Preparation method of compression-molded complex-shaped sintered permanent magnetic ferrite

Through molding and degumming and pressurized sintering technology, the problem of insufficient magnetic and mechanical properties of complex shape sintered permanent magnet ferrite in the existing technology is solved, and high-performance production of complex shape permanent magnet ferrite is achieved to meet the market's high standards. Performance product demand and improved thermal stability.

CN119049865APending Publication Date: 2024-11-29SICHUAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411287525.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

It is difficult to prepare complex shape sintered permanent magnet ferrites with high magnetic properties and mechanical strength, especially miniaturized and shaped products, and traditional bonded magnets have insufficient thermal stability under high temperature conditions.

Method used

Complex-shaped permanent magnet ferrite green body is prepared by molding and molding, and then degummed under vacuum conditions and pressurized sintering is carried out to remove organic components and improve the proportion and density of magnetic components.

Benefits of technology

It has achieved the improvement of high magnetic performance and mechanical performance, can meet the market's demand for high-performance small and complex shape permanent magnet ferrite products, and improves thermal stability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of preparation of sintered permanent magnetic ferrites, and provides a preparation method of compression molding complex-shaped sintered permanent magnetic ferrites, which comprises the following steps: (1) preparing a permanent magnetic ferrite master batch for compression molding; (2) carrying out compression molding on the master batch under the condition of applying an oriented magnetic field; and (3) putting the obtained green body into a low-pressure sintering furnace, heating to 300-600 DEG C under the condition of continuous vacuumizing, carrying out degumming treatment, stopping vacuumizing, heating to 1100-1250 DEG C, then filling nitrogen or argon until the pressure in the furnace is 2-5MPa, carrying out low-pressure sintering, and cooling to room temperature along with the furnace, so as to obtain the sintered permanent magnetic ferrite with the complex shape. According to the invention, the preparation of the sintered permanent magnetic ferrite with high magnetic performance and complex shape can be realized, and the problems of low magnetic performance, insufficient mechanical strength and the like of the permanent magnetic ferrite prepared by the existing preparation method of the bonded magnet can be solved; and the existing preparation method of the sintered magnet cannot meet the design requirements of high-performance small complex special-shaped permanent magnetic ferrite products.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sintered permanent ferrite preparation, and relates to a method for preparing a sintered permanent ferrite with a complex shape by compression molding. Background Art

[0002] In the field of permanent ferrites, there are more and more miniaturized, complex and special-shaped designs, and the requirements for the magnetic properties of the products are also getting higher and higher. In order to meet the requirements for miniaturized, complex and special-shaped products, traditional preparation technologies often use injection molding or molding to make bonded magnets. However, since bonded magnets contain a large amount of non-magnetic components such as adhesives, plasticizers and stabilizers, the proportion of magnetic powder filling is not high, resulting in low magnetic properties of bonded magnets. For bonded permanent ferrites, the best magnetic properties on the market are currently YN12 bonded permanent ferrites, and its magnetic properties related data: remanence (Br) is 240~250mT, coercive force (HCB) is 140~160KA / m, intrinsic coercive force (HCJ) is 200~230KA / m, maximum magnetic energy product (BH (max) ) is 11.4~13.6KJ / m 3 . Its magnetic properties are difficult to meet the market demand for high-performance products, and bonded magnets also have problems such as insufficient mechanical strength and poor thermal stability. The traditional method of preparing sintered permanent ferrites by dry pressing or wet pressing orientation molding followed by high-temperature sintering can produce sintered magnets with higher magnetic properties, but it is difficult to meet the requirements of the magnet for complex shapes and cannot achieve the preparation of small, complex, and special-shaped permanent ferrite devices. Summary of the invention

[0003] In view of the problems that permanent ferrite prepared by the existing bonding magnet preparation method has low magnetic properties and insufficient mechanical strength, and the problem that the existing sintered magnet preparation method cannot meet the requirements of high-performance small-scale complex and special-shaped permanent ferrite product design, the present invention provides a method for preparing sintered permanent ferrite with complex shapes by compression molding, so as to achieve the preparation of sintered permanent ferrite with complex shapes and higher magnetic properties.

