Photosensitive resin composition, photosensitive element, and method for producing wiring substrate

By using coumarin-based sensitizer and 3-functional monomer in the photosensitive resin composition, the problem of insufficient pattern shape and adhesion in the polymer film of the DBA photosensitive resin composition is solved, and high precision is achieved. Resist pattern with excellent adhesion and good pattern shape is suitable for wiring substrate manufacturing.

CN119045281APending Publication Date: 2024-11-29RESONAC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411391930.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2020-02-18
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the production of wiring substrates, it is difficult to form a resist pattern with high precision, excellent adhesion and good pattern shape in the photosensitive resin composition containing DBA, and there is a problem of permeation in the polymer film, especially in the polymer film.

Method used

The photosensitive resin composition including a binder polymer, a three-functional monomer photopolymerizable compound, a photopolymerization initiator and a coumarin-based sensitizer are used, and the coumarin-based sensitizer and a three-functional monomer are used. Combination, improves the adhesion and pattern shape of the resist pattern and reduces the amount of sensitizer used.

Benefits of technology

Excellent adhesion to the substrate and good pattern shape are achieved, the resolution and photocurable of the resist pattern are improved, the solvent amount and the absorption of the exposure light source are reduced, and the deep photocuring ability of the resin layer is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119045281A_ABST
    Figure CN119045281A_ABST
Patent Text Reader

Abstract

The invention relates to a photosensitive element and a method for manufacturing a wiring substrate. A photosensitive resin composition for a photosensitive element according to the present invention contains a binder polymer, a photopolymerizable compound containing a trifunctional monomer, a photopolymerization initiator, and a coumarin-based sensitizer.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of Chinese application No. 202080016031.X, whose application date is February 18, 2020 and whose invention name is “Photosensitive resin composition, photosensitive element and method for manufacturing wiring substrate”. Technical Field

[0002] The present invention relates to a photosensitive resin composition, a photosensitive element and a method for producing a wiring substrate. Background Art

[0003] In the manufacture of wiring boards, a resist pattern is formed to obtain the desired wiring. Photosensitive resin compositions are widely used in the formation of resist patterns. In recent years, MSAP (Modified SemiAdditive Process) has attracted attention as a method for forming fine wiring. In this method, in order to form fine wiring, it is necessary to form a resist pattern with higher precision than before.

[0004] In order to form a resist pattern with high precision, a photosensitizer is generally added to a photosensitive resin composition. As the photosensitizer, for example, anthracene derivatives such as 9,10-dibutoxyanthracene (DBA) are known (for example, refer to Patent Document 1).

[0005] Previous technical literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2007 / 004619 Summary of the invention

[0008] Technical issues to be solved by the invention

[0009] However, in order to obtain a more precise resist pattern, there is still room for improvement in the photosensitive resin composition containing DBA. In addition, the photosensitive resin composition is usually used in the form of a photosensitive element sandwiched between polymer films such as polyethylene. However, according to the research of the present inventors, when the photosensitive resin composition contains DBA, DBA permeates the polymer film, which may cause the problem that the desired pattern shape cannot be formed when the resist pattern is formed. This problem occurs particularly significantly when the polymer film is a polyethylene film.

[0010] Furthermore, the photosensitive resin composition containing DBA still has room for improvement in forming a resist pattern having excellent adhesion to a substrate.

[0011] Therefore, an object of the present invention is to provide a photosensitive resin composition and a photosensitive element capable of forming a resist pattern having excellent adhesion to a substrate and a good pattern shape, and a method for producing a wiring board using the same.

[0012] Means for solving technical problems

[0013] To achieve the above object, the present invention provides a photosensitive resin composition comprising a binder polymer, a photopolymerizable compound including a trifunctional monomer, a photopolymerization initiator, and a coumarin-based sensitizer.

[0014] According to the above-mentioned photosensitive resin composition, by using in combination 3 functional monomers and coumarin-based sensitizers as photopolymerizable compounds, it is possible to form a resist pattern having excellent adhesion to a substrate and having a good pattern shape. It can be considered that this is because coumarin-based sensitizers are more difficult to penetrate polymer films than DBA and can obtain higher sensitivity with less addition, so the pattern shape of the resist pattern can be made good, and by using this coumarin-based sensitizer and 3 functional monomers, the adhesion of the resist pattern to the substrate can be greatly improved. And, since the coumarin-based sensitizer can reduce the addition, it is also possible to reduce the amount of solvent for dissolving the sensitizer. And then, since the absorbance of the coumarin-based sensitizer is lower than DBA, when forming a resist pattern, the light exposed easily reaches the deep part of the photosensitive resin layer, and the photocurability at the bottom of the photosensitive resin layer can be improved. Therefore, adhesion, resolution and pattern shape can be further improved.

[0015] In the photosensitive resin composition, the coumarin-based sensitizer may include a compound represented by the following general formula (1).

[0016]

[0017] In the formula, Z 1 and Z 2 Each independently represents a halogen atom, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an amino group, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 20 carbon atoms, a mercapto group, an alkylmercapto group having 1 to 10 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 20 carbon atoms, a carboxyl group, a carboxyalkyl group having 1 to 10 carbon atoms in an alkyl group, an acyl group having 1 to 10 carbon atoms in an alkyl group, an alkoxy group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 1 to 20 carbon atoms, or a group containing a heterocyclic ring, and n represents an integer of 0 to 4, and m represents an integer of 0 to 2. In addition, n Z 1 and m Z 2 At least two of them may form a ring.

[0018] By using the compound represented by the above general formula (1) as a photosensitizer, the adhesiveness and pattern shape of the resist pattern can be improved.

[0019] In the photosensitive resin composition, the content of the coumarin sensitizer may be 0.01 to 0.5 parts by mass relative to 100 parts by mass of the total amount of the binder polymer and the photopolymerizable compound. Since the content of the coumarin sensitizer is within the above range, the excellent adhesion of the resist pattern and the good pattern shape can be achieved at a higher level.

[0020] In the photosensitive resin composition, the binder polymer may include a polymer containing a hydroxyalkyl (meth)acrylate unit. Since the binder polymer includes the hydroxyalkyl (meth)acrylate unit, both excellent adhesion of the resist pattern and a good pattern shape can be achieved at a higher level.

[0021] The photosensitive resin composition may further contain a polymerization inhibitor. Furthermore, the content of the polymerization inhibitor in the photosensitive resin composition may be 0.003 parts by mass or less relative to 100 parts by mass of the total amount of the binder polymer and the photopolymerizable compound. Since the content of the polymerization inhibitor is within the above range, the pattern shape of the resist pattern can be made better.

[0022] The present invention also provides a photosensitive element comprising: a support; and a photosensitive resin layer formed on the support using the photosensitive resin composition of the present invention.

[0023] The present invention also provides a method for manufacturing a wiring substrate, which comprises: a process of providing a photosensitive resin layer on a substrate using the above-mentioned photosensitive resin composition of the present invention or the above-mentioned photosensitive element of the present invention; a process of photocuring a portion of the above-mentioned photosensitive resin layer; a process of removing the uncured portion of the above-mentioned photosensitive resin layer to form a resist pattern; and a process of forming a wiring layer on the portion of the above-mentioned substrate where the above-mentioned resist pattern is not formed.

[0024] Effects of the Invention

[0025] According to the present invention, there can be provided a photosensitive resin composition and a photosensitive element capable of forming a resist pattern having excellent adhesion to a substrate and a good pattern shape, and a method for producing a wiring board using the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic cross-sectional view showing a photosensitive element according to one embodiment.

[0027] Figure 2It is a schematic diagram showing a method for manufacturing a wiring board according to one embodiment.

[0028] Figure 3 This is an electron microscope photograph of a resist pattern formed using the photosensitive resin composition of Example 1.

