ScPLA / PHBV binary blend fiber membrane for air filtration and preparation method and application of scPLA / PHBV binary blend fiber membrane
Through the preparation of scPLA/PHBV two-member blended fiber membranes, the problems of poor stability and insufficient antibacterial properties of PLLA fiber membranes are solved, and efficient air filtration performance and simplified process are achieved, which is suitable for industrial production.
Patent Information
- Application Number
- CN202411245016.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-29
AI Technical Summary
The PLLA fiber membranes of the existing air-filter fiber membranes have poor stability and insufficient antibacterial properties, and the existing processes are complex and costly.
Using the preparation method of scPLA/PHBV two-member blended fiber membrane, electrospinning is prepared by blending levo polylactic acid, dextropolylactic acid and polyhydroxybutyrate valeric acid copolyester, dissolved in a mixed solvent, and electrospinning is carried out. A fiber membrane for air filtration with excellent toughness, antibacteriality and stability was obtained.
It realizes high antibacteriality, stability and toughness of fiber membranes, while simplifying the process and reducing costs, making it suitable for industrial production.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of antibacterial fiber membranes, and in particular relates to a scPLA / PHBV binary blended fiber membrane for air filtration and a preparation method and application thereof. Background Art
[0002] At present, most of the synthetic fiber raw materials used on a large scale come from petroleum, but petroleum resources are limited and face the problem of resource depletion caused by over-exploitation. In addition, the large-scale use of petroleum resources has sharply increased the emission of carbon dioxide gas, bringing about the environmental problem of global warming. Therefore, bio-based polymer materials have attracted more and more attention due to their outstanding characteristics such as independent dependence on petroleum, good biocompatibility, and biodegradability. Vigorously developing renewable and environmentally friendly biodegradable polymer materials is an inevitable trend of development. In particular, biomass-based polymer materials based on renewable biomass resources such as starch, straw, and bagasse have been rapidly developed due to their good biodegradability and abundant and easy-to-obtain raw materials. Compared with traditional polymer materials, biomass-based polymer materials not only reduce the consumption of petrochemical resources, but also consume carbon dioxide and water during the photosynthesis experienced in the production process, reducing the release of carbon dioxide. Therefore, it is of great significance to select degradable polymer materials as raw materials to prepare environmentally friendly antibacterial materials.
[0003] Polylactic acid (PLA) is a completely degradable, environmentally friendly aliphatic polyester polymer material with excellent biodegradability, biocompatibility and absorbency, and can be used to prepare fiber membranes for air filtration. Due to the different lactides during synthesis, PLA can be divided into left-handed polylactic acid (PLLA), right-handed polylactic acid (PDLA) and meso-polylactic acid (PDLLA). Existing fiber membranes for air filtration are mainly made of PLLA. PLLA fiber membranes have poor heat resistance and are easily hydrolyzed, so they are not stable enough to meet the use requirements of air filtration fiber membranes. In addition, existing air filtration fiber membranes have high requirements for antibacterial properties, and pure PLLA fiber membranes are not antibacterial enough.
[0004] A fully biodegradable antibacterial PLA / PBAT film is disclosed in Chinese patent CN112679928A, which selects two biodegradable PLA and PBAT as the matrix blown film, and is modified by a composite antibacterial agent, a coupling agent and a lubricant to give it good mechanical properties such as antibacterial property, heat resistance and wear resistance. The process uses a variety of modifiers, and the preparation technology is complicated. A production process of polyhydroxybutyrate valeric acid copolyester (PHBV) and PLA blended bio-based fiber is disclosed in Chinese patent CN115012050A, PHBV and PLA are blended and melted, and the spinneret of the spinning box is sprayed out and then cooled to obtain nascent fibers, and PHBV and PLA blended bio-based fibers are obtained after drafting and winding. Adopting melt blending technology, rigidity and toughness are improved, but its heat resistance is poor. Because the process is low-temperature spinning, the temperature needs to be accurately controlled, too high will aggravate decomposition, too low will cause excessive viscosity, and normal spinning cannot be performed, so the process is complicated. Summary of the invention
[0005] In view of the problems of poor stability and insufficient antibacterial property of PLLA fiber membrane, the present invention provides a scPLA / PHBV binary blend fiber membrane for air filtration and a preparation method and application thereof. The scPLA / PHBV binary blend fiber membrane has excellent toughness, antibacterial property and stability, and has a simple process and low cost, which is conducive to industrialization.
