Crack template, metal grid transparent conductive film and preparation method and application of metal grid transparent conductive film

The liquid cracking material is secondary cracked by microwave heating technology to prepare a crack template with narrow line width and small cycles, which solves the problem of easy cracking and uneven performance in the preparation of transparent conductive films of metal mesh in the prior art. Efficient crack network formation and performance improvement are achieved.

CN119049797APending Publication Date: 2024-11-29CHINA BUILDING MATERIALS ACADEMY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411197376.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

It is difficult to prepare a metal grid transparent conductive film with narrow line width and small periods, and the film layer is too thin and prone to cracking unevenly, affecting the photoelectric performance.

Method used

The liquid crack material is secondary cracked by microwave heating technology to form a crack template with a narrow line width and small periods to ensure that the crack network is connected and distributed evenly. The crack formation is finely regulated by adjusting the microwave frequency, power and time.

Benefits of technology

The optical performance and electromagnetic shielding effect of the transparent conductive film of the metal grid are improved, and the crack template preparation with narrow line width and small cycles is achieved, ensuring the connectivity and depth of the crack network, and improving the film performance and processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049797A_ABST
    Figure CN119049797A_ABST
Patent Text Reader

Abstract

The invention provides a crack template, a metal grid transparent conductive film and a preparation method and application of the metal grid transparent conductive film. The preparation method of the crack template comprises the following steps: preparing a transparent substrate; coating the transparent substrate with a liquid crack material; drying and cracking the liquid crack material on the transparent substrate to obtain an original crack template; and carrying out microwave heating on the original crack template, and carrying out secondary cracking on the original crack template to obtain the crack template. Compared with a traditional crack template preparation method, microwave heating is rapid and uniform, the machining efficiency can be improved, and a crack network can be formed more rapidly; by changing parameters such as microwave power and time, the microwave absorption degree of the template is different, and the stress formed by the internal heat effect is different, so that the formation process of the crack is more accurately controlled, and the fine regulation and control of the crack network are realized. The crack template prepared by the method has the advantages of narrow crack line width, small period, good connectivity, uniform distribution and thorough depth, and is more practical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of transparent conductive film preparation, and in particular to a crack template, a metal grid transparent conductive film, and a preparation method and application thereof. Background Art

[0002] Metal grid transparent conductive film is a basic optoelectronic material with both conductivity and light transmittance, and is widely used in optoelectronic devices. The metal grid on it is composed of micro-nanoscale metal wires. The grid structure period is much larger than the wavelength of visible light (400nm~700nm), and most of the light can pass through the grid. When high-frequency electromagnetic waves contact the metal micro-nano grid, eddy currents (i.e., circular currents) will be induced on the metal surface. These induced currents will generate a magnetic field opposite to the original electromagnetic wave, thereby offsetting part of the incident electromagnetic wave. Conventionally arranged metal grids are usually prepared by photolithography or laser direct writing. Although these methods can accurately control the grid structure, their processing costs are high and the technical threshold is large. In addition, when the grid is periodically arranged, moiré fringes are easily generated when visible light passes through, affecting the optical performance. In contrast, randomly distributed metal grids can effectively reduce the coherent scattering of light and improve the light transmittance of the film. The crack template method has gradually attracted widespread attention due to its advantages such as simple process, low processing difficulty and low manufacturing cost.

[0003] With the development of semiconductor technology, the application of metal grid transparent conductive films with narrow line width and small period has become more widespread. In the process of crack template preparation, by reducing the crack template thickness to reduce the gap width and crack period, it is expected to obtain metal grid transparent conductive films with narrow line width and small period. However, when the film layer is too thin, it is easy to crack unevenly and incompletely, resulting in isolated cracks or partially connected crack networks. These defects will affect the optoelectronic properties of metal grid transparent conductive films and limit the promotion of crack template method in practical applications.