[0029] Figure 4 This is an electron microscope photograph of a resist pattern formed using the photosensitive resin composition of Comparative Example 1. DETAILED DESCRIPTION

[0030] Hereinafter, embodiments of the present invention will be described in detail.

[0031] In this specification, the term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the intended effect of the process is achieved. The numerical range represented by "to" means a range that includes the numerical values ​​recorded before and after "to" as the minimum and maximum values, respectively. Regarding the term "layer", when viewed in a top view, in addition to structures of shapes formed on the entire surface, structures of shapes formed on a part of the surface are also included. "(Meth)acrylic acid" refers to at least one of "acrylic acid" and its corresponding "methacrylic acid". The same applies to other similar expressions such as (meth)acrylates.

[0032] In this specification, "(poly)oxyethylene" refers to oxyethylene or a polyoxyethylene formed by two or more ethylene groups linked by an ether bond. "(Poly)oxypropylene" refers to a polyoxypropylene formed by an oxypropylene or two or more propylene groups linked by an ether bond. "EO modified" refers to a compound having (poly)oxyethylene. "PO modified" refers to a compound having (poly)oxypropylene. "EO / PO modified" refers to a compound having (poly)oxyethylene and / or (poly)oxypropylene.

[0033] In this specification, when there are multiple substances corresponding to each component in the composition, the amount of each component in the composition refers to the total amount of the multiple substances in the composition unless otherwise specified. In this specification, "solid content" refers to non-volatile components other than volatile substances (water, solvent, etc.) in the photosensitive resin composition. That is, "solid content" refers to components other than the solvent that does not volatilize and remains during the drying of the photosensitive resin composition described later, and also includes components that are liquid, maltose-like or waxy at room temperature (25°C).

[0034] <Photosensitive resin composition>

[0035] The photosensitive resin composition of the present embodiment contains (A) component: binder polymer, (B) component: photopolymerizable compound, (C) component: photopolymerization initiator and (D) component: coumarin-based sensitizer. Here, (B) component contains trifunctional monomers. In addition, the photosensitive resin composition of the present embodiment may also contain (E) component: polymerization inhibitor. The following describes each component.

[0036] (A) Component: Binder polymer

[0037] The photosensitive resin composition comprises one or more (A) components. Examples of (A) components include acrylic resins, styrene resins, epoxy resins, amide resins, amide epoxy resins, alkyd resins, and phenolic resins. From the perspective of further improving alkali developability, (A) component may include an acrylic resin.

[0038] The acrylic resin has a structural unit derived from, for example, (meth)acrylic acid, and may also have a structural unit derived from other monomers other than (meth)acrylic acid. The other monomers may be one or more.

[0039] The other monomers may be, for example, (meth)acrylates. Examples of (meth)acrylates include alkyl (meth)acrylates, cycloalkyl (meth)acrylates, and aryl (meth)acrylates.

[0040] From the viewpoint of improving alkali developability and stripping properties, the other monomer is preferably an alkyl (meth)acrylate. The alkyl group of the alkyl (meth)acrylate may be, for example, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, or a structural isomer thereof, and from the viewpoint of further improving stripping properties, may be an alkyl group having 1 to 4 carbon atoms.

[0041] When the other monomer is an alkyl (meth)acrylate, the content of the alkyl (meth)acrylate may be 1% by mass or more, 2% by mass or more, or 3% by mass or more from the viewpoint of excellent release properties, and may be 80% by mass or less, 60% by mass or less, or 50% by mass or less from the viewpoint of further improving resolution and adhesion, based on the total amount of monomers constituting the component (A).

[0042] From the viewpoint of further improving the resolution and adhesion, the other monomers may be styrene or styrene derivatives. For example, styrene derivatives may be vinyl toluene, α-methyl styrene, etc. When the other monomers are styrene or styrene derivatives, the content of styrene or styrene derivatives is based on the total amount of monomers constituting component (A). From the viewpoint of further improving the resolution, it may be 5% by mass or more, 10% by mass or more, or 20% by mass or more, and from the viewpoint of excellent peeling properties, it may be 65% by mass or less, 55% by mass or less, or 50% by mass or less.

[0043] From the viewpoint of further improving the developability, adhesion and stripping properties, the other monomers may be hydroxyalkyl (meth)acrylates. For example, hydroxyalkyl (meth)acrylates may be hydroxymethyl (meth)acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc. When the other monomers are hydroxyalkyl (meth)acrylates, the content of hydroxyalkyl (meth)acrylates is based on the total amount of monomers constituting component (A). From the viewpoint of further improving the developability and stripping properties, the content may be 2% by mass or more, 4% by mass or more, or 6% by mass or more, and from the viewpoint of maintaining high sensitivity, the content may be 14% by mass or less, 12% by mass or less, or 10% by mass or less.

[0044] From the viewpoint of being able to develop appropriately, the acid value of component (A) may be 100 mgKOH / g or more, 120 mgKOH / g or more, 140 mgKOH / g or more, or 150 mgKOH / g or more, and from the viewpoint of improving the adhesion (developer resistance) of the cured product of the photosensitive resin composition, it may be 250 mgKOH / g or less, 240 mgKOH / g or less, or 230 mgKOH / g or less. The acid value of component (A) can be adjusted by the content of the structural unit constituting component (for example, the structural unit derived from (meth)acrylic acid).

[0045] The weight average molecular weight (Mw) of the component (A) may be 10,000 or more, 20,000 or more, or 25,000 or more from the viewpoint of excellent adhesion (developer resistance) of the cured product of the photosensitive resin composition, and may be 100,000 or less, 80,000 or less, or 60,000 or less from the viewpoint of proper development. The degree of dispersion (Mw / Mn) of the component (A) may be, for example, 1.0 or more or 1.5 or more, and may be 3.0 or less or 2.5 or less from the viewpoint of further improving adhesion and resolution.

[0046] Weight average molecular weight and dispersity can be measured by gel permeation chromatography (GPC) and using the calibration curve of standard polystyrene, for example. More specifically, it is possible to measure under the conditions described in the embodiments. In addition, for compounds with low molecular weight, when it is difficult to measure by the measuring method of the above-mentioned weight average molecular weight, it is also possible to measure the molecular weight by other methods, and calculate its average value.

[0047] The content of component (A) may be 20% by mass or more, 30% by mass or more, or 40% by mass or more, based on the total solid content of the photosensitive resin composition, from the viewpoint of excellent film formability, and may be 90% by mass or less, 80% by mass or less, or 65% by mass or less, from the viewpoint of better sensitivity and resolution.

[0048] The content of component (A) relative to 100 parts by mass of the total amount of component (A) and component (B) may be 30 parts by mass or more, 35 parts by mass or more, or 40 parts by mass or more from the viewpoint of excellent film formability, and may be 70 parts by mass or less, 65 parts by mass or less, or 60 parts by mass or less from the viewpoint of further improving sensitivity and resolution.

[0049] (B) Component: Photopolymerizable compound

[0050] The photosensitive resin composition comprises one or more (B) components. The (B) component may be a compound polymerized by light, for example, a compound having an ethylenically unsaturated bond. From the viewpoint of improving adhesion, pattern shape, and developability, the (B) component comprises a trifunctional monomer.

[0051] Examples of the trifunctional monomer include trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, EO / PO-modified trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate. From the perspective of further improving the peelability, adhesion, and flexibility, the trifunctional monomer is preferably EO-modified, PO-modified, or EO / PO-modified.

[0052] The content of the trifunctional monomer can be 5% by mass or more or 10% by mass or more, based on the total amount of component (B), from the viewpoint of further improving developability, adhesion, and pattern shape, and can be 30% by mass or less or 25% by mass or less, from the viewpoint of further improving releasability.

[0053] From the viewpoint of further improving alkali developability, resolution, and release characteristics after curing, the component (B) may contain a bisphenol A-type (meth)acrylate compound.