[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0005] A method for preparing a sintered permanent ferrite with a complex shape by compression molding, comprising the following steps:

[0006] (1) Pre-sintering permanent magnet ferrite powder at 800-900° C. for 1-3 hours, and cooling to room temperature with the furnace to obtain annealed permanent magnet ferrite powder; using the annealed permanent magnet ferrite powder, adhesive and additives as raw materials, ball-milling all the raw materials to mix them evenly, drying, sieving, and then granulating them to obtain permanent magnet ferrite masterbatch for compression molding; the additives include plasticizers, lubricants and secondary additives;

[0007] (2) molding the permanent magnet ferrite masterbatch for molding into a permanent magnet ferrite green body of a desired complex shape;

[0008] (3) Placing the complex-shaped permanent ferrite green body in a low-pressure sintering furnace, evacuating the low-pressure sintering furnace to a pressure of 0.1 to 20 Pa, then heating it to 300 to 600°C, and keeping it warm for 2 to 4 hours to perform debonding treatment. During the heating and keeping warm process, evacuating the furnace continuously to maintain the pressure in the furnace at 0.1 to 20 Pa. After the debonding treatment is completed, stopping evacuating the furnace, heating it to 1100 to 1250°C, and then filling the low-pressure sintering furnace with nitrogen or argon to a pressure of 2 to 5 MPa. Keeping it warm for 1 to 2 hours to perform low-pressure sintering. After the sintering is completed, cooling it to room temperature with the furnace to obtain a complex-shaped sintered permanent ferrite.

[0009] In step (1) of the above preparation method, the contents of the annealed permanent magnet ferrite pre-sintered material magnetic powder, adhesive and auxiliary agent in all raw materials are preferably 88wt% to 93wt%, 3wt% to 5wt%, and 4wt% to 7wt%, respectively.

[0010] In the technical solution of the above preparation method, the permanent magnet ferrite pre-sintered material magnetic powder is at least one of strontium ferrite magnetic powder, barium ferrite magnetic powder, and strontium-barium mixed ferrite magnetic powder.

[0011] In the technical solution of the above preparation method, the average particle size of the permanent magnet ferrite pre-sintered magnetic powder in step (1) is preferably 3 to 4 μm.

[0012] In the technical solution of the above preparation method, the adhesive comprises at least one of phenolic resin, epoxy resin, amino resin and polyimide resin. The epoxy resin is preferably E-20 epoxy resin.

[0013] In the technical solution of the above preparation method, the plasticizer is di(2-ethylhexyl) phthalate, and the lubricant is selected from at least one of stearyl glycerol and stearic acid and any one of anhydrous ethanol and acetone.

[0014] In the technical solution of the above preparation method, the secondary additive can be selected according to the actual application requirements with reference to the prior art. For example, in order to improve the density and strength of the sintered permanent magnet ferrite, at least one of calcium carbonate, silicon dioxide and aluminum oxide can be selected as the secondary additive. When calcium carbonate, silicon dioxide and aluminum oxide are selected as the secondary additives, the amounts of calcium carbonate, silicon dioxide and aluminum oxide should be such that the contents of calcium carbonate, silicon dioxide and aluminum oxide in the masterbatch are 0.2wt% to 0.5wt%, 0.1wt% to 0.3wt%, and 0wt% to 0.2wt%, respectively.

[0015] In step (2) of the technical solution of the above preparation method, it is preferred to control the molding orientation magnetic field strength to be at least 8000 Oe, the molding temperature to be 120-150° C., and the molding pressure to be 600-1000 MPa.

[0016] In step (3) of the above preparation method, the heating rate is preferably controlled to be 3 to 5°C / min.

[0017] The main technical concept of the present invention is that first, the annealed permanent magnet ferrite pre-sintered material magnetic powder, adhesive and auxiliary agent (including plasticizer, lubricant and secondary additive) are made into a permanent magnet ferrite masterbatch for compression molding, and then compression molding is performed into a permanent magnet ferrite green body of the required complex shape, and then degumming treatment is performed under continuous vacuum conditions to carbonize and remove the auxiliary agents of organic components such as adhesives, plasticizers and lubricants. After the degumming treatment is completed, sintering is performed under pressurized conditions (the pressure in the furnace is 2-5MPa) to increase the density of the magnet, and a complex-shaped sintered permanent magnet ferrite is obtained. On the one hand, the present invention prepares the permanent magnet ferrite green body of the required complex shape by compression molding from the permanent magnet ferrite masterbatch for compression molding, which solves the problem that the existing preparation method of sintered permanent magnet ferrite can meet the requirements of high magnetic properties, but is difficult to meet the design and use requirements of complex-shaped products such as miniaturization and special-shaped. On the other hand, the present invention subjects the obtained permanent magnet ferrite green body of complex shape to carbonization debinding and pressure sintering, thereby removing the binder and auxiliary agent of organic components, increasing the proportion of magnetic components and the density of the magnet, thereby improving the magnetic properties and mechanical properties of the permanent magnet ferrite, solving the problem that the existing preparation method of bonded permanent magnet ferrite can meet the design and use requirements of complex-shaped products but has low magnetic properties and mechanical properties, and can also solve the problem of poor thermal stability of the magnet when used under high temperature conditions caused by the presence of binders and auxiliary agents of organic components.