[0006] To achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In a first aspect of the present invention, a method for preparing a scPLA / PHBV binary blended fiber membrane for air filtration is provided, the preparation method comprising the following steps:
[0008] S1. blending L-polylactic acid, D-polylactic acid and polyhydroxybutyrate-valeric acid copolyester to obtain a blend;
[0009] S2. The blend is dissolved in a mixed solvent and stirred until uniformly mixed to obtain a scPLA / PHBV spinning solution;
[0010] S3. The spinning solution is subjected to electrostatic spinning and dried to obtain the scPLA / PHBV binary blend fiber membrane for air filtration.
[0011] In some embodiments, in the blend, the mass ratio of L-polylactic acid to D-polylactic acid is 1:1.
[0012] In some embodiments, the mass ratio of L-polylactic acid to polyhydroxybutyrate-valeric acid copolyester is (1-3):1.
[0013] By adjusting the mass ratio of the total amount of L-polylactic acid and D-polylactic acid to the mass ratio of polyhydroxybutyrate-valeric acid copolyester, the degradation cycle of the obtained scPLA / PHBV binary blend fiber membrane for air filtration can be controlled.
[0014] In some embodiments, the mixed solvent is a mixed solvent of chloroform (CHL) and hexafluoroisopropanol (HF IP), and in the mixed solvent, the mass ratio of chloroform to hexafluoroisopropanol is (7-9): (3-1).
[0015] In some embodiments, in step S2, the stirring time is more than 30 minutes.
[0016] In some embodiments, the content of the blend in the spinning solution is 5-15 wt %.
[0017] In some embodiments, the electrospinning conditions are: spinning voltage of 15-20 kV, injection rate of 1 ml / h, spinning distance of 20 cm, and rotation speed of 80 r / min.
[0018] In some embodiments, the drying is performed by placing the mixture in an oven at 60°C.
[0019] In the second aspect of the present invention, there is also provided a scPLA / PHBV binary blended fiber membrane for air filtration prepared according to the above-mentioned preparation method.
[0020] In some embodiments, the above-mentioned scPLA / PHBV binary blend fiber membrane for air filtration is characterized in that the scPLA / PHBV binary blend fiber membrane has a thickness of 30-40 μm, a melting temperature of 200-230°C, an antibacterial rate of 90-99%, and a natural degradation period of 120-150 days.
[0021] In the third aspect of the present invention, there is also provided an application of the above-mentioned scPLA / PHBV binary blended fiber membrane for air filtration in air filtration materials.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) In the present invention, PLLA, PDLA and PHBV are blended into a spinning solution for electrospinning. Equal amounts of PLLA and PDLA form a stereocomplexed structure of stereopolylactic acid (scPLA) to improve its stability. PHBV improves the antibacterial property while improving the toughness of the sc-PLA fiber membrane. The obtained scPLA / PHBV binary blended fiber membrane can maintain a certain biodegradation rate and has excellent antibacterial properties, stability, toughness and other properties.
[0024] (2) The technical solution provided by the present invention can achieve controllability of the degradation cycle by changing the blending ratio of scPLA and PHBV. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] (1) Weigh corresponding amounts of PLLA, PDLA, and PHBV and blend them in a blending ratio of 1:1:1.
[0028] (2) A mixed solvent was prepared with CHL and HF IP in a blending ratio of 7:3.
[0029] (3) The blend obtained in step (1) is dissolved in a mixed solvent at a mass fraction of 5 wt %, and mixed evenly by a magnetic stirrer to obtain a scPLA / PHBV spinning solution.
[0030] (4) The spinning solution obtained in step (3) was injected into a syringe, and a membrane was obtained by electrospinning under the conditions of a spinning voltage of 15 kV, an injection rate of 1 ml / h, a spinning distance of 20 cm, and a rotation speed of 80 r / min.
[0031] (5) The membrane obtained in step (4) was placed in an oven at 60°C for drying to obtain a scPLA / PHBV binary blend fiber membrane. The obtained scPLA / PHBV binary blend fiber membrane had a thickness of 30 μm, a melting temperature of 200°C, an elongation at break of 90%, an antibacterial rate of 99%, a filtration efficiency of 99%, a filtration efficiency of 96% after 6 months, and a natural degradation period of 120 days.
[0032] Example 2
[0033] (1) Weigh corresponding amounts of PLLA, PDLA, and PHBV and blend them in a blending ratio of 1:1:1.
[0034] (2) A mixed solvent was prepared with CHL and HF IP in a blending ratio of 8:2.
[0035] (3) The blend obtained in step (1) is dissolved in a mixed solvent at a mass fraction of 8 wt %, and mixed evenly by a magnetic stirrer to obtain a scPLA / PHBV spinning solution.