[0054] Examples of bisphenol A type (meth)acrylate compounds include 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane (2,2-bis(4-((meth)acryloxypentaethoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolypropoxy)phenyl)propane, 2,2-bis(4-((meth)acryloxypolybutoxy)phenyl)propane, and 2,2-bis(4-((meth)acryloxypolyethoxypolypropoxy)phenyl)propane. From the viewpoint of further improving resolution and release properties, component (B) may include 2,2-bis(4-((meth)acryloxypolyethoxy)phenyl)propane (2,2-bis(4-((meth)acryloxypentaethoxy)phenyl)propane, etc.

[0055] From the viewpoint of further improving the resolution of the resist, the content of the bisphenol A (meth)acrylate compound may be 20% by mass or more, or 40% by mass or more, or 95% by mass or less, 90% by mass or less, or 80% by mass or less, based on the total amount of the component (B).

[0056] From the viewpoint of further appropriately improving the resolution and flexibility, the component (B) may also contain an α,β-unsaturated ester compound obtained by reacting a polyol with an α,β-unsaturated carboxylic acid other than the above-mentioned trifunctional monomer. Examples of the α,β-unsaturated ester compound include polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polyalkylene glycol di(meth)acrylate such as EO-modified polypropylene glycol, trimethylolpropane di(meth)acrylate, and tetramethylolmethane tetra(meth)acrylate.

[0057] The content of the α,β-unsaturated ester compound can be 20% by mass or more or 30% by mass or more based on the total amount of component (B) from the viewpoint of improving flexibility, and can be 70% by mass or less or 60% by mass from the viewpoint of further improving resolution.

[0058] From the viewpoint of further improving the stripping property and developing property, the component (B) may also contain a (meth)acrylate compound having a carbamate bond. As the (meth)acrylate compound having a carbamate bond, for example, a (meth)acrylic monomer having an OH group at the β position and a diisocyanate compound such as isophorone diisocyanate, 2,6-toluene diisocyanate, 2,4-toluene diisocyanate, 1,6-hexamethylene diisocyanate, a reaction product, tris ((meth)acryloyloxytetraethylene glycol isocyanate) hexamethylene isocyanurate, EO modified carbamate di(meth)acrylate, PO modified carbamate di(meth)acrylate, EO and PO modified carbamate di(meth)acrylate, carbamate (meth)acrylate containing a carboxyl group, etc. can be cited. In addition, as the (meth)acrylate compound having a carbamate bond, it is also preferred to use a carbamate oligomer.

[0059] From the viewpoints of applicability, operability, curing shrinkage after curing, surface curing, hardness, elongation and other physical properties in a liquid state, the weight average molecular weight of the (meth) acrylate compound having a carbamate bond is preferably 800 or more, more preferably 2000 or more, and further preferably 4000 or more. And, from the same viewpoint, the weight average molecular weight of the (meth) acrylate compound having a carbamate bond is preferably 10000 or less, more preferably 9000 or less, and further preferably 7000 or less. The weight average molecular weight is measured by gel permeation chromatography (GPC), and the value converted to standard polystyrene is used.

[0060] The content of the (meth)acrylate compound having a urethane bond may be 2% by mass or more or 4% by mass or more from the viewpoint of further improving the releasability and developability, and may be 10% by mass or less or 8% by mass or less from the viewpoint of further improving the fluidity, based on the total amount of the component (B).

[0061] The photosensitive resin composition may contain, as the component (B), a photopolymerizable compound other than the trifunctional monomer, the bisphenol A-based (meth)acrylate compound, the α,β-unsaturated ester compound, and the (meth)acrylate compound having a urethane bond.

[0062] As other photopolymerizable compounds, nonylphenoxy polyethyleneoxy acrylate, phthalic acid compounds, (meth) alkyl acrylates, photopolymerizable compounds having at least one cationically polymerizable cyclic ether group in the molecule (oxetane compounds, etc.), etc. From the viewpoint of further appropriately improving the resolution, adhesion, resist shape, and post-curing peeling characteristics, the other photopolymerizable compound may be at least one selected from the group consisting of nonylphenoxy polyethyleneoxy acrylate and phthalic acid compounds.

[0063] Examples of the nonylphenoxy polyethyleneoxy acrylate include nonylphenoxy trivinyloxy acrylate, nonylphenoxy tetravinyloxy acrylate, nonylphenoxy pentavinyloxy acrylate, nonylphenoxy hexavinyloxy acrylate, nonylphenoxy heptavinyloxy acrylate, nonylphenoxy octavinyloxy acrylate, nonylphenoxy nonavinyloxy acrylate, nonylphenoxy decavinyloxy acrylate, and nonylphenoxy undecvinyloxy acrylate.

[0064] Phthalic acid compounds include, for example, γ-chloro-β-hydroxypropyl-β'-(meth)acryloyloxyethyl-phthalate (also known as 3-chloro-2-hydroxypropyl-2-(meth)acryloyloxyethyl-phthalate), β-hydroxyethyl-β'-(meth)acryloyloxyethyl-phthalate, β-hydroxypropyl-β'-(meth)acryloyloxyethyl-phthalate, and the like, preferably γ-chloro-β-hydroxypropyl-β'-(meth)acryloyloxyethyl-phthalate.

[0065] When component (B) contains other photopolymerizable compounds, from the viewpoint of further appropriately improving the resolution, adhesion, resist shape and post-curing peeling characteristics, the content of other photopolymerizable compounds can be 1% by mass or more, 3% by mass or more, or 5% by mass or less, or 30% by mass or less, 25% by mass or less, or 20% by mass or less, based on the total amount of component (B).

[0066] From the viewpoint of further improving the sensitivity and resolution, the content of component (B) can be 3% by mass or more, 10% by mass or more, or 25% by mass or more, based on the total solid content of the photosensitive resin composition. From the viewpoint of excellent film formability, the content can be 70% by mass or less, 60% by mass or less, or 50% by mass or less.

[0067] Component (C): Photopolymerization initiator

[0068] The photosensitive resin composition contains one or more (C) components. Examples of (C) components include hexaarylbiimidazole compounds; benzophenone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholino)phenyl]-1-butanone, 4-(2-hydroxyethoxy)phenyl-2-(hydroxy-2-propyl)ketone, 2-methyl-1-[4-(methylthio)phenyl] -2-morpholine-propane-1 and other aromatic ketones; quinones such as alkyl anthraquinone; benzoin ether compounds such as benzoin alkyl ether; benzoin compounds such as benzoin and alkyl benzoin; benzyl derivatives such as benzyl dimethyl ketal; bis(2,4,6-trimethylbenzoyl)-phenyl phosphine oxide; bis(2,6-dimethylbenzoyl)-2,4,4-trimethyl-pentyl phosphine oxide; (2,4,6-trimethylbenzoyl)ethoxyphenyl phosphine oxide, etc.

[0069] From the viewpoint of further suppressing the penetration of the photosensitizer into the polyethylene film, the component (C) may contain a hexaarylbiimidazole compound. The aryl group in the hexaarylbiimidazole compound may be a phenyl group, etc. The hydrogen atom bonded to the aryl group in the hexaarylbiimidazole compound may be substituted with a halogen atom (chlorine atom, etc.).

[0070] The hexaaryl biimidazole compound may be a 2,4,5-triaryl imidazole dimer. As 2,4,5-triaryl imidazole dimers, for example, 2-(o-chlorophenyl)-4,5-diphenyl imidazole dimer, 2-(o-chlorophenyl)-4,5-bis-(q-methoxyphenyl) imidazole dimer and 2-(p-methoxyphenyl)-4,5-diphenyl imidazole dimer may be cited. From the viewpoint of being able to further inhibit the penetration of the photosensitizer into the polyethylene film, the hexaaryl biimidazole compound is preferably a 2-(o-chlorophenyl)-4,5-diphenyl imidazole dimer, and more preferably 2,2-bis(o-chlorophenyl)-4,5-4',5'-tetraphenyl-1,2'biimidazole.