[0018] Compared with the prior art, the technical solution provided by the present invention produces the following beneficial technical effects:

[0019] The present invention provides a method for preparing a sintered permanent ferrite with a complex shape by compression molding. The method firstly forms a permanent ferrite masterbatch for compression molding into a permanent ferrite green body with a desired complex shape by compression molding, then debonds under continuous vacuum conditions and sinters under pressure conditions to obtain a permanent ferrite with a complex shape. Compared with the prior art method of preparing sintered permanent ferrite by first dry pressing or wet pressing orientation molding and then high-temperature sintering, the present invention forms a permanent ferrite masterbatch for compression molding by compression molding, realizes free molding of the permanent ferrite green body, and can prepare a green body with a complex shape, solving the problem of the existing method for preparing sintered permanent ferrite that it is difficult to prepare small, complex and special-shaped permanent ferrite devices. Compared with the existing preparation method of bonded permanent magnet ferrite, which mixes a large amount of adhesive, plasticizer and stabilizer with magnetic powder and then forms it freely, the present invention carbonizes the green body of complex shape under continuous vacuum conditions, so that the adhesive and auxiliary agent of organic components are pyrolyzed and removed, and then sintered under pressure, which increases the proportion of magnetic components and the density of the magnet, thereby improving the magnetic properties and mechanical properties of the permanent magnet ferrite, and solves the problems of low magnetic properties and mechanical properties of existing bonded permanent magnet ferrite products, as well as poor thermal stability when used under high temperature conditions. The method of the present invention can realize the preparation of sintered permanent magnet ferrite with complex shapes and high magnetic properties, and can better meet the market demand for high-performance, miniaturized, and special-shaped permanent magnet ferrite components with complex shapes. DETAILED DESCRIPTION

[0020] The following examples further illustrate the preparation method of the sintered permanent magnet ferrite with complex shapes provided by the present invention. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. The technical personnel in the relevant field make some non-essential improvements and adjustments to the present invention according to the above invention content and implement them specifically, which still falls within the scope of protection of the present invention.

[0021] Example 1

[0022] In this embodiment, a method for preparing a sintered permanent ferrite with a complex shape by compression molding is provided, and the steps are as follows:

[0023] (1) Strontium ferrite permanent magnet powder is passed through a 60-80 mesh sieve to obtain strontium ferrite permanent magnet powder with an average particle size of 3.0 μm. Strontium ferrite permanent magnet powder with an average particle size of 3.0 μm is heated to 800° C. in a muffle furnace, kept at this temperature for 3 hours, and then cooled to room temperature for annealing treatment to obtain annealed strontium ferrite permanent magnet powder.

[0024] (2) Annealed strontium ferrite permanent magnet powder, adhesive and auxiliary agent are used as raw materials, and the ingredients are prepared according to the ratio of 88wt%, 5wt% and 7wt% of the annealed strontium ferrite permanent magnet powder, adhesive and auxiliary agent in all raw materials, respectively. The adhesive is phenolic resin and E-20 epoxy resin, and the auxiliary agent includes a plasticizer, a lubricant and a secondary additive. The plasticizer is di(2-ethylhexyl) phthalate (DEHP), the lubricant is stearic acid glycerol and anhydrous ethanol, and the secondary additive is calcium carbonate, silicon dioxide and aluminum oxide.

[0025] Weigh 880g of annealed strontium ferrite permanent magnet powder, 25g of phenolic resin, 25g of E-20 epoxy resin, 5g of DEHP, 5g of glyceryl stearate, 50g of anhydrous ethanol, 5g of calcium carbonate, 3g of silicon dioxide, and 2g of aluminum oxide. Fully ball-mill the weighed raw materials in a high-energy planetary ball mill to mix them evenly, dry and sieve them, and then granulate them to make permanent magnet ferrite masterbatch for molding.

