Resistance paste, preparation method thereof and flexible direct current converter valve
By using the resistive slurry prepared by modified glass powder and modified hydroxyethyl cellulose in a flexible DC converter valve, the problem of unstable slurry printing performance is solved, and the high-temperature sintering performance is improved and the film drying is dried Focus on improving the performance requirements of the flexible direct converter valve.
Patent Information
- Application Number
- CN202411270138.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-29
AI Technical Summary
The printing performance of the resistive slurry in the flexible DC converter valve is unstable, resulting in poor sintering performance of the slurry under high temperature conditions, which cannot meet the performance requirements of the slurry of the flexible DC converter valve.
Use silane coupling agent to modify glass powder, conductive phase, and modified hydroxyethyl cellulose as organic carriers to prepare resistive slurry through specific component ratios and treatment methods to ensure good sintering performance under high temperature conditions. Improve the adhesion of drying film.
It significantly improves the printing stability and film forming characteristics of the resistive paste, provides good drying film adhesion and temperature coefficient resistance, meets the performance requirements of the flexible direct converter valve, and reduces the temperature coefficient resistance.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of printing paste, and in particular to a resistor paste and a preparation method thereof, and a flexible DC converter valve. Background Art
[0002] The flexible DC converter valve is the core equipment of the flexible DC transmission project. Its cost accounts for about 22% to 25% of the complete set of converter station equipment. Its components include insulated gate bipolar transistors (IGBTs), control drive units, cooling systems, saturated reactors, capacitors and resistors, etc. Different from the semi-controlled thyristors used in conventional DC transmission projects, the flexible DC converter valve mostly uses fully controlled IGBTs, which can realize the conversion between AC and DC by controlling their on and off.
[0003] At present, the slurry used for the resistor component in the flexible DC converter valve usually has problems such as unstable printing performance. Therefore, it is necessary to improve the traditional resistor slurry for the flexible DC converter valve. Summary of the invention
[0004] Based on this, one or more embodiments of the present application provide a resistor slurry with good drying film adhesion, a preparation method thereof, and a flexible DC converter valve.
[0005] According to a first aspect of an embodiment of the present application, a resistor paste is provided, comprising the following components, by weight: 60 to 75 parts of silane coupling agent modified glass powder, 5 to 15 parts of a conductive phase, 15 to 30 parts of an organic vehicle, 5 to 15 parts of an organic solvent, 0.1 to 0.5 parts of a thixotropic agent, 0.1 to 0.5 parts of a dispersant, and 0.2 to 1 parts of a defoaming agent;
[0006] The organic carrier comprises the following components: 5-15 parts of modified hydroxyethyl cellulose, 1-5 parts of rosin resin, 1-5 parts of egg yolk lecithin, 1-5 parts of butyl carbitol acetate, 70-90 parts of terpineol and 0.1-1 part of glycerol.
[0007] In some embodiments, the silane coupling agent modified glass powder includes at least two types of glass powders, and the softening points and particle sizes of the different types of glass powders are different.
[0008] In some embodiments, the resistor paste satisfies at least one of the following characteristics:
[0009] (1) The particle sizes of the different types of glass powders are independently 0.5 μm to 5 μm;
[0010] (2) The softening points of the different types of the glass powder are independently 400° C. to 750° C.
[0011] In some embodiments, the resistor paste satisfies at least one of the following characteristics:
[0012] (1) The silane coupling agent in the silane coupling agent modified glass powder is selected from one or more of WD-26, WD-31, WD-50, WD-56, WD-42, A150, KMB5220, KBM602, KH550, KH570, KH560 and Z-6032;
[0013] (2) The conductive phase is selected from lead ruthenate;
[0014] (3) The particle size of the conductive phase is 500nm~5μm;
[0015] (4) The organic solvent is selected from one or more of terpineol, glycerol, terpineol, butyl carbitol acetate, butyl carbitol acetate, ethylene glycol ethyl ether acetate, tributyl citrate, dibutyl phthalate and lecithin;
[0016] (5) The thixotropic agent is selected from one or more of BYK607, fumed silica, organic bentonite, castor oil and polyamide wax;
[0017] (6) The dispersant is selected from one or more of Phobe 1000, SP-762, 7043, K-702, 9300, SDJ8006, SRE-47000, AD3013 and BYK111;
[0018] (7) The defoaming agent is selected from BYK A550, CBK-208, EDL-2100 or EDL2800.
