvious filling structure, excellent flexibility and skin-fitting properties, and has a significant effect on improving the output of piezoelectric devices;
[0028] (4) The present invention realizes for the first time the application of BTO@PDA nanoflowers / P(VDF-TrFE) composite nanofiber membranes in piezoelectric devices.
[0029] (5) The present invention realizes for the first time the application of mechanical enhancement and surface modification methods acting on nanofillers in flexible piezoelectric devices, which plays an important role in improving the performance of piezoelectric devices and enhancing the usability of piezoelectric devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0031] Figure 1 is a schematic diagram of a process for preparing a composite nanofiber membrane according to the present invention;
[0032] Figure 2 A schematic diagram of the process of preparing a composite nanofiber membrane according to the present invention;
[0033] Figure 3 is a schematic diagram of the morphology of the barium titanate nanoflower powder under a scanning electron microscope according to the present invention;
[0034] Figure 4 A schematic diagram of the morphology of the BTO@PDA nanoflower powder under a scanning electron microscope according to the present invention;
[0035] Figure 5 is a schematic diagram of the morphology of the composite nanofiber membrane under a scanning electron microscope according to the present invention;
[0036] Figure 6 is a schematic diagram of the morphology of the composite nanofiber membrane according to the present invention under a transmission electron microscope;
[0037] Figure 7 is the stress distribution of the nanosphere inside the piezoelectric material;
[0038] Figure 8 The stress distribution of the nanoflowers in the piezoelectric material according to the present invention;
[0039] Fig. 9 It is the voltage output of the flexible piezoelectric device under vertical force conditions according to the present invention. DETAILED DESCRIPTION
[0040] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0041] It should be noted that when an element is referred to as being "fixed to" or "arranged on" another element, it may be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or indirectly connected to the other element. In the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0042] It should be understood that the orientation or position relationship indicated by terms such as "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0043] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.
[0044] See also Figure 1 As shown, the first aspect of the embodiment of the present invention provides a method for preparing a composite nanofiber membrane, which is a filler surface modification and mechanical enhancement method for enhancing the performance of a composite piezoelectric device, specifically a method for filling a piezoelectric polymer matrix with a shape-optimized and surface-modified filler to improve the piezoelectric properties of the matrix and thus improve the output of the piezoelectric device. Specifically, the following steps are included:
[0045] Step S1, dissolving tetrabutyl titanate in an alcohol solvent to obtain a tetrabutyl titanate solution;
[0046] Step S2, sterilizing the tetrabutyl titanate solution at high temperature, washing and drying to obtain titanium-containing powder;
[0047] Step S3, calcining the titanium-containing powder at high temperature, washing and drying to obtain flower-shaped anatase titanium dioxide powder;
[0048] Step S4, mixing the flower-shaped anatase titanium dioxide powder and barium hydroxide into deionized water, stirring evenly with a magnetic stirrer, and then performing ultrasonic treatment to obtain a titanium-containing mixed solution;
[0049] Step S5, calcining the titanium-containing mixed solution at high temperature to obtain barium titanate nanoflower powder;
[0050] Step S6, mixing the barium titanate nanoflower powder and the dopamine hydrochloride powder, adding Tris-HCl to dissolve, performing magnetic stirring, and centrifuging and washing to obtain BTO@polydopamine (PDA) nanoflower powder;
[0051] Step S7, adding P(VDF-TrFE) nanoparticles into DMF, and preparing P(VDF-TrFE) electrospinning solution after magnetic stirring;
[0052] Step S8, adding BTO@PDA nanoflower powder to the P(VDF-TrFE) electrospinning solution, stirring evenly, and using electrospinning technology to prepare a composite nanofiber membrane.
[0053] The preparation method of the composite nanofiber membrane provided by the embodiment of the present invention prepares BTO@PDA nanoflower powder through barium titanate nanoflower powder, prepares P(VDF-TrFE) electrospinning solution through P(VDF-TrFE) nanoparticles, and prepares the composite nanofiber membrane through BTO@PDA nanoflower powder and P(VDF-TrFE) electrospinning solution, wherein the BTO@PDA nanoflower powder has good morphology, a coating shell structure and excellent filler surface modification effect, which can significantly improve the stress transfer efficiency. Compared with nanosphere particles, it can make the internal stress more concentrated and achieve higher piezoelectric output, so that the prepared composite nanofiber membrane has good morphology, and the surface-modified filler can achieve excellent coating effect and mechanical enhancement characteristics, thereby improving the piezoelectric properties of the composite nanofiber membrane and facilitating the output of the piezoelectric device.