[0026] (3) The permanent magnet ferrite masterbatch for compression molding is compression molded into a permanent magnet ferrite green body of the desired complex shape on a compression molding device, and the molding orientation magnetic field intensity is controlled to be 8000Oe, the molding temperature is 120°C, and the molding pressure is 600MPa.

[0027] (4) placing the permanent magnet ferrite green body in a low-pressure sintering furnace, evacuating the low-pressure sintering furnace until the pressure inside the furnace is 10Pa, then heating the temperature to 600°C at a heating rate of 3°C / min, and keeping the temperature for 2 hours to perform degreasing treatment. During the heating and keeping temperature process, vacuuming is continuously performed to maintain the pressure inside the furnace at a level of 0.1 to 10Pa. After the degreasing treatment is completed, vacuuming is stopped, and the temperature is increased to 1170°C at a heating rate of 3°C / min. Argon is filled into the low-pressure sintering furnace until the pressure inside the furnace is 5MPa. The temperature is kept for 1 hour for low-pressure sintering. After the sintering is completed, the furnace is cooled to room temperature to obtain a sintered permanent magnet ferrite with a complex shape.

[0028] The samples were taken and polished, and the magnetic properties were tested. The results showed that the remanence (Br) was 405.8mT, the coercive force (HCB) was 285KA / m, the intrinsic coercive force (HCJ) was 303KA / m, and the maximum magnetic energy product (BH (max) ) is 30KJ / m 3 .

[0029] Example 2

[0030] In this embodiment, a method for preparing a sintered permanent ferrite with a complex shape by compression molding is provided, and the steps are as follows:

[0031] (1) The barium ferrite permanent magnet powder is passed through a 60-80 mesh sieve to obtain a barium ferrite permanent magnet powder with an average particle size of 3.6 μm. The barium ferrite permanent magnet powder with an average particle size of 3.6 μm is heated to 850° C. in a muffle furnace, kept at this temperature for 2 hours, and cooled to room temperature for annealing treatment to obtain annealed barium ferrite permanent magnet powder.

[0032] (2) Annealed strontium ferrite permanent magnet powder, adhesive and auxiliary agent are used as raw materials, and the contents of annealed barium ferrite permanent magnet powder, adhesive and auxiliary agent in all raw materials are respectively 91wt%, 4wt% and 5wt%. The adhesive is phenolic resin, E-20 epoxy resin and amino resin. The auxiliary agent includes plasticizer, lubricant and secondary additive. The plasticizer is DEHP, the lubricant is stearic acid glyceryl ester and acetone, and the secondary additive is calcium carbonate, silicon dioxide and aluminum oxide.

[0033] Weigh 910g of annealed barium ferrite permanent magnet powder, 10g of phenolic resin, 20g of E-20 epoxy resin, 10g of amino resin, 3g of DEHP, 3g of glyceryl stearate, 40g of acetone, 2g of calcium carbonate, 1g of silicon dioxide, and 1g of aluminum oxide. Fully ball-mill the weighed raw materials in a high-energy planetary ball mill to mix them evenly, dry and sieve them, and then granulate them to make permanent magnet ferrite masterbatch for compression molding.

[0034] (3) The permanent magnet ferrite masterbatch for compression molding is compression molded into a permanent magnet ferrite green body of the desired complex shape on a compression molding device, and the molding orientation magnetic field intensity is controlled to be 10000Oe, the molding temperature is 130°C, and the molding pressure is 800MPa.

[0035] (4) placing the permanent magnet ferrite green body in a low-pressure sintering furnace, evacuating the low-pressure sintering furnace until the pressure inside the furnace is 5 Pa, then heating the temperature to 500° C. at a heating rate of 4° C. / min, and keeping the temperature for 3 hours to perform a degreasing treatment. During the heating and holding process, evacuating the body continuously to maintain the pressure inside the furnace at a level of 0.1 to 5 Pa. After the degreasing treatment is completed, stopping the evacuation, heating the body to 1210° C. at a heating rate of 4° C. / min, filling the low-pressure sintering furnace with argon until the pressure inside the furnace is 4 MPa, and keeping the temperature for 2 hours to perform low-pressure sintering. After the sintering is completed, cooling the body to room temperature with the furnace to obtain a sintered permanent magnet ferrite with a complex shape.