[0019] According to a second aspect of an embodiment of the present application, a method for preparing a resistor paste is provided, comprising the following steps:
[0020] Providing silane coupling agent modified glass powder, conductive phase, organic carrier, organic solvent, thixotropic agent, dispersant and defoaming agent according to the components of the resistor paste described in any one of the above items, and mixing the components uniformly to prepare a mixture;
[0021] The mixture is subjected to grinding and dispersion treatment to obtain the resistor paste.
[0022] In some embodiments, the method for preparing the organic carrier comprises the following steps:
[0023] Modified hydroxyethyl cellulose, rosin resin, egg yolk lecithin, butyl carbitol acetate, pinene alcohol and glycerin are provided and stirred uniformly to obtain an organic carrier.
[0024] In some embodiments, the method for preparing the modified hydroxyethyl cellulose comprises the following steps:
[0025] The natural cellulose material is subjected to alkalization treatment, activation treatment, hydroxyethylation treatment, desalination treatment and etherification treatment in sequence to obtain modified hydroxyethyl cellulose.
[0026] In some embodiments, the method for preparing the silane coupling agent modified glass powder comprises the following steps:
[0027] A silane coupling agent, ethanol and at least two glass powders are provided, and the mixture is stirred and mixed to obtain silane coupling agent modified glass powder.
[0028] The method for preparing the resistor paste also includes the following steps: filtering and vacuuming the resistor paste in sequence.
[0029] According to a third aspect of an embodiment of the present application, a flexible DC-DC converter valve is provided, which includes the resistor slurry of the first aspect or the resistor slurry prepared by the preparation method of the second aspect.
[0030] Compared with the traditional technology, this application has the following beneficial effects:
[0031] The resistor paste of the present application selects a specific modified hydroxyethyl cellulose as the raw material of the organic carrier. The hydroxyethyl cellulose has the characteristics of thickening, stabilization, good adhesion and dispersibility, has good solubility in the organic carrier, and can effectively prevent the solvent precipitation and stratification of the resistor paste, thereby effectively improving the thixotropic and film-forming properties of the resistor paste, improving the dispersibility of the solid components in the resistor paste, and enabling the paste to maintain good stability during printing or centrifugal stirring, greatly improving the printing performance of the resistor paste on the substrate, enabling the paste to have stability that can be continuously printed, and providing good drying film adhesion; in this way, the resistor paste of the present application can meet the performance requirements of the resistor component in the flexible DC converter valve for the paste.
[0032] Furthermore, a variety of glass powders with different particle sizes and softening points are selected for compounding, and the glass powders are modified so that the resistor paste can be fully sintered under high temperature conditions, thereby reducing its temperature coefficient resistance. DETAILED DESCRIPTION
[0033] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail. In the following description, many specific details are set forth to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present application, so the present application is not limited by the specific embodiments disclosed below.
[0034] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present application. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the present application, etc. can be purchased from the market or can be prepared by existing methods.
[0035] In the present application, "plurality", "multiple", "multiple times", "multiples", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0036] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0037] In the present application, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1-10, indicating that t is any integer selected from the integer group consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.
[0038] In a first aspect of the present application, a resistor paste is provided, comprising the following raw materials, by weight: 60-75 parts of silane coupling agent modified glass powder, 5-15 parts of conductive phase, 15-30 parts of organic carrier, 5-15 parts of organic solvent, 0.1-0.5 parts of thixotropic agent, 0.1-0.5 parts of dispersant, and 0.2-1 parts of defoaming agent;
[0039] The organic carrier comprises the following raw materials: 5-15 parts of modified hydroxyethyl cellulose, 1-5 parts of rosin resin, 1-5 parts of egg yolk lecithin, 1-5 parts of butyl carbitol acetate, 70-90 parts of pine alcohol and 0.1-1 part of glycerol.
[0040] In some embodiments, the silane coupling agent modified glass powder includes at least two types of glass powders, and the softening points and particle sizes of the different types of glass powders are different.
[0041] In some specific examples, the silane coupling agent modified glass powder of the present application does not contain lead, that is, it is a silane coupling agent modified lead-free glass powder.
[0042] In some specific examples, the silane coupling agent modified glass powder includes the following raw materials: a silane coupling agent, ethanol, and at least two glass powders.
[0043] In some specific examples, the silane coupling agent modified glass powder includes the following raw materials, by weight: 1-3 parts of silane coupling agent, 58-62 parts of ethanol and 36-40 parts of at least two glass powders.
[0044] In some embodiments, the particle sizes of different types of glass powders are independently 0.5 μm to 5 μm.