[0054] In some embodiments, in the above step S1, the alcohol solvent is a mixed solvent of any one of ethanol, deionized water, methanol, isopropanol and glycerol. Tetrabutyl titanate is a titanium source for titanium dioxide. After adding ethanol, methanol or isopropanol and dissolving, coordination can occur to form a complex, stabilize the molecular structure of tetrabutyl titanate, slow down the reaction rate, and reduce the generation of by-products. The addition of glycerol can control the pH and viscosity of the system, control the dynamic growth of the crystal, and form a special petal-like morphology.
[0055] In some embodiments, the alcohol solvent is a mixed solvent of ethanol and glycerol. The amount of ethanol added is 10ml to 50ml, the amount of glycerol added is 5ml to 15ml, and the amount of tetrabutyl titanate added is 1g to 3g. Ethanol and glycerol serve to control the crystal growth dynamics and promote the formation of petal-like morphology structures. Good particle size and morphology can be achieved within the addition range. Exemplarily, the amount of ethanol added is 30ml, the amount of glycerol added is 10ml, and the amount of tetrabutyl titanate added is 2g.
[0056] In some embodiments, in the above step S2, the tetrabutyl titanate solution is sterilized at high temperature, washed and dried to obtain a titanium-containing powder, and the tetrabutyl titanate solution is heated in an autoclave, wherein the heating temperature is 180°C, the heating time is 24 hours, the filling factor of the autoclave is 0.4, the washing centrifugal speed is 5000 rpm, and the washing times are 5 times.
[0057] In some embodiments, in the above step S3, the titanium-containing powder is calcined at high temperature, and after washing and drying, the flower-shaped rutile titanium dioxide powder is obtained. The titanium-containing powder is calcined at high temperature in an autoclave, wherein the high temperature calcination temperature is 450°C, the calcination time is 3 hours, the washing centrifugal speed is 5000 rpm, and the washing times are 5 times.
[0058] In some embodiments, in the above step S4, the flower-shaped anatase titanium dioxide powder and barium hydroxide are mixed and added to deionized water, and after magnetic stirring, ultrasonic treatment is performed to obtain a titanium-containing mixed solution, the amount of flower-shaped anatase titanium dioxide powder added is 0.1g~0.2g, the amount of barium hydroxide added is 0.5g~0.7g, the amount of deionized water added is 40ml, the magnetic stirring frequency is 500 times / minute (or 500 rpm), and the stirring time is 1 hour. Exemplarily, the amount of flower-shaped anatase titanium dioxide powder added is preferably 0.16g, and the amount of barium hydroxide added is 0.63g.
[0059] Among them, titanium dioxide serves as the titanium source of barium titanate, and barium hydroxide serves as the barium source. The two are mixed and sintered to form barium titanate nanoflowers with good morphology. Within the scope of use, it can be ensured that the generated product has good morphology, small size, and no obvious by-products are generated.
[0060] In some embodiments, in the above step S5, the titanium-containing mixed solution is added into a high pressure autoclave and calcined to obtain barium titanate (BaTiO3, BTO) nanoflower powder, wherein the high temperature calcination temperature is 600°C and the calcination time is 3 hours.
[0061] In some embodiments, in the above step S6, after the barium titanate nanoflower powder and the dopamine hydrochloride powder are mixed, Tris-HCl is added to dissolve, and after magnetic stirring, the BTO@PDA nanoflower powder is obtained by centrifugal washing, and the concentration of the barium titanate nanoflower powder in the configured dissolving solution is 10 g / L, and the concentration of dopamine hydrochloride is 0.1 mol / L.
[0062] In some embodiments, in the above step S7, P(VDF-TrFE) nanoparticles are added to DMF (N,N-dimethylformamide), and after magnetic stirring, P(VDF-TrFE) electrospinning solution is prepared, wherein the amount of P(VDF-TrFE) nanoparticles added is 0.1g to 3g, and the amount of DMF added is 2ml to 18ml. Exemplarily, the amount of P(VDF-TrFE) nanoparticles added is 1g, and the amount of DMF added is 8ml.