[0071] From the viewpoint of further suppressing the penetration of the photosensitizer into the polyethylene film, the content of the hexaarylbiimidazole compound may be 90 mass % or more, 95 mass % or more, or 99 mass % or more based on the total amount of the component (C). The component (C) may consist only of the hexaarylbiimidazole compound.

[0072] From the viewpoint of further improving sensitivity and adhesion, the content of the component (C) may be 0.1% by mass or more, 0.5% by mass or more, or 1% by mass or less, and may be 20% by mass or less, 10% by mass or less, or 5% by mass or less, based on the total solid content of the photosensitive resin composition.

[0073] (D) Ingredient: Coumarin-based sensitizer

[0074] The photosensitive resin composition contains one or more components (D). The component (D) serves as a photosensitizer. Examples of the component (D) include compounds represented by the following general formula (1).

[0075]

[0076] In the formula, Z 1 and Z 2 Each independently represents a halogen atom, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an amino group, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 20 carbon atoms, a mercapto group, an alkylmercapto group having 1 to 10 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 20 carbon atoms, a carboxyl group, a carboxyalkyl group having 1 to 10 carbon atoms in an alkyl group, an acyl group having 1 to 10 carbon atoms in an alkyl group, an alkoxy group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 1 to 20 carbon atoms, or a group containing a heterocyclic ring, and n represents an integer of 0 to 4, and m represents an integer of 0 to 2. In addition, n Z 1 and m Z 2 At least two of them may form a ring.

[0077] In the general formula (1), at least one Z 1 Preferably substituted at position 7, at least one Z 2 Preferably, the 4-position is substituted. Also, from the viewpoint of sensitivity, the 3-position is preferably unsubstituted.

[0078] Examples of the halogen atom in the general formula (1) include fluorine, chlorine, bromine, iodine, and astatine. Examples of the alkyl group having 1 to 20 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, isopentyl, neopentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, and structural isomers thereof. Examples of the cycloalkyl group having 3 to 10 carbon atoms include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, and cyclooctyl. Examples of the aryl group having 6 to 14 carbon atoms include phenyl, tolyl, xylyl, biphenyl, naphthyl, anthracenyl, and phenanthryl. These may be substituted with a halogen atom, an amino group, a nitro group, a cyano group, a mercapto group, an allyl group, or an alkyl group having 1 to 20 carbon atoms. Examples of the alkylamino group having 1 to 10 carbon atoms include methylamino, ethylamino, propylamino, and isopropylamino. Examples of the dialkylamino group having 2 to 20 carbon atoms include dimethylamino, diethylamino, dipropylamino, and diisopropylamino. Examples of the alkylmercapto group having 1 to 10 carbon atoms include methylmercapto, ethylmercapto, and propylmercapto. Examples of the hydroxyalkyl group having 1 to 20 carbon atoms include hydroxymethyl, hydroxyethyl, hydroxypropyl, hydroxyisopropyl, and hydroxybutyl. Examples of the carboxyalkyl group having 1 to 10 carbon atoms as the alkyl group include carboxymethyl, carboxyethyl, carboxypropyl, and carboxybutyl. In addition, examples of the acyl group having 1 to 10 carbon atoms in the alkyl group include formyl, acetyl, propionyl, butyryl, isobutyryl, valeryl, isovaleryl, pivaloyl, etc., and examples of the alkoxy group having 1 to 20 carbon atoms include methoxy, ethoxy, propoxy, butoxy, etc. In addition, examples of the alkoxycarbonyl group having 1 to 20 carbon atoms include methoxycarbonyl, ethoxycarbonyl, propoxycarbonyl, butoxycarbonyl, etc., and examples of the group containing a heterocyclic ring include furyl, thienyl, pyrrolyl, thiazolyl, indolyl, quinolyl, etc.

[0079] In the general formula (1), Z 1 and Z 2 Each of the Z groups independently is preferably an alkyl group having 1 to 20 carbon atoms, an amino group, an alkylamino group having 1 to 10 carbon atoms, or a dialkylamino group having 2 to 20 carbon atoms. 1 and m Z 2 At least two of them may form a ring.

[0080] From the viewpoint of resolution and photosensitivity, the coumarin compound represented by the general formula (1) is more preferably a compound represented by the following general formula (2). 1 , Z 2and m and the above Z 1 , Z 2 and m have the same meaning, Z 11 and Z 12 Each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, and r represents an integer of 0 to 3. 1 , m Z 2 , Z 11 and Z 12 At least two of them may form a ring. In the compound represented by the following general formula (2), Z 11 and Z 12 Each of them is independently preferably an alkyl group having 1 to 10 carbon atoms, and more preferably an alkyl group having 1 to 6 carbon atoms. 1 and Z 2 Same as above.

[0081]

[0082] As a compound represented by the general formula (2) and m Z 2 , Z 11 and Z 12 In the embodiment where at least two of the compounds form a ring, there can be mentioned compounds represented by the following general formula (3) and compounds represented by the following general formula (4).

[0083]

[0084] In the formula, Z 1 , Z 11 , Z 12 and r and the above Z 1 , Z 11 , Z 12 and r have the same meaning, Z 21 Indicates that the above Z 1 The same atom or group. Also, s represents an integer of 0 to 8. In addition, Z is preferably 1 , Z 11 and Z 12 Same as above.

[0085]

[0086] In the formula, Z 1 , Z 2 and m and the above Z 1 , Z 2 and m have the same meaning, Z 31 and Z 32 Respectively independently represent the above Z 1The same atom or group. In addition, t represents an integer of 0 to 1, u represents an integer of 0 to 6, and v represents an integer of 0 to 6. In addition, Z is preferably 1 and Z 2 Same as above.

[0087] Examples of the compound represented by the general formula (2) (including compounds represented by the general formulae (3) and (4)) include 7-amino-4-methylcoumarin, 7-dimethylamino-4-methylcoumarin, 7-diethylamino-4-methylcoumarin (a compound represented by the following formula (5)), 7-methylamino-4-methylcoumarin, 7-ethylamino-4-methylcoumarin, 4,6-dimethyl-7-ethylaminocoumarin (a compound represented by the following formula (6)), 4,6-diethyl-7-ethylaminocoumarin, 4,6-dimethyl-7-diethylaminocoumarin, 4,6-dimethyl-7-dimethylaminocoumarin, 4,6-diethyl-7-diethylaminocoumarin, 4,6-diethyl -7-dimethylaminocoumarin, 4,6-dimethyl-7-ethylaminocoumarin, 7-dimethylaminocyclopentane[c]coumarin (a compound represented by the following formula (7)), 7-aminocyclopentane[c]coumarin, 7-diethylaminocyclopentane[c]coumarin, 2,3,6,7,10,11-hexahydrate-1H,5H-cyclopenta[3,4][1]benzopyrano[6,7,8-ij]quinolizin-12(9H)-one, 7-diethylamino-5',7'-dimethoxy-3,3'-carbonylbiscoumarin, 3,3'-carbonylbis[7-(diethylamino)coumarin], 7-(diethylamino)-3-(2-thienyl)coumarin, and a compound represented by the following formula (8).

[0088]

[0089] As the coumarin compound represented by the general formula (1), the compound represented by the general formula (4) is particularly preferred. By using the compound represented by the general formula (4) as the component (D) in combination with the trifunctional monomer as the component (B), the sensitivity, adhesion and resolution can be greatly improved, and even if only a small amount of the component (D) is added, this effect can be fully obtained.

[0090] From the viewpoint of further improving sensitivity, adhesion and resolution, the content of component (D) is, for example, 0.01 part by mass or more, preferably 0.02 part by mass or more, more preferably 0.03 part by mass or more, and further preferably 0.04 part by mass or more, relative to 100 parts by mass of the total amount of component (A) and component (B). From the viewpoint of making the resist pattern shape better, the content is, for example, 0.5 part by mass or less, preferably 0.4 part by mass or less, more preferably 0.3 part by mass or less, further preferably 0.2 part by mass or less, and particularly preferably 0.15 part by mass or less.