[0004] Therefore, how to prepare crack templates with narrow linewidth and small period while ensuring that the crack network is completely broken and obtaining a highly uniform crack distribution is of great significance for improving the optical properties and electromagnetic shielding effect of metal grids. Summary of the invention

[0005] The main purpose of the present invention is to provide a crack template, a metal grid transparent conductive film, and a preparation method and application thereof. The technical problem to be solved by the invention is how to prepare a crack template with a narrow line width and a small period, and ensure that the crack network is interconnected, the crack distribution is uniform and the depth is thorough, so as to improve its performance in practical applications.

[0006] The purpose of the present invention and the technical problem solved are achieved by adopting the following technical solutions. A method for preparing a crack template according to the present invention comprises the following steps:

[0007] (1) Preparing a transparent substrate;

[0008] (2) coating a liquid crack material on the aforementioned transparent substrate;

[0009] (3) drying and cracking the aforementioned liquid crack material on the aforementioned transparent substrate to obtain an original crack template;

[0010] (4) The original crack template is subjected to microwave heating to cause secondary cracking of the original crack template to obtain a crack template.

[0011] The purpose of the present invention and the solution to its technical problems can be further achieved by adopting the following technical measures.

[0012] In some embodiments, according to the aforementioned preparation method, the aforementioned transparent substrate is a silica transparent glass slide or organic glass.

[0013] In some embodiments, according to the aforementioned preparation method, the aforementioned liquid crack material is one of egg white, water-based acrylic emulsion, crack nail polish, titanium dioxide solution and colloidal silicon dioxide.

[0014] In some embodiments, according to the aforementioned preparation method, in step (2), the aforementioned liquid crack material on the aforementioned transparent substrate is a water-based acrylic emulsion, and the thickness of the coated dry film is less than 5 μm.

[0015] In some embodiments, according to the aforementioned preparation method, in step (2), the aforementioned liquid crack material is coated on the aforementioned transparent substrate by spin coating, pulling method or blade coating method.

[0016] In some embodiments, according to the aforementioned preparation method, in step (4), during microwave heating, the power of the microwave is 200 to 600 W, and the time is 20 to 60 s.

[0017] The purpose of the present invention and the technical problems solved therein are also achieved by the following technical solutions: A crack template proposed in the present invention is prepared by any of the above-mentioned preparation methods, wherein the average period of the above-mentioned crack template is 6-11 μm and the average line width is 0.7-0.9 μm.

[0018] The purpose of the present invention and the solution to its technical problems are also achieved by the following technical solutions. According to a method for preparing a metal grid transparent conductive film proposed by the present invention, it includes the following steps: preparing a crack template according to any of the aforementioned preparation methods; depositing metal on the aforementioned crack template and removing the crack material to obtain a metal grid transparent conductive film.

[0019] The purpose of the present invention and the technical problems solved therein are also achieved by the following technical solutions: According to the present invention, a metal grid transparent conductive film is prepared by the above-mentioned preparation method, and the average period of the metal grid thereon is 6-11 μm, and the average line width is 0.7-0.9 μm.

[0020] The purpose of the present invention and the technical problem solved are also achieved by adopting the following technical solutions: An optoelectronic device proposed in the present invention includes the aforementioned metal grid transparent conductive film.

[0021] Through the above technical solution, the crack template, metal grid transparent conductive film and preparation method and application thereof of the present invention have at least the following advantages:

[0022] Aiming at the problem that the existing crack template method for preparing metal mesh transparent conductive film cannot obtain narrow slit width and small period metal micro-nano mesh, the preparation method of the crack template provided by the present invention exposes the original crack template to the microwave field, and the crack material absorbs microwave energy, so that heat is generated inside the material, thereby forming stress, inducing crack formation, and then the incompletely cracked original crack template is subjected to secondary cracking to obtain a crack template. Compared with the traditional crack template preparation method, microwave heating is rapid and uniform, which can improve processing efficiency and form a crack network faster; by changing microwave frequency, power, time and other parameters, the degree of microwave absorption by the template is different, and the stress formed by the internal thermal effect is different, so as to more accurately control the crack formation process, so as to achieve fine regulation of the crack network. The crack template prepared by the method of the present invention ensures that the crack network is interconnected, the crack distribution is uniform and the depth is thorough while ensuring narrow line width and small period.