[0063] In some embodiments, in the above step S8, a certain amount of BTO@PDA nanoflower powder is added to the P(VDF-TrFE) electrospinning solution and stirred evenly, and then an electrospinning machine is used to prepare a composite nanofiber membrane, wherein the inter-electrode voltage of the electrospinning machine is 15kV, the distance between the positive and negative electrodes is 10cm, the injection speed is 0.3ml / h, and the injection depth is 1ml.
[0064] The second aspect of the embodiment of the present invention provides a composite nanofiber membrane, which is prepared by the preparation method of the first aspect. The composite nanofiber membrane prepared by the present invention has good morphology, and the surface-modified filler can achieve excellent coating effect and mechanical enhancement properties, improve the piezoelectric properties of the composite nanofiber membrane, and is conducive to improving the output of the piezoelectric device.
[0065] The third aspect of the embodiment of the present invention provides a flexible piezoelectric device, including the composite nanofiber membrane of the second aspect, wherein aluminum-platinum electrodes are respectively provided on the upper and lower sides of the composite nanofiber membrane, and a flexible piezoelectric device is obtained after packaging. The composite nanofiber membrane prepared by the present invention utilizes the electrostatic interaction between the modified polydopamine (PDA) surface and the P (VDF-TrFE) segment to improve the sensitivity of the pressure sensor, and utilizes the special structure of the barium titanate nanoflower to concentrate the internal stress, thereby ultimately enhancing the electrical output of the pressure sensor, improving the sensitivity and self-powered power.
[0066] The following describes the invention in conjunction with specific embodiments.
[0067] Example 1
[0068] See also Figure 2 As shown, the preparation of BTO@PDA nanoflower filler includes the following steps:
[0069] Step S1, mixing ethanol and glycerol to dissolve tetrabutyl titanate to obtain a tetrabutyl titanate solution, wherein the added amount of ethanol is 30 ml, the added amount of glycerol is 10 ml, and the added amount of tetrabutyl titanate is 2 g;
[0070] Step S2, adding tetrabutyl titanate solution into an autoclave for high temperature sterilization, followed by washing and drying, to obtain titanium-containing powder, wherein the high temperature heating temperature is 180° C., the heating time is 24 h, the filling factor of the autoclave is 0.4, the washing centrifugal speed is 5000 rpm, and the washing times are 5 times;
[0071] Step S3, placing the titanium-containing powder in an autoclave for high-temperature calcination, and then washing and drying to obtain a flower-shaped anatase titanium dioxide powder, wherein the high-temperature calcination temperature is 450° C., the calcination time is 3 h, the washing centrifugal speed is 5000 rpm, and the washing times are 5 times;
[0072] Step S4, adding the flower-shaped anatase titanium dioxide powder and barium hydroxide to deionized water and magnetically stirring them, followed by ultrasonic treatment to obtain a titanium-containing mixed solution, wherein the amount of deionized water added is 40 ml, the magnetic stirring frequency is 500 times / min (or 500 rpm), the stirring time is 1 hour, the amount of the flower-shaped anatase titanium dioxide powder added is 0.16 g, and the amount of the barium hydroxide added is 0.63 g;
[0073] Step S5, adding the titanium-containing mixed solution into an autoclave and calcining to obtain barium titanate (BaTiO3, BTO) nanoflower powder, wherein the high-temperature calcination temperature is 600° C. and the calcination time is 3 hours;
[0074] Step S6, mixing a certain amount of barium titanate nanoflower powder and a certain amount of dopamine hydrochloride powder, adding Tris-HCl to dissolve, magnetically stirring and centrifugally washing to obtain BTO@PDA nanoflower powder, wherein the concentration of barium titanate nanoflower powder is 10 g / L, and the concentration of dopamine hydrochloride is 0.1 mol / L.
[0075] like Figure 3 The scanning electron microscopy results shown in the figure show that the surface of the prepared barium titanate nanoflower powder has an obvious thorn-like petal structure, indicating that the nanoflower structure is well formed and can achieve the improvement of the mechanical structure.
[0076] like Figure 4 The scanning electron microscopy results shown in the figure show that the prepared BTO@PDA nanoflower powder has a good coating structure and completes the surface modification.