[0036] (4) The spinning solution obtained in step (3) was injected into a syringe, and a membrane was obtained by electrospinning under the conditions of a spinning voltage of 15 kV, an injection rate of 1 ml / h, a spinning distance of 20 cm, and a rotation speed of 80 r / min.
[0037] (5) The membrane obtained in step (4) was placed in an oven at 60° C. for drying to obtain a scPLA / PHBV binary blend fiber membrane. The obtained scPLA / PHBV binary blend fiber membrane had a thickness of 32 μm, a melting temperature of 200° C., an elongation at break of 88%, an antibacterial rate of 99%, a filtration efficiency of 98%, a filtration efficiency of 95% after 6 months, and a natural degradation period of 128 days.
[0038] Example 3
[0039] (1) Weigh corresponding amounts of PLLA, PDLA, and PHBV and blend them in a blending ratio of 2:2:1.
[0040] (2) A mixed solvent was prepared with CHL and HF IP in a blending ratio of 8:2.
[0041] (3) The blend obtained in step (1) is dissolved in a mixed solvent at a mass fraction of 12 wt %, and mixed evenly by a magnetic stirrer to obtain a scPLA / PHBV spinning solution.
[0042] (4) The spinning solution obtained in step (3) was injected into a syringe, and a membrane was obtained by electrospinning under the conditions of a spinning voltage of 18 kV, an injection rate of 1 ml / h, a spinning distance of 20 cm, and a rotation speed of 80 r / min.
[0043] (5) The membrane obtained in step (4) was placed in an oven at 60° C. for drying to obtain a scPLA / PHBV binary blend fiber membrane. The obtained scPLA / PHBV binary blend fiber membrane had a thickness of 35 μm, a melting temperature of 215° C., an elongation at break of 81%, an antibacterial rate of 95%, a filtration efficiency of 96%, a filtration efficiency of 93% after 6 months, and a natural degradation period of 142 days.
[0044] Example 4
[0045] (1) Weigh corresponding amounts of PLLA, PDLA, and PHBV and blend them in a blending ratio of 2:2:1.
[0046] (2) A mixed solvent was prepared with CHL and HF IP in a blending ratio of 9:1.
[0047] (3) The blend obtained in step (1) is dissolved in a mixed solvent at a mass fraction of 10 wt %, and mixed evenly by a magnetic stirrer to obtain a scPLA / PHBV spinning solution.
[0048] (4) The spinning solution obtained in step (3) was injected into a syringe, and a membrane was obtained by electrospinning under the conditions of a spinning voltage of 18 kV, an injection rate of 1 ml / h, a spinning distance of 20 cm, and a rotation speed of 80 r / min.
[0049] (5) The membrane obtained in step (4) was placed in an oven at 60° C. for drying to obtain a scPLA / PHBV binary blend fiber membrane. The obtained scPLA / PHBV binary blend fiber membrane had a thickness of 38 μm, a melting temperature of 215° C., an elongation at break of 83%, an antibacterial rate of 95%, a filtration efficiency of 96%, a filtration efficiency of 94% after 6 months, and a natural degradation period of 138 days.
[0050] Example 5
[0051] (1) Weigh corresponding amounts of PLLA, PDLA, and PHBV and blend them in a blending ratio of 3:3:1.
[0052] (2) A mixed solvent was prepared with CHL and HF IP in a blending ratio of 8:2.
[0053] (3) The blend obtained in step (1) is dissolved in a mixed solvent at a mass fraction of 15 wt %, and mixed evenly by a magnetic stirrer to obtain a scPLA / PHBV spinning solution.
[0054] (4) The spinning solution obtained in step (3) was injected into a syringe, and a membrane was obtained by electrospinning under the conditions of a spinning voltage of 20 kV, an injection rate of 1 ml / h, a spinning distance of 20 cm, and a rotation speed of 80 r / min.
[0055] (5) The membrane obtained in step (4) was placed in an oven at 60° C. for drying to obtain a scPLA / PHBV binary blend fiber membrane. The obtained scPLA / PHBV binary blend fiber membrane had a thickness of 40 μm, a melting temperature of 230° C., an elongation at break of 60%, an antibacterial rate of 90%, a filtration efficiency of 95%, a filtration efficiency of 91% after 6 months, and a natural degradation period of 150 days.
[0056] Comparative Example 1
[0057] (1) Weigh corresponding amounts of PLLA and PHBV and blend them at a blending ratio of 1:1.
[0058] (2) A mixed solvent was prepared with CHL and HF IP in a blending ratio of 5:5.