[0023] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic diagram of a process of preparing a crack template disclosed in an embodiment of the present invention;

[0025] Figure 2 is a depth of field microscope observation diagram of the original crack template in Example 1 of the present invention;

[0026] Figure 3 is a depth of field microscope observation image of the crack template prepared in Example 1 of the present invention;

[0027] Figure 4 is a depth of field microscope observation image of the crack template prepared in Example 2 of the present invention;

[0028] Figure 5This is a depth of field microscope observation image of the crack template prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0029] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the following is a detailed description of the crack template, metal grid transparent conductive film and its preparation method and its specific implementation, structure, characteristics and effects of the application proposed by the present invention in combination with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.

[0030] The present invention provides these embodiments to make the present invention thorough and complete, and fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of materials, numerical expressions and numerical values ​​set forth in these embodiments should be interpreted as being merely exemplary, rather than as limiting.

[0031] The present invention proposes a method for preparing a crack template, and its flow diagram is as follows: Figure 1 As shown, it includes the following steps:

[0032] (1) Preparing a transparent substrate;

[0033] (2) coating a liquid crack material on the aforementioned transparent substrate;

[0034] (3) drying and cracking the aforementioned liquid crack material on the aforementioned transparent substrate to obtain an original crack template;

[0035] (4) The original crack template is subjected to microwave heating to cause secondary cracking of the original crack template to obtain a crack template.

[0036] Specifically, the crack template prepared by the present invention is used to prepare a metal mesh transparent conductive film. The metal mesh transparent conductive film is a basic optoelectronic material with both conductivity and light transmittance. Therefore, the substrate here uses a transparent substrate. For example, the material of the transparent substrate can be a silicon dioxide transparent glass slide or organic glass. These two materials have good optical properties and high light transmittance, which are conducive to improving the performance of the metal mesh transparent conductive film. After the transparent substrate is cleaned, the subsequent steps can be performed.

[0037] In step (2), a liquid crack material is coated on the transparent substrate. The main function of the liquid crack material is to form a crack template on the transparent substrate as a forming template for the metal grid. Therefore, the liquid crack material is a material that can be cracked after drying. For example, the liquid crack material is egg white, water-based acrylic emulsion, crack nail polish, titanium dioxide solution or colloidal silicon dioxide. The liquid crack material can be evenly coated on the transparent substrate by a spin coating method, a pull coating method or a scraping method.

[0038] In step (3), after being allowed to stand and air-dry, the liquid crack material is naturally cracked to obtain an original crack template having a random crack network.

[0039] In step (4), the original crack template is heated by microwaves to undergo secondary cracking of the original crack template to obtain a crack template. The original crack template is exposed to a microwave field, and the crack material absorbs microwave energy, causing heat to be generated inside the material, thereby forming stress, inducing crack formation, and then the incompletely cracked original crack template is subjected to secondary cracking to obtain a crack template. Compared with traditional crack template preparation methods, microwave heating is rapid and uniform, which can improve processing efficiency and form a crack network more quickly; by changing microwave frequency, power, time and other parameters, the degree of microwave absorption by the template is different, and the stress formed by the internal thermal effect is different, thereby more accurately controlling the crack formation process to achieve fine regulation of the crack network.

[0040] The crack template prepared by the method of the present invention ensures narrow line width and small period, while the crack networks are interconnected, the cracks are evenly distributed and the depth is thorough.

[0041] In some embodiments, in step (2), the aforementioned liquid crack material on the aforementioned transparent substrate is a water-based acrylic emulsion, and the thickness of the coated dry film is less than 5 μm.