[0077] Example 2
[0078] The preparation of the composite nanofiber membrane specifically comprises the following steps:
[0079] Step S7, adding a certain amount of P(VDF-TrFE) nanoparticles into DMF and magnetically stirring to prepare a P(VDF-TrFE) electrospinning solution, wherein the amount of P(VDF-TrFE) nanoparticles added is 0.1 g to 3 g, and the amount of DMF added is 2 ml to 18 ml. Further, the amount of P(VDF-TrFE) nanoparticles added is preferably 1 g, and the amount of DMF added is preferably 8 ml;
[0080] Step S8, adding a certain amount of BTO@PDA nanoflower powder to the P(VDF-TrFE) electrospinning solution and stirring evenly, using an electrospinning machine to prepare a composite nanofiber membrane, the inter-electrode voltage of the electrospinning machine is 15 kV, the distance between the positive and negative electrodes is 10 cm, the injection speed is 0.3 ml / h, and the injection depth is 1 ml.
[0081] like Figure 5 As shown, the scanning electron microscopy results indicate that the nanofibers of the prepared composite nanofibrous membrane are neatly arranged and have a good longitudinal distribution state.
[0082] like Figure 6 As shown, the results of transmission electron microscopy showed that the BTO@PDA nanoflower fillers after mechanical reinforcement and surface modification were well wrapped in the fibers.
[0083] Example 3
[0084] Composite piezoelectric nanomaterials are prepared using nanoflowers@polymer composite nanofillers. Different nanoflower structures are used, such as titanium dioxide nanoflowers, gold nanoflowers, etc., and surface modifications are achieved using polymers, such as PDA (p-phenylenediamine), etc. The mechanically enhanced and surface-modified nanofillers are composited with flexible piezoelectric polymers to enhance the piezoelectric effect.
[0085] like Figure 7 As shown in the COMSOL multi-physics simulation results, the stress distribution inside the matrix of the nanosphere structure is relatively scattered, and the high-energy areas at the upper and lower ends of the sphere are not concentrated. Figure 8 As shown, the petal structure of the nanoflower can achieve stress concentration inside the matrix, and the high-energy area is concentrated at the top of the thorn-shaped petals. Compared with nanospheres, it can better enhance the output effect of the piezoelectric device.
[0086] Example 4
[0087] Flexible piezoelectric devices were prepared using nanoflower@polymer / P(VDF-TrFE) composite nanofiber membrane, and the voltage output was tested under applied pressure.
[0088] Aluminum foil was applied as electrodes on the upper and lower surfaces of the composite nanofiber membrane, and a flexible piezoelectric device was prepared after encapsulation. The sensor output voltage was tested under different vertical forces. When different forces were applied to the sensor surface, the composite nanofiber membrane would be deformed to different degrees, thus generating voltage values of different amplitudes. By detecting the generated voltage, the output of the flexible piezoelectric device was collected.
[0089] like Fig. 9 As shown, the prepared flexible piezoelectric device can achieve a piezoelectric voltage output of up to 90V under the action of mechanical reinforcement and surface modified fillers, which achieves a very excellent improvement effect compared with Chinese patent CN201911342594.3.
[0090] In summary, the preparation method of the composite nanofiber membrane and the preparation method thereof, and the flexible piezoelectric device provided in this embodiment have at least the following beneficial technical effects:
[0091] (1) Composite nanofiber membranes were prepared by combining mechanically enhanced and surface-modified fillers with piezoelectric polymers, and then flexible piezoelectric devices were prepared. This surface modification and mechanical enhancement method for fillers significantly enhanced the output of flexible piezoelectric devices.
[0092] (2) The present invention improves the availability of flexible piezoelectric devices, saves costs, and fills the market gap in improving the structure of piezoelectric fillers and enhancing surface effects, and has important application value.