[0036] The samples were taken and polished, and the magnetic properties were tested. The results showed that the remanence (Br) was 410mT, the coercive force (HCB) was 288KA / m, the intrinsic coercive force (HCJ) was 308KA / m, and the maximum magnetic energy product (BH (max) ) is 32KJ / m 3 .

[0037] Example 3

[0038] In this embodiment, a method for preparing a sintered permanent ferrite with a complex shape by compression molding is provided, and the steps are as follows:

[0039] (1) Strontium ferrite permanent magnet powder, barium ferrite permanent magnet powder, and strontium-barium mixed ferrite permanent magnet powder are respectively passed through a 60-80 mesh sieve, and then the sieved strontium ferrite permanent magnet powder, barium ferrite permanent magnet powder, and strontium-barium mixed ferrite permanent magnet powder are mixed in a mass ratio of 1:1:1 to obtain a permanent magnet ferrite mixed magnetic powder with an average particle size of 3.2 μm. The permanent magnet ferrite mixed magnetic powder with an average particle size of 3.2 μm is heated to 900°C in a muffle furnace, kept at this temperature for 1 hour, and cooled to room temperature for annealing treatment to obtain an annealed permanent magnet ferrite mixed magnetic powder.

[0040] (2) Annealed strontium ferrite permanent magnet powder, adhesive and auxiliary agent are used as raw materials, and the contents of annealed permanent magnet ferrite mixed magnetic powder, adhesive and auxiliary agent in all raw materials are respectively 93wt%, 3wt% and 4wt%. The adhesive is E-20 epoxy resin, and the auxiliary agent includes a plasticizer, a lubricant and a secondary additive. The plasticizer is DEHP, the lubricant is stearic acid and anhydrous ethanol, and the secondary additive is calcium carbonate, silicon dioxide and aluminum oxide.

[0041] Weigh 930g of annealed permanent ferrite mixed magnetic powder, 30g of E-20 epoxy resin, 2g of DEHP, 2g of stearic acid, 30g of anhydrous ethanol, 2g of calcium carbonate, and 2g of silicon dioxide. Fully mill and mix the weighed raw materials in a high-energy planetary ball mill, dry, sieve, and then granulate to make a permanent ferrite masterbatch for compression molding.

[0042] (3) The permanent magnet ferrite masterbatch for compression molding is compression molded into a permanent magnet ferrite green body of the desired complex shape on a compression molding device, and the molding orientation magnetic field intensity is controlled to be 12000Oe, the molding temperature is 150°C, and the molding pressure is 1000MPa.

[0043] (4) placing the permanent magnet ferrite green body in a low-pressure sintering furnace, evacuating the low-pressure sintering furnace until the pressure inside the furnace is 0.1 Pa, then heating the temperature to 450°C at a heating rate of 5°C / min, and keeping the temperature for 4 hours to perform a degreasing treatment. During the heating and holding process, vacuuming is continuously performed to maintain the pressure inside the furnace at a level of 0.1 Pa. After the degreasing treatment is completed, vacuuming is stopped, and the temperature is increased to 1240°C at a heating rate of 4°C / min. Nitrogen is filled into the low-pressure sintering furnace until the pressure inside the furnace is 3.5MPa. The temperature is kept for 1.5 hours to perform low-pressure sintering. After the sintering is completed, the furnace is cooled to room temperature to obtain a sintered permanent magnet ferrite with a complex shape.

[0044] The samples were taken and polished, and the magnetic properties were tested. The results showed that the remanence (Br) was 407mT, the coercive force (HCB) was 288KA / m, the intrinsic coercive force (HCJ) was 308KA / m, and the maximum magnetic energy product (BH (max) ) is 31KJ / m 3 .

[0045] At present, the bonded permanent ferrite with the best magnetic properties on the market is YN12 bonded permanent ferrite. Its magnetic properties are as follows: remanence (Br) is 240-250mT, coercive force (HCB) is 140-160KA / m, intrinsic coercive force (HCJ) is 200-230KA / m, maximum magnetic energy product (BH (max) ) is 11.4~13.6KJ / m 3 . Combined with Examples 1 to 3, it can be seen that, compared with the YN12 bonded permanent magnet ferrite, the magnetic properties of the complex-shaped sintered permanent magnet ferrite prepared by the method of the present invention have been improved. At the same time, since the method of the present invention performs debonding and pressure sintering, the density of the magnet is further increased on the basis of removing the adhesive and auxiliary agent of the organic component. Therefore, compared with the existing bonded permanent magnet ferrite, the complex-shaped sintered permanent magnet ferrite prepared by the method of the present invention also has more advantages in mechanical properties, which can better meet the market demand for high-performance small-sized complex and special-shaped permanent magnet ferrite products.