[0059] (3) dissolving the blend obtained in step (1) in a mixed solvent at a mass fraction of 20 wt %, and mixing evenly with a magnetic stirrer to obtain a PLLA / PHBV spinning solution.
[0060] (4) The spinning solution obtained in step (3) was injected into a syringe, and a membrane was obtained by electrospinning under the conditions of a spinning voltage of 20 kV, an injection rate of 1 ml / h, a spinning distance of 20 cm, and a rotation speed of 80 r / min.
[0061] (5) The film obtained in step (4) was placed in an oven at 60° C. for drying to obtain a PLLA / PHBV binary blend fiber membrane. The obtained PLLA / PHBV binary blend fiber membrane had a thickness of 28 μm, a melting temperature of 150° C., an elongation at break of 85%, an antibacterial rate of 95%, a filtration efficiency of 92%, a filtration efficiency of 52% after 6 months, and a natural degradation period of 115 days.
[0062] Comparative Example 2
[0063] (1) Weigh corresponding amounts of PLLA and PDLA and blend them in a blending ratio of 1:1.
[0064] (2) A mixed solvent was prepared with CHL and HF IP in a blending ratio of 5:5.
[0065] (3) dissolving the blend obtained in step (1) in a mixed solvent at a mass fraction of 5 wt %, and mixing evenly with a magnetic stirrer to obtain a scPLA spinning solution.
[0066] (4) The spinning solution obtained in step (3) was injected into a syringe, and a membrane was obtained by electrospinning under the conditions of a spinning voltage of 20 kV, an injection rate of 1 ml / h, a spinning distance of 20 cm, and a rotation speed of 80 r / min.
[0067] (5) The membrane obtained in step (4) was placed in an oven at 60° C. for drying to obtain a scPLA fiber membrane. The obtained scPLA fiber membrane had a thickness of 50 μm, a melting temperature of 220° C., an elongation at break of 24%, an antibacterial rate of 40%, a filtration efficiency of 84%, a filtration efficiency of 83% after 6 months, and a natural degradation period of 180 days.
Claims
1. A method for preparing a scPLA / PHBV binary blend fiber membrane for air filtration, characterized in that: The preparation method comprises the following steps: S1. blending L-polylactic acid, D-polylactic acid and polyhydroxybutyrate-valeric acid copolyester to obtain a blend; S2. The blend is dissolved in a mixed solvent and stirred until uniformly mixed to obtain a scPLA / PHBV spinning solution; S3. The spinning solution is subjected to electrostatic spinning and dried to obtain the scPLA / PHBV binary blended fiber membrane for air filtration.
2. The preparation method according to claim 1, characterized in that: In the blend, the mass ratio of L-polylactic acid to D-polylactic acid is 1:
1.
3. The preparation method according to claim 2, characterized in that: The mass ratio of L-polylactic acid to polyhydroxybutyrate-valeric acid copolyester is (1-3):
1.
4. The preparation method according to claim 1, characterized in that: The mixed solvent is a mixed solvent of chloroform and hexafluoroisopropanol, and the mass ratio of chloroform to hexafluoroisopropanol in the mixed solvent is (7-9):(3-1).
5. The preparation method according to claim 1, characterized in that: In the spinning solution, the content of the blend is 5-15wt%.
6. The preparation method according to claim 1, characterized in that: The conditions of the electrospinning are: spinning voltage of 15-20 kV, injection rate of 1 ml / h, spinning distance of 20 cm, and rotation speed of 80 r / min.
7. The preparation method according to claim 1, characterized in that: The drying step is to place the mixture in an oven at 60°C for drying.
8. The scPLA / PHBV binary blend fiber membrane for air filtration prepared according to the preparation method according to any one of claims 1 to 7.
9. A scPLA / PHBV two-component blended fiber membrane for air filtration as claimed in claim 8, characterized in that: The scPLA / PHBV two-component blended fiber membrane has a thickness of 30-40 μm, a melting temperature of 200-230° C., a bacteriostatic rate of 90-99%, and a natural degradation period of 120-150 days.
10. Use of the scPLA / PHBV binary blended fiber membrane for air filtration according to claim 8 in air filtration materials.
Citation Information
Patent Citations
Full-biodegradable antibacterial PLA / PBAT film and preparation method thereof
CN112679928A
Production process of PHBV and PLA blended bio-based fiber
CN115012050A
Preparation method of fibroin / microorganism-based polymer solution and preparation method of composite nanofiber thereof
CN111041603A
High-porosity self-powered stereocomplex polylactic acid fiber filter membrane and preparation method thereof
CN116712874A
Solvent-resistant hydrophilic stereocomplex polylactic acid oil-water separation membrane and preparation method thereof