[0091] The photosensitive resin composition may contain a known photosensitizer as another photosensitizer in addition to the component (D). The content of the other sensitizer may be, for example, 0.01 to 0.50 parts by mass or 0.05 to 0.20 parts by mass relative to 100 parts by mass of the total amount of the components (A) and (B).

[0092] (E) Component: Polymerization Inhibitor

[0093] From the viewpoint of suppressing polymerization in the unexposed portion during resist pattern formation and further improving the resolution, the photosensitive resin composition may further contain component (E): a polymerization inhibitor. Examples of the polymerization inhibitor include tert-butylcatechol and 4-hydroxy-2,2,6,6-tetramethylpiperidin-N-oxyl.

[0094] Since the photosensitive resin composition contains component (D), even if it does not contain a polymerization inhibitor, it is possible to suppress polymerization in the unexposed portion during the formation of the resist pattern, and the resist pattern can be formed with higher precision, compared to the case of containing an existing photosensitizer (e.g., DBA). Thus, the content of component (E) can be 0.01 parts by mass or less, 0.005 parts by mass or less, 0.003 parts by mass or less, 0.0025 parts by mass or less relative to 100 parts by mass of the total amount of components (A) and (B), and the photosensitive resin composition may not contain component (E). The content of component (E) can be 0.001 parts by mass or more relative to 100 parts by mass of the total amount of components (A) and (B).

[0095] The photosensitive resin composition may also contain one or more other ingredients other than the above-mentioned ingredients. As other ingredients, hydrogen donors (bis[4-(dimethylamino)phenyl]methane, bis[4-(diethylamino)phenyl]methane, colorless crystal violet, N-phenylglycine, etc.), dyes (malachite green, etc.), tribromophenyl sulfone, photochromic agents, thermal color inhibitors, plasticizers (p-toluenesulfonamide, etc.), pigments, fillers, defoamers, flame retardants, stabilizers, adhesion imparting agents, leveling agents, peeling accelerators, antioxidants, fragrances, imaging agents, thermal crosslinking agents, etc. can be listed. The content of other ingredients can be 0.005 mass parts or more or 0.01 mass parts or less, or 20 mass parts or less relative to the total amount of 100 mass parts of (A) component and (B) component.

[0096] From the viewpoint of adjusting viscosity, the photosensitive resin composition may also contain one or more organic solvents. As organic solvents, for example, methanol, ethanol, acetone, methyl ethyl ketone, methyl cellosolve, ethyl cellosolve, toluene, N,N-dimethylformamide, propylene glycol monomethyl ether, etc. may be cited. The content of the organic solvent may be more than 40% by mass or less than 70% by mass based on the total amount of the photosensitive resin composition. As organic solvents, for example, a mixed solvent of toluene and other solvents (methanol, ethanol, methyl cellosolve, ethyl cellosolve, etc.) may be used. In the case where the photosensitive resin composition includes a coumarin-based sensitizer, even if the proportion of toluene in the above-mentioned mixed solvent is reduced, good solubility is easily obtained, so the amount of toluene used can be reduced.

[0097] The photosensitive resin composition can be suitably used for formation of a resist pattern, and can be particularly suitably used for a method for producing a wiring board to be described later.

[0098] <Photosensitive element>

[0099] Figure 1 is a schematic cross-sectional view of a photosensitive element according to one embodiment. Figure 1 As shown, the photosensitive element 1 includes a support 2 , a photosensitive resin layer 3 provided on the support 2 , and a protective layer 4 provided on the side of the photosensitive resin layer 3 opposite to the support 2 .

[0100] The support 2 and the protective layer 4 may be polymer films having heat resistance and solvent resistance, for example, polyester films such as polyethylene terephthalate films, polyolefin films such as polyethylene films and polypropylene films, etc. The support 2 and the protective layer 4 may be films of hydrocarbon polymers other than polyolefins. The film of hydrocarbon polymers including polyolefins may be low-density, for example, it may have a density of 1.014 g / cm or less. The support 2 and the protective layer 4 may be stretched films formed by stretching the low-density hydrocarbon polymer film. The type of the polymer film constituting the protective layer 4 may be the same as or different from the type of the polymer film constituting the support 2.

[0101] These polymer films are commercially available as polyethylene terephthalate films such as PS series (e.g., PS-25) manufactured by Teijin Limited, polyethylene films such as NF-15 manufactured by TAMAPOLY CO., LTD., or polypropylene films such as OJI PAPER CO., LTD. (e.g., ALPHAN MA-410, E-200C) and SHIN-ETSU FILM CO., LTD.

[0102] From the viewpoint of suppressing damage to the support 2 when peeling the support 2 from the photosensitive resin layer 3, the thickness of the support 2 may be greater than 1 μm or greater than 5 μm, and from the viewpoint of enabling appropriate exposure when exposure is performed through the support 2, the thickness may be less than 100 μm, less than 50 μm, or less than 30 μm.

[0103] When the photosensitive resin layer 3 and the support body 2 are laminated on the substrate while peeling off the protective layer 4, the thickness of the protective layer 4 can be greater than 1 μm, greater than 5 μm or greater than 15 μm from the viewpoint of suppressing damage to the protective layer 4, and can be less than 100 μm, less than 50 μm or less than 30 μm from the viewpoint of improving productivity.

[0104] The photosensitive resin layer 3 is composed of the above-mentioned photosensitive resin composition. From the viewpoint of facilitating coating and improving productivity, the thickness of the photosensitive resin layer 3 after drying (after volatilizing the organic solvent when the photosensitive resin composition contains an organic solvent) can be 1 μm or more or 5 μm or more, and from the viewpoint of further improving adhesion and resolution, it can be 100 μm or less, 50 μm or less, or 40 μm or less.

[0105] The photosensitive element 1 can be obtained, for example, as follows. First, a photosensitive resin layer 3 is formed on a support 2. The photosensitive resin layer 3 can be formed, for example, by coating a photosensitive resin composition containing an organic solvent to form a coating layer and drying the coating layer. Next, a protective layer 4 is formed on the surface of the photosensitive resin layer 3 on the opposite side of the support 2.

[0106] The coating layer is formed by a known method such as roll coating, comma coating, gravure coating, air knife coating, die coating, rod coating, etc. The coating layer is dried so that the amount of the organic solvent remaining in the photosensitive resin layer 3 is, for example, 2% by mass or less, specifically, for example, at 70 to 150° C. for about 5 to 30 minutes.

[0107] In another embodiment, the photosensitive element may not include the protective layer, and may include other layers such as a buffer layer, an adhesive layer, a light absorbing layer, and a gas barrier layer.

[0108] The photosensitive element 1 may be in the form of a sheet, or may be in the form of a photosensitive element roll wound on a core in a roll shape. In the photosensitive element roll, the photosensitive element 1 is preferably wound so that the support 2 is on the outside. The core is formed of, for example, polyethylene, polypropylene, polystyrene, polyvinyl chloride, acrylonitrile-butadiene-styrene copolymer, etc. From the viewpoint of end face protection, an end face separator may be provided on the end face of the photosensitive element roll, and from the viewpoint of edge fusion resistance, a moisture-proof end face separator may be provided. The photosensitive element 1 may be packaged with, for example, a black sheet material with low moisture permeability.

[0109] The photosensitive element 1 can be applied to the formation of a resist pattern, and can be particularly applied to the method for manufacturing a wiring substrate described later. Compared with the conventional photosensitive element, the photosensitive element 1 can suppress the penetration of the photosensitizer into the polyethylene film, so at least one of the support 2 and the protective layer 4 can be a polyethylene film, or can be the above-mentioned low-density hydrocarbon polymer film or its stretched film.