[0045] In some of the embodiments, the particle sizes of different types of glass powders can be independently selected from any value between 1 μm and 5 μm (for example, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm, 1.6 μm, 1.7 μm, 1.8 μm, 1.9 μm, 2.0 μm, 3.0 μm, 4.0 μm or 5.0 μm), and the particle sizes of different glass powders are different.
[0046] As an example, the glass frit mixture may include a first glass frit having a particle size of 0.5 μm and a second glass frit having a particle size of 1.5 μm.
[0047] It is understandable that the glass powder mixture may contain two, three, four or more glass powders with different particle sizes.
[0048] In some embodiments, the softening points of different types of glass powders are independently 400° C. to 750° C.
[0049] In some embodiments, the softening points of different types of glass powders can be independently selected from any value in the range of 400°C to 750°C (e.g., 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 451°C, 452°C, 453°C, 454°C, 455°C, 456°C, 457°C, 458°C, 459°C, 460°C, 470°C, 480°C, 490°C, 500°C, ℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃, 600℃, 610℃, 620℃, 630℃, 640℃, 650℃, 660℃, 670℃, 680℃, 690℃, 700℃, 710℃, 720℃, 730℃, 740℃ or 750℃), and the softening point of each glass powder is different.
[0050] As an example, the glass frit mixture may include a first glass frit having a softening point of 400°C and a second glass frit having a softening point of 750°C.
[0051] It is understandable that the glass powder mixture may contain two, three, four or more glass powders having different softening points.
[0052] Glass powders with different particle sizes and softening points are selected for compounding. During the printing and film forming process, high and low softening point glass powders with different particle sizes are compounded, which can effectively reduce the holes inside the printed film layer, enhance the self-supporting ability, and improve the density and strength of the sintered film layer. The high softening point glass itself has good high-pressure stability, but the density of the sintered film layer is poor and the temperature coefficient is high. The addition of low softening point glass can reduce the softening temperature of the glass system. Under the premise of not affecting the pressure resistance stability of the sintered film layer, it can effectively improve the density of the sintered film layer. The temperature coefficient of the low softening point glass is negative. The compounding of the two glasses can effectively concentrate the positive and negative temperature coefficients within a suitable range.
[0053] In some embodiments, the silane coupling agent is selected from one or more of WD-26, WD-31, WD-50, WD-56, WD-42, A150, KMB5220, KBM602, KH550, KH570, KH560 and Z-6032.
[0054] In some of these embodiments, the conductive phase is selected from lead ruthenate.
[0055] In some embodiments, the particle size of the conductive phase is 500 nm to 5 μm. As an example, the particle size of the conductive phase can be selected from 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm or 5 μm; or a range consisting of any two of these values.
[0056] In some embodiments, the organic solvent is selected from one or more of terpineol, glycerol, terpineol, butyl carbitol acetate, butyl carbitol acetate, ethylene glycol ethyl ether acetate, tributyl citrate, dibutyl phthalate and lecithin.
[0057] In some embodiments, the thixotropic agent is selected from one or more of BYK607, fumed silica, organic bentonite, castor oil and polyamide wax.
[0058] In some embodiments, the dispersant is selected from one or more of Phobe 1000, SP-762, 7043, K-702, 9300, SDJ8006, SRE-47000, AD3013 and BYK111.
[0059] In some embodiments, the defoaming agent is selected from BYKA550, CBK-208, EDL-2100 or EDL2800.
[0060] In some embodiments, the viscosity of the resistor paste is 100 Pa·s to 300 Pa·s.
[0061] As an example, the viscosity of the resistor paste can be 100 Pa·s, 110 Pa·s, 120 Pa·s, 130 Pa·s, 140 Pa·s, 150 Pa·s, 160 Pa·s, 170 Pa·s, 180 Pa·s, 190 Pa·s, 200 Pa·s, 250 Pa·s or 300 Pa·s; or a range consisting of any two of these values.
[0062] The above-mentioned resistor paste of the present application has good printing stability, drying film adhesion, temperature coefficient resistance and high-voltage pulse resistance characteristics, and can be used as a resistor paste for flexible DC converter valves.
[0063] In a second aspect of the present application, a method for preparing a resistor paste is provided, comprising steps S10 to S20:
[0064] Step S10: providing the above-mentioned components of the resistor paste, and mixing them evenly to prepare a mixture.
[0065] In some embodiments, in step S10, the components of the resistor paste include 60-75 parts of silane coupling agent modified glass powder, 5-15 parts of conductive phase, 15-30 parts of organic vehicle, 5-15 parts of organic solvent, 0.1-0.5 parts of thixotropic agent, 0.1-0.5 parts of dispersant, and 0.2-1 parts of defoaming agent.