[0093] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite nanofiber membrane, characterized in that: It includes the following steps: Step S1, dissolving tetrabutyl titanate in an alcohol solvent to obtain a tetrabutyl titanate solution; Step S2, sterilizing the tetrabutyl titanate solution at high temperature, washing and drying to obtain titanium-containing powder; Step S3, calcining the titanium-containing powder at high temperature, washing and drying to obtain flower-shaped anatase titanium dioxide powder; Step S4, mixing the flower-shaped anatase titanium dioxide powder and barium hydroxide into deionized water, stirring evenly with a magnetic stirrer, and then performing ultrasonic treatment to obtain a titanium-containing mixed solution; Step S5, calcining the titanium-containing mixed solution at high temperature to obtain barium titanate nanoflower powder; Step S6, mixing the barium titanate nanoflower powder and dopamine hydrochloride powder, adding Tris-HCl to dissolve, performing magnetic stirring, and centrifuging and washing to obtain BTO@PDA nanoflower powder; Step S7, adding P(VDF-TrFE) nanoparticles into DMF, and preparing P(VDF-TrFE) electrospinning solution after magnetic stirring; Step S8, adding the BTO@PDA nanoflower powder to the P(VDF-TrFE) electrospinning solution, stirring evenly, and using electrospinning technology to prepare a composite nanofiber membrane.
2. The method for preparing the composite nanofiber membrane according to claim 1, characterized in that: The alcohol solvent is a mixed solvent of any one of ethanol, deionized water, methanol, isopropanol and glycerol.
3. The method for preparing the composite nanofiber membrane according to claim 2, characterized in that: The alcohol solvent is a mixed solvent of ethanol and glycerol, the added amount of the ethanol is 10ml-50ml, the added amount of the glycerol is 5ml-15ml, and the added amount of the tetrabutyl titanate is 1g-3g.
4. The method for preparing the composite nanofiber membrane according to claim 1, characterized in that: In step S2, the tetrabutyl titanate solution is sterilized at high temperature, washed and then dried to obtain a titanium-containing powder, and the tetrabutyl titanate solution is heated in an autoclave, wherein the heating temperature is 180° C., the heating time is 24 hours, the filling factor of the autoclave is 0.4, the washing centrifuge speed is 5000 rpm, and the washing times are 5 times.
5. The method for preparing the composite nanofiber membrane according to claim 1, characterized in that: In step S3, the titanium-containing powder is calcined at high temperature, washed and then dried to obtain a flower-shaped anatase titanium dioxide powder, and the titanium-containing powder is calcined at high temperature in an autoclave, wherein the high-temperature calcination temperature is 450° C., the calcination time is 3 hours, the washing centrifugal speed is 5000 rpm, and the washing times are 5 times.
6. The method for preparing the composite nanofiber membrane according to claim 1, characterized in that: Step S4: adding the flower-shaped anatase titanium dioxide powder and barium hydroxide to deionized water, stirring evenly by magnetic stirring, and then performing ultrasonic treatment to obtain a titanium-containing mixed solution, wherein the amount of the flower-shaped anatase titanium dioxide powder added is 0.1g to 0.2g, the amount of the barium hydroxide added is 0.5g to 0.7g, the amount of the deionized water added is 40ml, the magnetic stirring frequency is 500 times / minute, and the stirring time is 1 hour.
7. The method for preparing the composite nanofiber membrane according to claim 1, characterized in that: The concentration of the barium titanate nanoflower powder in the prepared dissolving solution is 10 g / L, and the concentration of the dopamine hydrochloride is 0.1 mol / L.
8. The method for preparing the composite nanofiber membrane according to claim 1, characterized in that: The added amount of the P(VDF-TrFE) nanoparticles is 0.1 g to 3 g, and the added amount of the DMF is 2 ml to 18 ml.
9. A composite nanofiber membrane, characterized in that: The method is prepared according to any one of claims 1 to 8.
10. A flexible piezoelectric device, characterized in that: It comprises the composite nanofiber membrane as claimed in claim 9, wherein aluminum-platinum electrodes are respectively arranged on the upper and lower sides of the composite nanofiber membrane, and a flexible piezoelectric device is obtained after packaging.
Citation Information
Patent Citations
Method for preparing anatase-shaped nano TiO2
CN101671052A
Preparation method of high-dispersion titanium dioxide nanopowder
CN102515268A
Method for treating nano composite film through near-infrared light and application
CN118078994A
Perovskite polymer composite nanofiber as well as preparation method and application thereof
CN118166442A
Nano-barium titanate microcrystal and preparation method therefor, and barium titanate powder and preparation method therefor
WO2020215536A1
Cited By
Preparation method of flexible P (VDF-TrFE) / BaTiO3 piezoelectric composite film with layer-by-layer interlocking structure
CN119768028A
Composite fiber membrane based on sea urchin-shaped pollen carbon, preparation method and application
CN120797314A