[0110] <Method for Manufacturing Wiring Board>

[0111] Figure 2 Schematic diagram showing a method for manufacturing a wiring board (also called a printed wiring board) according to an embodiment of the present invention. In the manufacturing method, first, Figure 2 As shown in (a), a substrate (for example, a circuit-forming substrate) is prepared that has an insulating layer 11 and a conductive layer 12 formed on the insulating layer 11. The conductive layer 12 may be, for example, a metal copper layer.

[0112] Then, if Figure 2As shown in (b), a photosensitive resin layer 13 is provided on the substrate (conductive layer 12). In this process, the photosensitive resin composition or the photosensitive element 1 is used to form a photosensitive resin layer 13 composed of the photosensitive resin composition on the substrate (conductive layer 12). For example, the photosensitive resin layer 13 is formed by applying the photosensitive resin composition on the substrate and drying it. Alternatively, the photosensitive resin layer 13 is formed by removing the protective layer 4 from the photosensitive element 1 and then pressing the photosensitive resin layer 3 of the photosensitive element 1 onto the substrate while heating it. When pressing, at least one of the photosensitive resin layer 3 and the substrate can be heated at 70 to 130° C., for example. The pressure during pressing can be 0.1 to 1.0 MPa, for example.

[0113] Then, if Figure 2 As shown in (c), a mask 14 is arranged on the photosensitive resin layer 13, and an active light 15 is irradiated to expose the region other than the region where the mask 14 is arranged to photo-cure the photosensitive resin layer 13. The light source of the active light 15 can be, for example, an ultraviolet light source or a visible light source such as a carbon arc lamp, a mercury vapor arc lamp, a high-pressure mercury lamp, a xenon lamp, a gas laser (argon laser, etc.), a solid-state laser (YAG laser, etc.), or a semiconductor laser.

[0114] In another embodiment, the active light 15 may be irradiated in a desired pattern by a direct writing exposure method such as an LDI exposure method or a DLP exposure method without using the mask 14 , thereby exposing a portion of the photosensitive resin layer 13 .

[0115] Then, if Figure 2 As shown in (d), the region (uncured portion) other than the photocured portion formed by exposure is removed from the substrate by development, thereby forming a resist pattern 16 composed of the photocured portion (cured product of the photosensitive resin layer). The development method may be, for example, wet development or dry development, preferably wet development.

[0116] Wet development is performed using a developer corresponding to the photosensitive resin composition by methods such as dipping, paddle, spray, brushing, slapping, scraping, shaking and dipping. The developer is appropriately selected according to the structure of the photosensitive resin composition and may be an alkali developer or an organic solvent developer.

[0117] The alkaline developer can be an aqueous solution of an alkali such as a hydroxide of lithium, sodium or potassium; an alkali carbonate such as a carbonate or bicarbonate of lithium, sodium, potassium or ammonium; an alkali metal phosphate such as potassium phosphate and sodium phosphate; an alkali metal pyrophosphate such as sodium pyrophosphate and potassium pyrophosphate; borax; sodium metasilicate; tetramethylammonium hydroxide; ethanolamine; ethylenediamine; diethylenetriamine; 2-amino-2-hydroxymethyl-1,3-propanediol; 1,3-diamino-2-propanol; or morpholine.

[0118] The alkali developer may be, for example, a 0.1-5 mass % sodium carbonate aqueous solution, a 0.1-5 mass % potassium carbonate aqueous solution, a 0.1-5 mass % sodium hydroxide aqueous solution, a 0.1-5 mass % sodium tetraborate aqueous solution, etc. The pH of the alkali developer may be, for example, 9-11.

[0119] The alkaline developer may further contain a surfactant, a defoamer, an organic solvent, etc. Examples of the organic solvent include acetone, ethyl acetate, an alkoxyethanol having an alkoxy group having 1 to 4 carbon atoms, ethanol, isopropanol, butanol, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether. The content of the organic solvent may be 2 to 90% by mass based on the total amount of the alkaline developer.

[0120] The organic solvent developer may contain an organic solvent such as 1,1,1-trichloroethane, N-methylpyrrolidone, N,N-dimethylformamide, cyclohexanone, methyl isobutyl ketone, and γ-butyrolactone. The organic solvent developer may further contain 1 to 20% by mass of water.

[0121] In this step, after removing the unexposed portion, heating at 60 to 250° C. or 0.2 to 10 J / cm 2 The resist pattern 16 is further cured by exposure.

[0122] Then, if Figure 2 As shown in FIG. 5 , a wiring layer 17 is formed by performing a plating process, for example, on a portion of the conductor layer 12 where the resist pattern 16 is not formed. The wiring layer 17 may be formed of the same material as the conductor layer 12, or may be formed of a different material. The wiring layer 17 may be, for example, a metal copper layer. The plating process may be one or both of an electroplating process and an electroless plating process.

[0123] Then, if Figure 2 As shown in (f), the resist pattern 16 is removed, and the conductor layer 12 provided at a position corresponding to the resist pattern 16 is removed. Thus, a wiring board 18 having a wiring layer 17 formed on the board can be obtained.

[0124] The resist pattern 16 can be removed by developing by dipping, spraying, or the like using a strong alkaline aqueous solution, for example, a 1-10 mass % sodium hydroxide aqueous solution, a 1-10 mass % potassium hydroxide aqueous solution, or the like.

[0125] The conductor layer 12 can be removed by etching. The etching solution is appropriately selected according to the type of the conductor layer 12, and may be, for example, a cupric chloride solution, a ferric chloride solution, an alkali etching solution, a hydrogen peroxide etching solution, or the like.

[0126] Example

[0127] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0128] <Synthesis of component (A)>

[0129] The monomers shown in Table 1 were mixed with 0.9 parts by mass of azobisisobutyronitrile in the amounts shown in Table 1 (unit: parts by mass) to prepare a solution (a). 0.6 parts by mass of azobisisobutyronitrile was dissolved in 50 parts by mass of a mixed solution (x) of 30 parts by mass of methyl cellosolve and 20 parts by mass of toluene to prepare a solution (b). After 500 g of the mixed solution (x) was put into a flask equipped with a stirrer, a reflux cooler, a thermometer, a dropping funnel and a nitrogen inlet tube, nitrogen was blown into the flask while stirring, and the temperature was raised to 80°C. After the above solution (a) was added dropwise to the above mixed solution in the flask at a constant dropping speed for 4 hours, it was stirred at 80°C for 2 hours. Then, after the above solution (b) was added dropwise to the solution in the flask at a constant dropping speed for 10 minutes, the solution in the flask was stirred at 80°C for 3 hours. Furthermore, the solution in the flask was heated to 95°C over 30 minutes, and after being kept at 95°C for 2 hours, stirring was stopped and cooled to room temperature (25°C) to obtain solutions of binder polymers A-1 to A-3. The non-volatile component (solid content) of the solutions of binder polymers A-1 to A-3 was 49.0% by mass. The weight average molecular weight (Mw), glass transition temperature (Tg) and acid value of binder polymers A-1 to A-3 are shown in Table 1.

[0130] The weight average molecular weight is measured by gel permeation chromatography (GPC) and derived by conversion using a calibration curve of standard polystyrene. The conditions of GPC are as follows.

[0131] (GPC conditions)

[0132] Pump: Hitachi L-6000 (manufactured by Hitachi, Ltd., trade name)

[0133] Pipeline: 3 pipes in total

[0134] Gelpack GL-R420

[0135] Gelpack GL-R430

[0136] Gelpack GL-R440 (the above are product names made by Showa Denko Materials Co., Ltd.)