[0066] In some embodiments, the method for preparing the organic carrier comprises the following steps: providing modified hydroxyethyl cellulose, rosin resin, egg yolk lecithin, butyl carbitol acetate, terpineol and glycerol, and stirring them uniformly to obtain the organic carrier.
[0067] In some embodiments, the uniform stirring comprises the following steps: placing each material into a mixer, heating to 78° C. to 82° C., and mechanically stirring for 4.5 h to 5.5 h.
[0068] In some embodiments, the components of the organic carrier include: 5-15 parts of modified hydroxyethyl cellulose, 1-5 parts of rosin resin, 1-5 parts of egg yolk lecithin, 1-5 parts of butyl carbitol acetate, 70-90 parts of terpineol, and 0.1-1 part of glycerol, which are mixed evenly to prepare the organic carrier.
[0069] In some embodiments, the method for preparing modified hydroxyethyl cellulose comprises the following steps: sequentially subjecting natural cellulose material to alkalization treatment, activation treatment, hydroxyethylation treatment, desalination treatment and etherification treatment to prepare modified hydroxyethyl cellulose.
[0070] In some embodiments, the natural cellulosic material includes one or more of cotton, linen, and cotton batting.
[0071] In some embodiments, the natural cellulosic material is alkalized using a sodium hydroxide solution.
[0072] In some embodiments, the alkalization treatment comprises the following steps: immersing the natural cellulose material in a sodium hydroxide solution, heating to 95°C~100°C, ultrasonically stirring for 65min~75min, washing with deionized water at 78°C~82°C for 4~5 times, and drying to obtain an alkalized natural cellulose material.
[0073] In some embodiments, the activation treatment comprises the following steps: immersing the alkalized natural cellulose material in a sodium hydroxide solution with a concentration of 16% to 20% and a temperature of 34° C. to 36° C. for 38 min to 42 min to obtain a first reactant.
[0074] In some embodiments, the reaction formulas for the alkalization treatment and the activation treatment are as follows:
[0075] [C6H7O2(OH)3] n+nNaOH→ [C6H7O2(OH)2OH·NaOH] n
[0076] In some embodiments, the hydroxyethylation treatment comprises the following steps: immersing the first reactant in isopropanol, and adding ethylene oxide to react with ultrasonic stirring for 1.8 hours to 2.2 hours to obtain a second reactant.
[0077] In some embodiments, the reaction formula for the hydroxyethylation treatment is as follows:
[0078] C6H7O2(OH)2OH·NaOH+C2H4O→C6H7(OH)2OCH2CH2OH
[0079] In some embodiments, the desalting treatment comprises the following steps: adjusting the pH value of the second reactant to 6.5-7.5 using acetic acid, performing desalting washing 2-3 times using ethanol, and drying at 58° C.-62° C. for 7 h-9 h to obtain hydroxyethyl cellulose.
[0080] Optionally, in the desalting step, the amount of ethanol added is 14 to 16 times the sum of the masses of isopropanol and ethylene oxide.
[0081] In some embodiments, the etherification treatment comprises the following steps: modifying hydroxyethyl cellulose with an amphiphilic active monomer to obtain modified hydroxyethyl cellulose.
[0082] In some embodiments, the preparation method of the above-mentioned amphiphilic active monomer comprises the following steps: mixing dimethyltetradecylamine with 150 g / L isopropanol, heating to 70°C~80°C, mechanically stirring for 30min~40min, slowly dropping epichlorohydrin of equal molar mass to dimethyltetradecylamine, and refluxing under mechanical stirring for 1.5h~3.5h to obtain an amphiphilic active monomer.
[0083] In some examples, the etherification treatment includes the following steps: adding hydroxyethyl cellulose to 150 g / L isopropanol, mechanically stirring for 30 min to 40 min, slowly dripping NaOH solution until the concentration of NaOH is 0.05 g / L, mechanically stirring at room temperature for 36 hours, passing nitrogen and heating to 70°C to 80°C, slowly dripping amphiphilic active monomer, mechanically stirring at room temperature for 2 h to 4 h, adjusting the pH value to neutral, soaking in n-hexane at room temperature for 8 h, washing with acetone 3 to 4 times, and drying at 40°C to 60°C for 5 h to 8 h to obtain modified hydroxyethyl cellulose.
[0084] In the present application, the modified hydroxyethyl cellulose prepared by the above-mentioned specific method has the advantages of thickening, stability, good adhesion and dispersibility; it has good solubility in organic carriers and can effectively prevent the resistor paste from solvent precipitation and stratification.