Claims

1. A method for preparing a sintered permanent ferrite with a complex shape by compression molding, characterized in that: The following steps are involved: (1) Pre-sintering permanent magnet ferrite powder at 800-900° C. for 1-3 hours, and cooling to room temperature with the furnace to obtain annealed permanent magnet ferrite powder; using the annealed permanent magnet ferrite powder, adhesive and additives as raw materials, ball-milling all the raw materials to mix them evenly, drying, sieving, and then granulating them to obtain permanent magnet ferrite masterbatch for compression molding; the additives include plasticizers, lubricants and secondary additives; (2) molding the permanent magnet ferrite masterbatch for molding, applying an oriented magnetic field during molding, and manufacturing a permanent magnet ferrite green body with a desired complex shape; (3) Placing the complex-shaped permanent ferrite green body in a low-pressure sintering furnace, evacuating the low-pressure sintering furnace to a pressure of 0.1 to 20 Pa, then heating it to 300 to 600°C, and keeping it warm for 2 to 4 hours to perform debonding treatment. During the heating and keeping warm process, evacuating the furnace continuously to maintain the pressure in the furnace at 0.1 to 20 Pa. After the debonding treatment is completed, stopping evacuating the furnace, heating it to 1100 to 1250°C, and then filling the low-pressure sintering furnace with nitrogen or argon to a pressure of 2 to 5 MPa. Keeping it warm for 1 to 2 hours to perform low-pressure sintering. After the sintering is completed, cooling it to room temperature with the furnace to obtain a complex-shaped sintered permanent ferrite.

2. The method for preparing a sintered permanent ferrite with a complex shape by compression molding according to claim 1, characterized in that: In step (1), the contents of the annealed permanent magnet ferrite pre-sintered material magnetic powder, adhesive and auxiliary agent in all raw materials are 88wt% to 93wt%, 3wt% to 5wt% and 4wt% to 7wt% respectively.

3. The method for preparing a sintered permanent ferrite with a complex shape by compression molding according to claim 1, characterized in that: The magnetic powder of the permanent ferrite pre-sintered material is at least one of strontium ferrite magnetic powder, barium ferrite magnetic powder and strontium-barium mixed ferrite magnetic powder.

4. The method for preparing a sintered permanent ferrite with a complex shape by compression molding according to claim 1, characterized in that: The adhesive includes at least one of phenolic resin, epoxy resin, amino resin and polyimide resin.

5. The method for preparing a sintered permanent ferrite with a complex shape by compression molding according to claim 1, characterized in that: In the auxiliary agent, the mass ratio of the plasticizer, the lubricant and the secondary additive is (2-5):(32-55):(4-10).

6. The method for preparing a sintered permanent ferrite with a complex shape by compression molding according to claim 1, characterized in that: The plasticizer is di(2-ethylhexyl) phthalate, and the lubricant is selected from at least one of stearyl glycerol and stearic acid and any one of anhydrous ethanol and acetone.

7. The method for preparing a sintered permanent ferrite with a complex shape by compression molding according to claim 1, characterized in that: The secondary additive includes at least one of calcium carbonate, silicon dioxide and aluminum oxide.

8. The method for preparing a sintered permanent ferrite with a complex shape by compression molding according to any one of claims 1 to 7, characterized in that: In step (2), the molding orientation magnetic field strength is controlled to be at least 8000 Oe, the molding temperature is controlled to be 120-150° C., and the molding pressure is controlled to be 600-1000 MPa.

9. The method for preparing a sintered permanent ferrite with a complex shape by compression molding according to any one of claims 1 to 7, characterized in that: The heating rate during the temperature increase in step (3) is controlled to be 3 to 5°C / min.

10. The method for preparing a sintered permanent ferrite with a complex shape by compression molding according to any one of claims 1 to 7, characterized in that: The average particle size of the permanent magnet ferrite pre-sintered magnetic powder in step (1) is 3 to 4 μm.