[0137] Eluent: Tetrahydrofuran

[0138] Measurement temperature: 40℃

[0139] Flow rate: 2.05mL / min

[0140] Detector: Hitachi L-3300 RI (manufactured by Hitachi, Ltd., trade name)

[0141] The glass transition temperature was measured using DSC (DSC-7, manufactured by PerkinElmer Co., Ltd.) under the following conditions: a sample amount of 10 mg, a heating rate of 10° C. / min, and a measurement environment of air.

[0142] The acid value is measured by a neutralization titration method based on JIS K0070. First, a solution of the binder polymer is heated at 130°C for 1 hour to remove volatile components to obtain a solid component. Then, after accurately weighing 1 g of the binder polymer of the solid component, 30 g of acetone is added to the binder polymer to uniformly dissolve it, thereby obtaining a resin solution. Next, an appropriate amount of phenolphthalein as an indicator is added to the resin solution, and a neutralization titration is performed using a 0.1 mol / L potassium hydroxide aqueous solution. Then, the acid value is calculated by the following formula.

[0143] Acid value = 0.1 × V × f1 × 56.1 / (Wp × I / 100)

[0144] In the formula, V represents the titration amount (mL) of the 0.1 mol / L potassium hydroxide aqueous solution used for titration, f1 represents the factor (concentration conversion coefficient) of the 0.1 mol / L potassium hydroxide aqueous solution, Wp represents the measured mass of the resin solution (g), and I represents the measured proportion of the non-volatile component in the above resin solution (mass %).

[0145] [Table 1]

[0146]

[0147] [Examples 1 to 10 and Comparative Examples 1 to 3]

[0148] <Preparation of Photosensitive Resin Composition>

[0149] The photosensitive resin compositions were prepared by mixing the components shown in Tables 2 to 3 in the amounts (parts by mass) shown in Tables 2 to 3. In addition, the amount (parts by mass) of the component (A) shown in Tables 2 to 3 is the mass (solid content) of the non-volatile component. The details of the components shown in Tables 2 to 3 are as follows.

[0150] (B) Ingredients

[0151] FA-321M(70): 70% solution of 2,2-bis(4-(methacryloyloxyethoxy)phenyl)propane (ethylene oxide 10 mol average addition product) in propylene glycol monomethyl ether (manufactured by Showa Denko Materials Co., Ltd.)

[0152] FA-137M: EO-modified trimethylolpropane trimethacrylate (manufactured by Showa Denko Materials Co., Ltd.)

[0153] FA-024M: EO, PO modified dimethacrylate (manufactured by Showa Denko Materials Co., Ltd., number of EO groups: 6 (average value), number of PO groups: 12 (average value)

[0154] UA-13: EO, PO modified urethane dimethacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., number of EO groups: 2 (average value), number of PO groups: 18 (average value))

[0155] (C) Ingredients

[0156] BCIM: 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole (manufactured by Hampford)

[0157] (D) Ingredients

[0158] Coumarin 102: 2,3,6,7-tetrahydro-9-methyl-1H,5H,11H-[1]benzopyrano[6,7,8-ij]quinolizin-11-one (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0159] (D)'Ingredients

[0160] DBA: 9,10-dibutoxyanthracene (manufactured by KAWASAKI KASEI CHEMICALS LTD.)

[0161] (E) Ingredients

[0162] DIC-TBC-20: 4-tert-butylcatechol (manufactured by DIC Corporation)

[0163] (Other ingredients)

[0164] LCV: Colorless crystal violet (manufactured by YAMADA CHEMICAL CO., LTD.)

[0165] SF-808H: A mixture of carboxybenzotriazole, 5-amino-1H-tetrazole, and methoxypropanol (manufactured by SANWA KASEICORP)

[0166] LA-7RD: 4-TEMPO (manufactured by Asahi Denka Kogyo Kabushiki Kaisha)

[0167] MKG: Malachite green (manufactured by OSAKA ORGANIC CHEMICAL INDUSTRY LTD.)

[0168] (Solvent)

[0169] TLS: Toluene

[0170] MAL: Methanol

[0171] ACS: Acetone

[0172] <Production of Photosensitive Element>

[0173] A polyethylene terephthalate film (manufactured by Teijin Limited, trade name "HTF-01") with a thickness of 16 μm was prepared as a support, and a photosensitive resin composition was applied to the support so that the thickness became uniform, and then dried in a hot air convection dryer at 70°C and 110°C in sequence to form a photosensitive resin layer with a thickness of 25 μm after drying. A polyethylene film (manufactured by TAMAPOLY CO., LTD., trade name "NF-15") was laminated on the photosensitive resin layer as a protective layer to obtain a photosensitive element in which a support, a photosensitive resin layer, and a protective layer were laminated in sequence.

[0174] <Production of Laminated Body>

[0175] A glass epoxy material, i.e., a copper-clad laminate (substrate, manufactured by ShowaDenko Materials co., Ltd., trade name "MCL-E-679"), in which copper foil (thickness: 35 μm) was laminated on both sides, was surface treated using a surface roughening treatment liquid "Mech-Etch Bond CZ-8100" (manufactured by MEC COMPANY LTD., trade name). Then, after water washing, acid washing and water washing, it was dried with an air flow. The surface-treated copper-clad laminate was heated to 80°C, and while peeling off the protective layer, the above-mentioned photosensitive elements were laminated respectively so that the photosensitive resin layer was in contact with the copper surface. Thus, a laminated body in which the copper-clad laminate, the photosensitive resin layer and the support were laminated in this order was obtained. The obtained laminated body was used as a test piece in the test shown below. In addition, lamination was performed using a hot roller at 110°C, a crimping pressure of 0.4 MPa and a roller speed of 1.5 m / min.

[0176] <Evaluation>

[0177] (Measurement of absorbance)

[0178] The absorbance of the photosensitive resin layer was measured using a UV spectrophotometer (Hitachi High-Technologies Corporation, spectrophotometer U-3310). The measurement was performed by placing a photosensitive element with the protective layer peeled off on the measurement side, placing a support film on the reference sample side, continuously measuring to a wavelength of 300 to 700 nm in the absorbance mode, and reading the values ​​at a wavelength of 375 nm and a wavelength of 405 nm. The results are shown in Tables 2 and 3.

[0179] (Measurement of minimum development time)

[0180] The above-mentioned laminate was cut into 5 cm squares to obtain a test piece for measuring the minimum development time. After peeling off the support from the test piece, the unexposed photosensitive resin layer was spray-developed at a pressure of 0.15 MPa using a 1 mass % sodium carbonate aqueous solution at 30°C, and the shortest time that can visually confirm the removal of the unexposed portion of more than 1 mm was set as the shortest development time. A full cone was used for the nozzle. The distance between the above-mentioned test piece and the tip of the nozzle was 6 cm, and the center of the test piece was configured to coincide with the center of the nozzle. The shorter the minimum development time (unit: seconds), the better the developability. The results are shown in Tables 2 to 3.

[0181] (Evaluation of Adhesion)

[0182] The photosensitive resin layer of the laminate was exposed (drawn) using a drawing pattern with a line width (L) / space width (S) (hereinafter referred to as "L / S") of 3 / 400 to 30 / 400 (unit: μm) at an energy level of 14 residual steps on a 41-step exposure meter.

[0183] After exposure, the support was peeled off from the laminate to expose the photosensitive resin layer, and a 1 mass % sodium carbonate aqueous solution was sprayed at 30 ° C for 60 seconds to remove the unexposed portion. After development, the minimum value of the line width / space width value in the resist pattern in which the space portion (unexposed portion) was removed without residue and the line portion (exposed portion) was formed without winding and notching was evaluated for adhesion. The smaller the value, the better the adhesion. The results are shown in Tables 2 to 3.

[0184] (Evaluation of Resist Pattern Formability)

[0185] The resist pattern with a line width of 10 μm prepared in the above-mentioned adhesion evaluation was observed with a scanning electron microscope, and the shape of the resist pattern and the presence or absence of line thickening were evaluated. Electron microscope photographs of the resist patterns of Example 1 and Comparative Example 1 are shown in FIG. Figure 3 and Figure 4 The resist pattern shape was evaluated based on the ratio of the top width to the bottom width of the resist pattern (bottom width / top width) according to the following evaluation criteria. The results are shown in Tables 2 and 3.