[0085] In some embodiments, the method for preparing the silane coupling agent modified glass powder comprises the following steps:
[0086] A silane coupling agent, ethanol and at least two glass powders are provided, and the mixture is stirred and mixed to obtain silane coupling agent modified glass powder.
[0087] In some embodiments, stirring and mixing comprises the following steps: reacting with magnetic stirring at room temperature for 2h~3h.
[0088] Step S20: grinding and dispersing the mixture to obtain resistor slurry.
[0089] In some examples, in step S20, a three-roll mill is used to perform high-speed shearing, grinding and dispersion on the mixture.
[0090] In some embodiments, the method for preparing the resistor paste further includes step S30: filtering and vacuuming the resistor paste in sequence.
[0091] In some examples, in step S30, a 380-420 mesh screen is used to filter the resistor slurry to remove impurities or unevenly dispersed large particles in the slurry. Optionally, a 400 mesh screen is used to filter the resistor slurry.
[0092] According to a third aspect of the present application, a flexible DC-DC converter valve is provided, which includes the resistor slurry according to the first aspect or the resistor slurry prepared by the preparation method of the second aspect.
[0093] The present application will be further described below in conjunction with specific examples and comparative examples, but they should not be construed as limiting the scope of protection of the present application. The raw materials involved in the following specific examples, unless otherwise specified, can all be sourced from commercial sources, the instruments used, unless otherwise specified, can all be sourced from commercial sources, and the processes involved, unless otherwise specified, are all conventionally selected by those skilled in the art.
[0094] Example 1
[0095] (1) Preparation of organic carrier: Place cotton, linen and cotton wool fragments in a beaker containing 2% sodium hydroxide solution for alkalization, raise the temperature to 95°C, and perform ultrasonic stirring for 70 minutes. After ultrasonic stirring, wash them with deionized water at 80°C for 5 times and dry them. Soak the alkalized cotton, linen and cotton wool fragments in a sodium hydroxide solution with a concentration of 18% and a temperature of 35°C for 40 minutes for activation. Add the activated cotton, linen and cotton wool fragments to a beaker containing isopropanol, then add ethylene oxide and perform ultrasonic stirring for 2 hours. After the reaction is completed, use acetic acid to adjust the pH value to 7.5, and then use ethanol for desalination and washing. The amount of ethanol added is 15 times the total mass of isopropanol and ethylene oxide. After washing 3 times, dry them in an oven at 60°C for 9 hours to obtain hydroxyethyl cellulose.
[0096] Add dimethyltetradecylamine into a three-necked flask filled with isopropanol, the concentration of isopropanol is 150g / L, heat to 80°C, stir mechanically for 30 minutes, slowly add epichlorohydrin in an amount equimolar to dimethyltetradecylamine, keep warm and reflux for 2.5 hours under mechanical stirring to obtain an amphiphilic active monomer.
[0097] Add hydroxyethyl cellulose into a three-necked flask filled with isopropanol, the concentration of isopropanol is 150g / L, after mechanical stirring for 30min, slowly drip NaOH solution until the concentration of NaOH is 0.05g / L, mechanically stir at room temperature for 36h, pass nitrogen and heat to 80°C, slowly drip amphiphilic active monomer, mechanically stir at room temperature for 2h, adjust the pH value to neutral, soak in n-hexane at room temperature for 8h, wash with acetone 4 times, and dry at 60°C for 8h to obtain modified hydroxyethyl cellulose.
[0098] The following materials were weighed in parts by weight: 10 parts of modified hydroxyethyl cellulose, 1 part of rosin resin, 3 parts of egg yolk lecithin, 1 part of butyl carbitol acetate, 84.5 parts of terpineol, and 0.5 parts of glycerol. The above raw materials were put into a blender, heated to 80° C., and mechanically stirred for 5 hours to dissolve evenly to obtain an organic carrier.
[0099] (2) Preparation of silane coupling agent modified glass powder: Weigh 2 parts of silane coupling agent, 60 parts of ethanol, 10 parts of 1 μm glass powder (softening point: 500°C), and 28 parts of 1.5 μm glass powder (softening point: 720°C) by mass, and react the above raw materials under magnetic stirring at room temperature for 3 hours to obtain silane coupling agent modified glass powder.
