Heterojunction diode and preparation method thereof

By using the preparation method of β-Ga2O3/SiC heterojunction diode in gallium oxide power devices, the problem of insufficient reliability and voltage resistance characteristics of gallium oxide power devices at high temperatures is solved, and the device performance and high temperature reliability are improved Improvement.

CN119049970APending Publication Date: 2024-11-29XIAMEN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411237032.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

In the prior art, the reliability and voltage resistance characteristics of gallium oxide power devices are insufficient at high temperatures, and the P-type epitaxial process and ion implantation process are immature, resulting in difficult improvement of device performance and reliability.

Method used

Using the preparation method of β-Ga2O3/SiC heterojunction diode, the β-Ga2O3 layer is formed on the P-type SiC substrate, and combined with the intelligent ion knife and the ozone-enhanced PEALD process, the inclined structure and buffer layer are formed to improve the device's Voltage withstand performance and conduction current, and improve electric field distribution through ozone surface passivation treatment.

Benefits of technology

It significantly improves the reverse breakdown voltage and withstand voltage characteristics of heterojunction devices, reduces switching losses, and improves high-temperature reliability and heat dissipation, improving the overall performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119049970A_ABST
    Figure CN119049970A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of power radio frequency discrete devices, in particular to a heterojunction diode and a preparation method thereof. The method comprises the following steps: providing a P-type substrate; forming a bonding intermediate layer with a corundum crystal structure on the upper surface of the P-type substrate; a beta-Ga2O3 layer is provided; ion implantation is carried out on the beta-Ga2O3 layer; transferring the beta-Ga2O3 layer to the bonding intermediate layer to form a heterogeneous integrated substrate; forming a semiconductor layer on the upper surface of the heterogeneous integrated substrate; the heterojunction diode is round from the overlook direction, the semiconductor layer and the round side wall of the heterogeneous integrated substrate are inclined towards the interior of the heterojunction diode through etching to form an inclined plane, and the positive oblique angle theta of the inclined plane is smaller than 70 degrees and larger than or equal to 60 degrees; performing ozone passivation treatment on the semiconductor layer; forming a metal anode on the upper surface of the semiconductor layer; the heterojunction diode provided by the invention has relatively high voltage resistance / breakdown performance and relatively good device reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of power radio frequency discrete devices, and in particular to a heterojunction diode and a preparation method thereof. Background Art

[0002] As an emerging ultra-wide bandgap semiconductor material, β-Ga2O3 has the characteristics of an ultra-wide bandgap of 4.8eV, a relatively high theoretical breakdown electric field strength of 8MV / cm, and a high saturation drift rate. The theoretical breakdown field strength is three times that of SiC and GaN materials. Not only does it have physical properties such as high temperature resistance, high pressure resistance, and strong radiation resistance that are superior to SiC and GaN, but it also has other unique material properties, such as photoelectric detection characteristics in the deep ultraviolet band and highly sensitive gas-sensitive properties, and has both the transparency of sapphire and the conductivity of SiC. At the same time, since the low-cost, low-energy melt-growth preparation process of large-inch gallium oxide substrates has become increasingly mature, and high-quality N-type Ga2O3 epitaxial layers can be obtained through molecular beam epitaxy (MBE), chemical vapor deposition (CVD), pulsed laser deposition (PLD) and other methods, it has a large application space in high-frequency, high-power devices, ultraviolet photodetectors, transparent conductive films, etc., and has broad application prospects in aerospace, military, and nuclear energy, becoming an emerging research direction that has attracted attention from industry and academia.

[0003] The Baliga figure of merit (BFOM=3444) of Ga2O3 is very high and is an indicator of the performance of semiconductor materials, which is defined as ε·μ·E c 3 , where ε, μ and E c They are dielectric constant, carrier mobility and critical breakdown field strength. The BFOM of Ga2O3 is 4 times that of GaN material and more than 10 times that of SiC material. Therefore, it is considered suitable for the preparation of next-generation power devices including PN junction diodes (PND), Schottky diodes (SBD) and field effect transistors (FET). How to achieve high-performance and high-reliability gallium oxide power devices is attracting more and more attention. Summary of the invention

[0004] In order to solve the deficiencies in the above-mentioned prior art, the present invention aims to provide a PND device based on β-Ga2O3 / SiC heterojunction, which can effectively improve the performance of diode devices, achieve lower on-resistance and on-voltage, improve the high-temperature reliability of the device, greatly improve the reverse breakdown voltage and withstand voltage characteristics of the device, and reduce the switching loss of the device.