[0042] Specifically, water-based acrylic emulsion has the advantages of easy application, quick drying, and excellent adhesion, and is a preferred material for preparing crack templates. The diluent of the water-based acrylic emulsion can be deionized water or anhydrous ethanol, and its mass concentration is controlled to be 40% to 80%. When the liquid crack material is a water-based acrylic emulsion, the thickness of the dry film of the original crack template obtained after natural drying is controlled to be less than 5μm. When the thickness of the dry film is ≥5μm, the internal stress generated during the solute shrinkage process will increase significantly, resulting in warping of the crack template unit, which is not conducive to the production of a metal grid transparent conductive film with excellent photoelectric properties.

[0043] In some embodiments, in step (4), during microwave heating, the microwave power is 200-600 W, and the time is 20-60 s. Within the range of microwave power and time, the controllability of the crack can be improved, and the obtained secondary crack template has a smaller period and a thinner line width. When the microwave power is lower than 200 W, or the microwave time is lower than 20 s, some cracks are not completely formed, which affects the performance of the produced metal mesh transparent conductive film. When the microwave power is higher than 600 W, or the microwave time is higher than 60 s, the period is smaller and the crack line width is wider, which affects the performance of the produced metal mesh transparent conductive film. Therefore, during microwave heating, the microwave power is controlled at 200-600 W, and the time is controlled at 20-60 s.

[0044] The present invention provides a crack template, which is prepared by any of the aforementioned preparation methods. The crack template has an average period of 6 to 11 μm and an average line width of 0.7 to 0.9 μm.

[0045] The present invention provides a method for preparing a metal grid transparent conductive film, which comprises the following steps: preparing a crack template according to any of the aforementioned preparation methods; depositing metal on the aforementioned crack template and removing crack materials to obtain a metal grid transparent conductive film.

[0046] Specifically, metal deposition can be performed by existing technologies, for example, magnetron sputtering, thermal evaporation or electroplating. Crack materials can be removed by existing technologies. For example, crack materials can be removed by the following method: immerse the metal deposition sample in a mixed solution of acetone and KOH with a mass ratio of 1:1, and then place it in an ultrasonic cleaning machine, set the ultrasonic power to 60W, and perform ultrasonic cleaning for about 15 minutes to remove the crack materials.

[0047] The present invention provides a metal grid transparent conductive film, which is prepared by the above-mentioned preparation method. The average period of the metal grid on the film is 6-11 μm, and the average line width is 0.7-0.9 μm.

[0048] An optoelectronic device proposed by the present invention includes the aforementioned metal grid transparent conductive film. For example, the metal grid transparent conductive film can be applied to large-size touch panels. Its high conductivity and good optical transmittance characteristics make the metal grid transparent conductive film an ideal choice for touch panels. In addition, the cost of this film is relatively low, which further improves its competitiveness in touch panel applications. The metal grid transparent conductive film also shows application potential in the field of electromagnetic shielding. It can effectively absorb and block electromagnetic waves, protecting equipment and personnel from interference and influence of electromagnetic radiation.

[0049] The present invention will be further described below in conjunction with specific embodiments, but this should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.

[0050] Unless otherwise specified, the materials, reagents, etc. involved below are all commercially available products well known to those skilled in the art; unless otherwise specified, the methods described are all methods well known in the art. Unless otherwise defined, the technical terms or scientific terms used should have the common meanings understood by ordinary technicians in the field to which the present invention belongs.

[0051] Example 1

[0052] This embodiment provides a method for preparing a crack template and a crack template, such as Figure 1 As shown, the preparation method thereof comprises the following steps:

[0053] (1) A silica transparent glass slide is used as a transparent substrate and is cleaned.

[0054] (2) Using water-based acrylic emulsion as the crack material, 45% of the water-based acrylic emulsion by mass was evenly dispersed on the substrate by spin coating, wherein the spin coating speed was 1500 r / min and the time was 15 s.