[0100] (3) Preparation of resistor paste: Weigh 18 parts of the organic vehicle prepared in step (1), 62 parts of the silane coupling agent modified glass powder prepared in step (2), 14 parts of a conductive phase (lead ruthenate with a particle size of 1.5 μm), 5 parts of pine alcohol, 0.1 parts of fumed silica, 0.5 parts of BYK111, and 0.4 parts of BYKA550, by weight, and mix the above materials in a mixer for 1 hour, and then perform high-speed shear grinding and dispersion in a three-roll mill to obtain a resistor paste.
[0101] Example 2
[0102] The method is basically the same as Example 1, except that step (3) is different:
[0103] Preparation of resistor paste: Weigh 18 parts of the organic vehicle prepared in step (1), 66 parts of the silane coupling agent modified glass powder prepared in step (2), 10 parts of a conductive phase (lead ruthenate with a particle size of 1.5 μm), 5 parts of pineol, 0.1 parts of fumed silica, 0.5 parts of BYK111, and 0.4 parts of BYKA550, by weight, mix the above raw materials in a mixer for 1 hour, and then perform high-speed shear grinding and dispersion in a three-roll mill to obtain a resistor paste.
[0104] Example 3
[0105] The method is basically the same as Example 1, except that step (3) is different:
[0106] Preparation of resistor paste: 16 parts of the organic vehicle prepared in step (1), 70 parts of the silane coupling agent modified glass powder prepared in step (2), 8 parts of a conductive phase (lead ruthenate with a particle size of 1.5 μm), 5 parts of pineol, 0.1 parts of fumed silica, 0.5 parts of BYK111, and 0.4 parts of BYKA550 were weighed in parts by weight, and the above raw materials were mixed in a mixer for 1 hour, and then dispersed by high-speed shear grinding in a three-roll mill to obtain a resistor paste.
[0107] Example 4
[0108] The method is basically the same as Example 1, except that step (3) is different:
[0109] Preparation of resistor paste: Weigh 15 parts of the organic vehicle prepared in step (1), 73 parts of the silane coupling agent modified glass powder prepared in step (2), 6 parts of a conductive phase (lead ruthenate with a particle size of 1.5 μm), 5 parts of pineol, 0.1 parts of fumed silica, 0.5 parts of BYK111, and 0.4 parts of BYKA550, by weight, mix the above raw materials in a mixer for 1 hour, and then perform high-speed shear grinding and dispersion in a three-roll mill to obtain a resistor paste.
[0110] Example 5
[0111] The method is basically the same as Example 1, except that step (2) is different:
[0112] Preparation of silane coupling agent modified glass powder: According to mass percentage, weigh 2 parts of silane coupling agent, 60 parts of ethanol, 11.4 parts of 1.5μm glass powder (softening point is 510℃), and 26.6 parts of 0.9μm glass powder (softening point is 620℃), and react the above raw materials under magnetic stirring and room temperature for 3 hours to obtain silane coupling agent modified lead-free glass powder.
[0113] Example 6
[0114] The method is basically the same as Example 1, except that step (2) is different:
[0115] Preparation of silane coupling agent modified glass powder: According to mass percentage, weigh 2 parts of silane coupling agent, 60 parts of ethanol, 7.6 parts of 1.0μm glass powder (softening point is 490℃), and 30.4 parts of 1.1μm glass powder (softening point is 750℃), and react the above raw materials under magnetic stirring and room temperature for 2-3 hours to obtain silane coupling agent modified lead-free glass powder.
[0116] Example 7
[0117] The method is basically the same as Example 2, except that step (2) is different:
[0118] Preparation of silane coupling agent modified glass powder: According to mass percentage, weigh 2 parts of silane coupling agent, 60 parts of ethanol, and 38 parts of 1μm glass powder (softening point is 500°C), react the above raw materials under magnetic stirring and room temperature for 2-3 hours to obtain silane coupling agent modified lead-free glass powder.
[0119] Example 8
[0120] The method is basically the same as Example 2, except that step (2) is different:
[0121] Preparation of silane coupling agent modified glass powder: According to mass percentage, weigh 2 parts of silane coupling agent, 60 parts of ethanol, and 38 parts of 1.5μm glass powder (softening point is 720°C), react the above raw materials under magnetic stirring and room temperature for 2 to 3 hours to obtain silane coupling agent modified lead-free glass powder.
[0122] Comparative Example 1
[0123] The method is basically the same as Example 2, except that a glass powder mixture is used to replace the silane coupling agent-modified glass powder. Specifically, step (2) and step (3) are different:
[0124] (2) Weigh 10 parts by mass of 1 μm glass powder (softening point: 500°C) and 28 parts by mass of 1.5 μm glass powder (softening point: 720°C) and mix the above raw materials in a mixer for 2 hours to obtain a glass powder mixture.