[0005] In this regard, one of the technical solutions provided by the present invention is as follows:

[0006] A method for preparing a heterojunction diode comprises the following steps:

[0007] Providing a P-type substrate;

[0008] forming a bonding intermediate layer having a corundum type crystal structure on the upper surface of the P-type substrate;

[0009] Providing a β-Ga2O3 layer, the β-Ga2O3 layer having a first surface and a second surface;

[0010] Performing ion implantation on the second surface of the β-Ga2O3 layer;

[0011] Transferring the β-Ga2O3 layer to the bonding intermediate layer so that the second surface of the β-Ga2O3 layer contacts the upper surface of the bonding intermediate layer to form a heterogeneous integrated substrate;

[0012] A semiconductor layer is formed on the upper surface of the heterogeneous integrated substrate, wherein the semiconductor layer includes a buffer N-type layer and an N + Epitaxial layer;

[0013] The heterojunction diode is circular when viewed from above, and etching causes the circular side surfaces of the heterogeneous integrated substrate and the semiconductor layer to be inclined toward the inside of the heterojunction diode to form an inclined surface, and the positive bevel angle θ of the inclined surface is less than 70° and greater than or equal to 60°;

[0014] Performing ozone passivation treatment on the semiconductor layer;

[0015] forming a metal anode on the upper surface of the semiconductor layer;

[0016] Optionally, after forming the heterogeneous integrated substrate, a metal cathode is formed on the lower surface of the heterogeneous integrated substrate.

[0017] In one embodiment, the P-type substrate is a P-type SiC substrate;

[0018] Preferably, the thickness of the P-type substrate is 2 μm-100 μm;

[0019] Preferably, the ion types implanted on the upper surface of the β-Ga2O3 layer include hydrogen, iron or magnesium, and the implantation angle is 7°;

[0020] Preferably, the method further comprises, after completing the ion implantation of the second surface, bombarding the surface of the ion implantation layer with Ar ions;

[0021] Preferably, the thickness of the β-Ga2O3 layer is 60-100 nm.

[0022] In one embodiment, forming the bonding intermediate layer comprises: plasma PEALD deposition;

[0023] Preferably, the PEALD (plasma enhanced ALD) deposition includes forming the bonding intermediate layer at a certain temperature using trimethyl aluminum (TMA) and ozone as reaction precursors;

[0024] Preferably, the thickness of the bonding intermediate layer is 10-40 nm.

[0025] In one embodiment, the material of the buffer N-type layer is an unintentionally doped UID β-Ga2O3 layer;

[0026] Preferably, the thickness of the buffer N-type layer is 6 μm, and the carrier concentration of the buffer N-type layer is 1×10 14 cm -3 -1×10 16 cm -3 .

[0027] In one embodiment, the N + The material of the epitaxial layer is β-Ga2O3 doped with any one or at least two of Sn, Si and Ge;

[0028] Preferably, the N + The thickness of the epitaxial layer is 300-500nm. + The carrier concentration of the epitaxial layer is 1×10 18 cm -3 -1×10 20 cm -3 .

[0029] In one embodiment, after forming the semiconductor layer, the semiconductor layer is annealed;

[0030] Preferably, the annealing temperature of the annealing treatment is 500-700° C., the annealing time is 20-60 min, and the annealing atmosphere is selected from any one of ozone, oxygen, nitrogen, and argon, or a combination of at least two of them.

[0031] In one embodiment, after the annealing treatment is completed, ultraviolet ozone treatment is performed;

[0032] Preferably, the wavelength of the ultraviolet lamp source for the ultraviolet ozone treatment is 185nm or 254nm, the ultraviolet ozone treatment time is 15-30min, and the ultraviolet ozone treatment temperature is 25-200°C.

[0033] In one embodiment, the oxygen-based passivation treatment includes: performing a surface passivation treatment based on ozone (O3) or oxygen (O2) or oxygen plasma on the product after the inclined surface is formed.

[0034] In one embodiment, the thickness of the metal cathode is 200-300 nm;

[0035] The material of the metal cathode is selected from Au, Al, Ti, Sn, Ge, In, Ni, Co, Pt, W, Mo, Cr, Cu, Pb or any combination of alloys thereof or any combination of laminates or conductive compounds thereof; and / or

[0036] The thickness of the metal anode is 200-300nm;

[0037] The material of the metal anode is selected from Au, Al, Ti, Sn, Ge, In, Ni, Co, Pt, W, Mo, Cr, Cu, Pb, or an alloy of any combination thereof, or a stack of any combination thereof, or a conductive compound.

[0038] The second technical solution provided by the present invention is as follows:

[0039] A heterojunction diode manufactured by the manufacturing method as described above.

[0040] Based on the above, compared with the prior art, the heterojunction diode prepared by the preparation method provided by the present invention adopts a terminal structure with a beveled sidewall, effectively alleviates the maximum surface electric field at the heterojunction by controlling the positive bevel angle, and improves the bevel passivation effect by combining the ozone surface passivation process, so that the distribution of the electric field inside the device is readjusted, the electric field concentration effect is alleviated, the withstand voltage performance of the heterojunction device is improved, and the on-state current of the device is improved, and the breakdown voltage is greatly increased;

[0041] In addition, the use of P-type SiC and N-type Ga2O3 to form a heterojunction can effectively solve the current problem of the immaturity of the P-type epitaxial process and ion implantation process of wide bandgap semiconductor Ga2O3 materials;

[0042] Furthermore, combined with the intelligent ion knife Smart-Cut TM The process, ozone enhanced PEALD process, wet etching / dry etching or chemical mechanical polishing process are used to improve the peeling and transfer effects, so as to better realize the heterogeneous integration of β-Ga2O3 / 4H-SiC, β-Ga2O3 / 6H-SiC and β-Ga2O3 / 3C-SiC heterojunctions. The β-Ga2O3 / SiC heterojunction realized by the above process can greatly improve the thermal dissipation, operating temperature and preparation cost of the device, and alleviate the high temperature reliability problem in high-power applications.