[0055] (3) After the aqueous acrylic emulsion on the substrate is naturally dried, the original crack template is obtained. The original crack template is observed using a depth of field microscope. Figure 2 As shown, the crack period and crack width were calculated using software Nano-Measurer. The average crack width was 1.11 μm and the average period was 17.09 μm.

[0056] (4) The original crack template is sent into an industrial microwave chamber for microwave heating at a microwave power of 400 W for 20 s, which causes the original crack template to undergo secondary cracking to obtain a crack template.

[0057] The crack template was observed using a depth-of-field microscope. Figure 3 As shown in the figure, the crack cycle and crack width were statistically calculated using the software Nano-Measurer. The average crack width was 0.83 μm and the average cycle was 10.59 μm. Compared with the original crack template, the average crack width and average cycle were reduced. This is because many small cracks were generated between the original large-cycle crack blocks. In the statistical process, the line width of the small cracks was smaller, thereby reducing the overall average line width. The reduction in the average cycle also proved that the crack template was secondary cracked. These results show that microwave induction can effectively increase the crack density.

[0058] Example 2

[0059] The difference between this embodiment and embodiment 1 is that in step (4), the microwave heating time is 40 seconds.

[0060] The crack template obtained in this embodiment was observed using a depth of field microscope. Figure 4 As shown, the crack cycle and crack width were calculated using the software Nano-Measurer, and the average crack cycle was 7.73 μm and the average line width was 0.78 μm. Compared with the crack template obtained in Example 1, the average crack cycle and average line width of the crack template obtained in this example were further reduced, indicating that the crack template can be further cracked after increasing the microwave-induced heating time. In addition, as the size of the crack cycle decreases, the uniformity of the crack cycle and crack line width is also better, which shows that the quality and uniformity of the crack template can be effectively improved by optimizing the microwave heating time.

[0061] Example 3

[0062] The difference between this embodiment and embodiment 1 is that in step (4), during microwave heating, the microwave power is 600 W and the time is 40 s.

[0063] The crack template obtained in this embodiment was observed using a depth of field microscope. Figure 5 As shown in the figure, the crack period and crack width were calculated using the software Nano-Measurer. The measurement results showed that the average crack period was 6.15 μm and the average line width was 0.82 μm. Compared with the crack template in Example 2, the average line width increased from 0.78 μm to 0.82 μm after the power was increased. Although the crack width increased, it still remained in a lower size range and was similar to the crack width in Example 2. Figure 4 Compared with the microscopic pattern of , the phenomenon of incomplete crack cleavage is significantly reduced. This shows that by adjusting the microwave power, the complete cleavage of the crack network can be promoted and a crack template with smaller period and more uniformity can be obtained.

[0064] From the observation results of the line width and period of the crack templates in the above-mentioned Examples 1 to 3 and the original crack template in Example 1, it can be seen that in the crack template obtained after the original crack template is treated by microwave induction, the period and line width of the crack block are significantly reduced; when the microwave power and microwave time are within a certain range, for the same microwave induced power, the longer the heating time, the smaller the period and line of the crack block; for the same microwave heating time, the greater the microwave power, the smaller the period and line of the crack block, thereby achieving the controllable crack template.

[0065] Example 4

[0066] This embodiment provides a method for preparing a metal mesh transparent conductive film and a metal mesh transparent conductive film.

[0067] Metal deposition was performed using the original crack template in Example 1 and the crack templates prepared in Examples 1-3, and then the crack material was removed to obtain four metal grid transparent conductive films, whose transmittance and square resistance are shown in Table 1.