[0125] (3) Preparation of resistor paste: Weigh 18 parts of the organic vehicle prepared in step (1), 62 parts of the glass powder mixture prepared in step (2), 14 parts of a conductive phase (lead ruthenate with a particle size of 1.5 μm), 5 parts of pineol, 0.1 parts of fumed silica, 0.5 parts of BYK111, and 0.4 parts of BYKA550, by weight, and mix the above materials in a mixer for 1 hour, and then perform high-speed shear grinding and dispersion in a three-roll mill to obtain a resistor paste.
[0126] Comparative Example 2
[0127] The method is basically the same as Example 1, except that hydroxyethyl cellulose is used instead of modified hydroxyethyl cellulose. The specific steps are as follows:
[0128] (1) Preparation of organic carrier: Place cotton, linen and cotton wool fragments in a beaker containing 2% sodium hydroxide solution for alkalization, raise the temperature to 95℃~100℃, and perform ultrasonic stirring for 70min. After ultrasonic stirring, wash with 80℃ deionized water for 4~5 times and dry. Soak the alkalized cotton, linen and cotton wool fragments in a sodium hydroxide solution with a concentration of 18% and a temperature of 35℃ for 40min for activation. Add the activated cotton, linen and cotton wool fragments to a beaker containing isopropanol, then add ethylene oxide and perform ultrasonic stirring for 2h. After the reaction is completed, use acetic acid to adjust the pH value to 6.5~7.5, and then use ethanol for desalination and washing. The amount of ethanol added is 15 times the mass of the reaction solution. After washing 2~3 times, dry in an oven at 60℃ for 7~9 hours to obtain hydroxyethyl cellulose.
[0129] The following materials were weighed in parts by weight: 10 parts of hydroxyethyl cellulose, 1 part of rosin resin, 3 parts of egg yolk lecithin, 1 part of butyl carbitol acetate, 84.5 parts of terpineol, and 0.5 parts of glycerol. The above raw materials were put into a blender, heated to 80° C., and mechanically stirred for 5 hours to dissolve evenly to obtain an organic carrier.
[0130] (2) Preparation of silane coupling agent modified glass powder: Weigh 2 parts of silane coupling agent, 60 parts of ethanol, 10 parts of 1 μm glass powder (softening point: 500°C), and 28 parts of 1.5 μm glass powder (softening point: 720°C) by mass, and react the above raw materials under magnetic stirring at room temperature for 3 hours to obtain silane coupling agent modified lead-free glass powder.
[0131] (3) Preparation of resistor paste: Weigh by weight 18 parts of ethyl cellulose prepared in step (1), 62 parts of glass powder prepared in step (2), 14 parts of conductive phase (lead ruthenate with a particle size of 1.5 μm), 5 parts of pine alcohol, 0.1 parts of fumed silica, 0.5 parts of BYK111, and 0.4 parts of BYK A550, and mix the above materials in a mixer for 1 hour, and then perform high-speed shear grinding and dispersion in a three-roll mill to obtain a resistor paste.
[0132] The resistor paste prepared in the above Examples 1-8 and Comparative Examples 1-2 was screen-printed once on an alumina substrate through a 325-mesh screen, and the sintered film thickness was 13 μm-15 μm. The screen-printed substrate was baked in a drying furnace at 180°C for 10 min-15 min, and then sintered in a sintering furnace at 845°C for 10 min. After the film was formed, the performance was tested. The test method is shown in Table 1, and the test results are shown in Table 2.
[0133] Table 1
[0134]
[0135] Table 2
[0136]
[0137] In the above embodiments of the present application, the resistor paste prepared by using a specific hydroxyethyl cellulose carrier and a silane coupling agent modified glass powder greatly improves the printing performance of the resistor paste on the substrate, makes the paste stable for continuous printing, and provides good drying film adhesion.
[0138] The silane coupling agent modified glass powder of Example 7 and Example 8 only contains one kind of glass powder, and the TCR value of the sintered coating formed on the alumina substrate by the finally prepared resistor paste is relatively high. This indicates that the silane coupling agent modified glass powder prepared by using two or more glass powders with different particle sizes and softening points can make the resistor paste fully sintered under high temperature conditions of 800°C to 850°C, and the positive and negative temperature coefficients after sintering are within -50~+50ppm / °C, and have good high voltage pulse resistance characteristics.