[0186] A: The cross-sectional shape is a rectangle (the bottom width / top width is greater than 0.9)

[0187] B: The cross-sectional shape is a small tapered shape (the bottom width / top width is greater than 0.8 and less than 0.9)

[0188] C: The cross-sectional shape is a tapered shape (bottom width / top width is less than 0.8)

[0189] In addition, regarding line thickening, the difference between the designed dimension of the line width in the drawing pattern and the line width (top width) of the formed resist pattern was measured and evaluated based on the following evaluation criteria. The results are shown in Tables 2 and 3.

[0190] A: The difference is less than 0.5μm

[0191] B: The difference is greater than 0.5 μm and less than 1.0 μm

[0192] C: The difference is greater than 1.0 μm and less than 2.0 μm

[0193] D: Difference greater than 2.0μm

[0194]

[0195]

[0196] Explanation of symbols

[0197] 1- photosensitive element, 2- support, 3, 13- photosensitive resin layer, 4- protective layer, 11- insulating layer, 12- conductor layer, 14- mask, 15- active light, 16- resist pattern, 17- wiring layer, 18- wiring substrate.

Claims

1. A photosensitive element comprising: a support; and A photosensitive resin layer is formed on the support using a photosensitive resin composition. in, The photosensitive resin composition contains a binder polymer, a photopolymerizable compound including a trifunctional monomer, a photopolymerization initiator, and a coumarin-based sensitizer.

2. The photosensitive element according to claim 1, wherein The coumarin-based sensitizer comprises a compound represented by the following general formula (1): In the formula, Z 1 and Z 2 each independently represents a halogen atom, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an amino group, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 20 carbon atoms, a mercapto group, an alkylmercapto group having 1 to 10 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 20 carbon atoms, a carboxyl group, a carboxyalkyl group having 1 to 10 carbon atoms in an alkyl group, an acyl group having 1 to 10 carbon atoms in an alkyl group, an alkoxy group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 1 to 20 carbon atoms, or a group containing a heterocyclic ring, n represents an integer of 0 to 4, m represents an integer of 0 to 2, and n Z 1 and m Z 2 At least two of them may form a ring.

3. The photosensitive element according to claim 1, wherein The coumarin-based sensitizer comprises a compound represented by the following general formula (2): In the formula, Z 1 and Z 2 each independently represents a halogen atom, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an amino group, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 20 carbon atoms, a mercapto group, an alkylmercapto group having 1 to 10 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 20 carbon atoms, a carboxyl group, a carboxyalkyl group having 1 to 10 carbon atoms in an alkyl group, an acyl group having 1 to 10 carbon atoms in an alkyl group, an alkoxy group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 1 to 20 carbon atoms, or a group containing a heterocyclic ring, and Z 11 and Z 12 each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, m represents an integer of 0 to 2, r represents an integer of 0 to 3, and r Z 1 , m Z 2 , Z 11 and Z 12 At least two of them may form a ring.

4. The photosensitive element according to claim 1, wherein The coumarin-based sensitizer comprises a compound represented by the following general formula (3): In the formula, Z 1 and Z 21 each independently represents a halogen atom, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an amino group, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 20 carbon atoms, a mercapto group, an alkylmercapto group having 1 to 10 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 20 carbon atoms, a carboxyl group, a carboxyalkyl group having 1 to 10 carbon atoms in an alkyl group, an acyl group having 1 to 10 carbon atoms in an alkyl group, an alkoxy group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 1 to 20 carbon atoms, or a group containing a heterocyclic ring, and Z 11 and Z 12 each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms, r represents an integer of 0 to 3, s represents an integer of 0 to 6, and r Z 1 At least two of them may form a ring.

5. The photosensitive element according to claim 1, wherein The coumarin-based sensitizer comprises a compound represented by the following general formula (4): In the formula, Z 1 , Z 2 , Z 31 and Z 32 each independently represents a halogen atom, an alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 14 carbon atoms, an amino group, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 20 carbon atoms, a mercapto group, an alkylmercapto group having 1 to 10 carbon atoms, an allyl group, a hydroxyalkyl group having 1 to 20 carbon atoms, a carboxyl group, a carboxyalkyl group having 1 to 10 carbon atoms in an alkyl group, an acyl group having 1 to 10 carbon atoms in an alkyl group, an alkoxy group having 1 to 20 carbon atoms, an alkoxycarbonyl group having 1 to 20 carbon atoms, or a group containing a heterocyclic ring, m represents an integer of 0 to 2, t represents an integer of 0 to 1, u represents an integer of 0 to 6, and v represents an integer of 0 to 6. When m is 2, the two Z 2 A ring may be formed.

6. The photosensitive element according to any one of claims 1 to 5, wherein The content of the coumarin-based sensitizer in the photosensitive resin composition is 0.01 to 0.5 parts by mass based on 100 parts by mass of the total amount of the binder polymer and the photopolymerizable compound.

7. The photosensitive element according to any one of claims 1 to 5, wherein The content of the coumarin-based sensitizer in the photosensitive resin composition is 0.01 to 0.15 parts by mass based on 100 parts by mass of the total amount of the binder polymer and the photopolymerizable compound.

8. The photosensitive element according to any one of claims 1 to 5, wherein The binder polymer contains a polymer including a hydroxyalkyl (meth)acrylate unit.

9. The photosensitive element according to any one of claims 1 to 5, wherein The binder polymer contains an acrylic resin having a structural unit derived from (meth)acrylic acid and a structural unit derived from a monomer other than (meth)acrylic acid.

10. The photosensitive element according to claim 9, wherein The other monomers include styrene or styrene derivatives.

11. The photosensitive element according to claim 10, wherein The content of the styrene and the styrene derivative is 5 to 65% by mass based on the total amount of monomers constituting the acrylic resin.

12. The photosensitive element according to claim 9, wherein The other monomers include hydroxyalkyl (meth)acrylates.

13. The photosensitive element according to claim 12, wherein The content of the hydroxyalkyl (meth)acrylate is 2 to 14% by mass based on the total amount of monomers constituting the acrylic resin.

14. The photosensitive element according to any one of claims 1 to 5, wherein The trifunctional monomer includes at least one selected from trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, EO / PO-modified trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate.

15. The photosensitive element according to any one of claims 1 to 5, wherein The content of the trifunctional monomer is 5 to 30% by mass based on the total amount of the photopolymerizable compound.

16. The photosensitive element according to any one of claims 1 to 5, wherein The photopolymerizable compound further includes a bisphenol A type (meth)acrylate compound.

17. The photosensitive element according to any one of claims 1 to 5, wherein The photopolymerization initiator consists only of a hexaarylbiimidazole compound.

18. The photosensitive element according to any one of claims 1 to 5, wherein The photosensitive resin composition further contains a polymerization inhibitor.

19. The photosensitive element according to claim 18, wherein The content of the polymerization inhibitor in the photosensitive resin composition is 0.003 parts by mass or less relative to 100 parts by mass of the total amount of the binder polymer and the photopolymerizable compound.

20. A method for manufacturing a wiring substrate, comprising: A step of providing a photosensitive resin layer on a substrate using the photosensitive element according to any one of claims 1 to 19; a step of photocuring a portion of the photosensitive resin layer; a step of removing an uncured portion of the photosensitive resin layer to form a resist pattern; and A step of forming a wiring layer on a portion of the substrate where the resist pattern is not formed.

Citation Information

Patent Citations

  • Photosensitive resin composition, and, photosensitive element, method for forming resist pattern, method for manufacturing printed wiring board and method for manufacturing partition wall for plasma display panel using the composition

    WO2007004619A1