[0068] It can be seen from the data in Table 1 that compared with the metal mesh transparent conductive film corresponding to the original crack template, the transmittance of the metal mesh transparent conductive film prepared by the crack template obtained in Examples 1-3 has decreased, indicating that the secondary pyrolysis of microwave-induced cracks does increase the number of cracks, and the depth of the crack pyrolysis of the secondary pyrolysis is thorough, and the density of the metal mesh is increased. However, the decrease in transmittance is not obvious, and the metal mesh transparent conductive film prepared by the crack template obtained in Examples 1-3 still has a high transmittance, greater than or equal to 78.9%. Compared with the metal mesh transparent conductive film corresponding to the original crack template, the square resistance of the metal mesh transparent conductive film prepared by the crack template obtained in Examples 1-3 is significantly reduced, indicating that its conductivity is significantly improved. It shows that the crack template prepared by the method provided by the present invention has a narrow line width and a small period, and its cracks are uniform and the depth is thorough. The metal mesh transparent conductive film prepared by the crack template provided by the present invention has a high transmittance and good conductivity.

[0069] Table 1 Transmittance and square resistance of each metal grid transparent conductive film

[0070] Crack template Light transmittance (%) Square resistance (Ω / sq) Original crack template 83.01 6.5 Example 1 81.1 4.7 Example 2 80.3 3.2 Example 3 78.9 2.2

[0071] It should be pointed out that the above embodiments are only further explanations of the present invention, rather than limitations. For example, in addition to using a transparent glass slide made of silicon dioxide, other cheap transparent substrate materials (PMMA, PC, PVC, PP, etc.) can also be used to make the substrate for preparing the sample. The microwave heating power is not limited to 400w and 600w in the above embodiments, and the heating time is not limited to 20s and 40s. Other specific parameter values ​​are within the scope of the technical solution and can also achieve the purpose of the present invention. Therefore, any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

[0072] The technical features in the claims and / or the specification of the present invention may be combined, and the combination is not limited to the combination obtained by reference in the claims. The technical solution obtained by combining the technical features in the claims and / or the specification is also within the protection scope of the present invention.

[0073] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a crack template, characterized in that: It includes the following steps: (1) Preparing a transparent substrate; (2) coating a liquid crack material on the transparent substrate; (3) drying and cracking the liquid crack material on the transparent substrate to obtain an original crack template; (4) The original crack template is subjected to microwave heating to cause secondary cracking of the original crack template to obtain a crack template.

2. The preparation method according to claim 1, characterized in that: The transparent substrate is a silicon dioxide transparent glass slide or organic glass.

3. The preparation method according to claim 1, characterized in that: The liquid crack material is one of egg white, water-based acrylic emulsion, crack nail polish, titanium dioxide solution and colloidal silicon dioxide.

4. The preparation method according to claim 1, characterized in that: In step (2), the liquid crack material on the transparent substrate is a water-based acrylic emulsion, and the thickness of the coated dry film is less than 5 μm.

5. The preparation method according to claim 1, characterized in that: In step (2), the liquid crack material is coated on the transparent substrate by spin coating, Czochralski coating or doctor blade coating.

6. The preparation method according to claim 1, characterized in that: In step (4), during microwave heating, the microwave power is 200 to 600 W and the heating time is 20 to 60 seconds.

7. A crack template, characterized in that: The crack template is prepared by the preparation method according to any one of claims 1 to 6, wherein the average period of the crack template is 6 to 11 μm, and the average line width is 0.7 to 0.9 μm.

8. A method for preparing a metal grid transparent conductive film, characterized in that: It includes the following steps: A crack template is prepared according to the preparation method described in any one of claims 1 to 6; metal deposition is performed on the crack template and crack materials are removed to obtain a metal grid transparent conductive film.

9. A metal grid transparent conductive film, characterized in that: The metal grid is prepared by the preparation method of claim 8, and the average period of the metal grid is 6 to 11 μm, and the average line width is 0.7 to 0.9 μm.

10. An optoelectronic device, characterized in that: It includes the metal grid transparent conductive film as described in claim 9.

Citation Information

Cited By

  • Transparent conductive film containing double-layer grid structure and preparation method thereof

    CN119920539A