[0139] Compared with Example 2, in Comparative Example 1, a glass powder mixture is used instead of silane coupling agent modified glass powder, and the resistance concentration and temperature coefficient of resistance of the sintered coating formed by the resistor slurry finally prepared on the alumina substrate are increased, and the adhesion of the dried film is poor.
[0140] Compared with Example 1, in Comparative Example 2, hydroxyethyl cellulose is used instead of modified hydroxyethyl cellulose, and the resistance concentration of the sintered coating formed on the alumina substrate by the finally prepared resistor slurry is increased, and the adhesion of the dried film is significantly worse.
[0141] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0142] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
Claims
1. A resistor paste, characterized in that: The composition comprises the following components by weight: 60-75 parts of silane coupling agent modified glass powder, 5-15 parts of conductive phase, 15-30 parts of organic carrier, 5-15 parts of organic solvent, 0.1-0.5 parts of thixotropic agent, 0.1-0.5 parts of dispersant and 0.2-1 parts of defoaming agent; The organic carrier comprises the following components: 5-15 parts of modified hydroxyethyl cellulose, 1-5 parts of rosin resin, 1-5 parts of egg yolk lecithin, 1-5 parts of butyl carbitol acetate, 70-90 parts of terpineol and 0.1-1 part of glycerol.
2. The resistor paste according to claim 1, characterized in that: The silane coupling agent modified glass powder includes at least two types of glass powders, and the softening points and particle sizes of the different types of glass powders are different.
3. The resistor paste according to claim 2, characterized in that: The resistor paste meets at least one of the following characteristics: (1) The particle sizes of the different types of glass powders are independently 0.5 μm to 5 μm; (2) The softening points of the different types of the glass powder are independently 400° C. to 750° C.
4. The resistor paste according to any one of claims 1 to 3, characterized in that: The resistor paste meets at least one of the following characteristics: (1) The silane coupling agent in the silane coupling agent modified glass powder is selected from one or more of WD-26, WD-31, WD-50, WD-56, WD-42, A150, KMB5220, KBM602, KH550, KH570, KH560 and Z-6032; (2) The conductive phase is selected from lead ruthenate; (3) The particle size of the conductive phase is 500nm~5μm; (4) The organic solvent is selected from one or more of terpineol, glycerol, terpineol, butyl carbitol acetate, butyl carbitol acetate, ethylene glycol ethyl ether acetate, tributyl citrate, dibutyl phthalate and lecithin; (5) The thixotropic agent is selected from one or more of BYK607, fumed silica, organic bentonite, castor oil and polyamide wax; (6) The dispersant is selected from one or more of Phobe 1000, SP-762, 7043, K-702, 9300, SDJ8006, SRE-47000, AD3013 and BYK111; (7) The defoaming agent is selected from BYK A550, CBK-208, EDL-2100 or EDL2800.
5. A method for preparing a resistor paste, characterized in that: The steps include: According to the components of the resistor paste according to any one of claims 1 to 4, a silane coupling agent-modified glass powder, a conductive phase, an organic carrier, an organic solvent, a thixotropic agent, a dispersant and a defoaming agent are provided, and the components are mixed uniformly to prepare a mixture; The mixture is subjected to grinding and dispersion treatment to obtain the resistor paste.
6. The method for preparing the resistor paste according to claim 5, characterized in that: The preparation method of the organic carrier comprises the following steps: Modified hydroxyethyl cellulose, rosin resin, egg yolk lecithin, butyl carbitol acetate, terpineol and glycerol are provided and stirred uniformly to obtain an organic carrier.
7. The method for preparing the resistor paste according to claim 6, characterized in that: The preparation method of the modified hydroxyethyl cellulose comprises the following steps: The natural cellulose material is subjected to alkalization treatment, activation treatment, hydroxyethylation treatment, desalination treatment and etherification treatment in sequence to obtain modified hydroxyethyl cellulose.
8. The method for preparing a resistor paste according to claim 5, characterized in that: The preparation method of the silane coupling agent modified glass powder comprises the following steps: A silane coupling agent, ethanol and at least two glass powders are provided, and the mixture is stirred and mixed to obtain silane coupling agent modified glass powder.
9. The method for preparing a resistor paste according to any one of claims 5 to 8, characterized in that: The method further comprises the following steps: filtering and vacuuming the resistor paste in sequence.
10. A flexible direct current valve, characterized in that: A resistor paste comprising the resistor paste according to any one of claims 1 to 4 or a resistor paste prepared by the method for preparing the resistor paste according to any one of claims 5 to 9.
Citation Information
Cited By
Silver paste, preparation method thereof and solar cell
CN121583608A