[0043] Other features and beneficial effects of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other beneficial effects of the present invention can be realized and obtained by the structures particularly pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. The positional relationships described in the drawings in the following description are based on the directions in which the components are drawn in the diagrams, unless otherwise specified.

[0045] Figure 1 A top view (top) and a cross-sectional view (bottom) of a heterojunction diode provided in Example 1 of the present invention;

[0046] Figures 2 to 11 Schematic diagram of the process flow of the heterojunction diode according to Example 1 of the present invention.

[0047] Reference numerals:

[0048] 10. Metal cathode; 20. Heterogeneous integrated substrate; 21. P-type substrate; 22. Bonding intermediate layer; 23. β-Ga2O3 layer; 24. Ion implantation layer; 30. Semiconductor layer; 31. Buffer N-type layer; 32. N + Epitaxial layer; 40, metal anode; 50, photolithography mask I; 60, physical mask I. DETAILED DESCRIPTION

[0049] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments; the technical features designed in different implementation modes of the present invention described below can be combined with each other as long as they do not conflict with each other; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0050] In the description of the present invention, it should be noted that all terms used in the present invention (including technical terms and scientific terms) have the same meanings as those generally understood by ordinary technicians in the field to which the present invention belongs, and cannot be understood as limiting the present invention; it should be further understood that the terms used in the present invention should be understood to have the same meanings as these terms in the context of this specification and in the relevant fields, and should not be understood in an idealized or overly formal sense, unless explicitly defined in the present invention.

[0051] Example 1

[0052] refer to Figure 1 , an embodiment of the present invention provides a heterojunction diode, the heterojunction diode comprising, from bottom to top, a metal cathode 10, a heterogeneous integrated substrate 20, a semiconductor layer 30, and a metal anode 40;

[0053] The heterogeneous integrated substrate 20 includes, from bottom to top, a P-type substrate 21, a bonding intermediate layer 22 having a corundum-type crystal structure, an ion implantation layer 24, and a β-Ga2O3 layer 23;

[0054] The semiconductor layer 30 includes a buffer N-type layer 31 and an N-type layer 32 from bottom to top. + Epitaxial layer 32;

[0055] When viewed from above, the heterojunction diode is circular, and the circular side surfaces of the semiconductor layer 30 and the heterogeneous integrated substrate 20 are respectively inclined toward the inside of the heterojunction diode to form a first inclined surface 20a and a second inclined surface 30a. Preferably, the first inclined surface 20a and the second inclined surface 30a are continuous, and the positive bevel angle θ of the first inclined surface 20a and the second inclined surface 30a is less than 70° and greater than or equal to 60°. Preferably, the positive bevel angle θ of the first inclined surface 20a and the second inclined surface 30a is less than or equal to 68° and greater than or equal to 64°.

[0056] This embodiment provides a method for preparing the above heterojunction diode, comprising the following steps:

[0057] Step 1: Reference Figure 2 , prepare a β-Ga2O3 layer 23 with a thickness of 200μm-600μm and a size of 1-6 inches, the β-Ga2O3 layer 23 has a first surface 23a and a second surface 23b, and pre-treat and clean the β-Ga2O3 layer 23.

[0058] β-Ga2O3 is an emerging wide bandgap semiconductor material. It can effectively improve the device performance of the dual-gate device because of its bandgap width (4.7-4.9 eV) far exceeding that of SiC and GaN, its theoretical breakdown electric field (8 MV / cm), and its low price relative to SiC and GaN substrates. Therefore, it is used as one of the semiconductor substrate materials of the heterogeneous integrated substrate 20.

[0059] The β-Ga2O3 layer 23 is sequentially subjected to organic cleaning and inorganic cleaning;

[0060] The steps of the organic cleaning are as follows:

[0061] The first step is to use ethanol ultrasonic cleaning for 3 minutes; the second step is to use acetone ultrasonic cleaning for 3 minutes; the third step is to use ethanol ultrasonic cleaning for 3 minutes; the fourth step is to use deionized water or ultrapure water to rinse for 3 minutes; the fifth step is to use running deionized water to rinse for 5 minutes;

[0062] The inorganic cleaning steps are as follows:

[0063] The first step is to soak in deionized water or ultrapure water and heat to 90°C; the second step is to prepare SPM solution according to the volume ratio of deionized water: 30% hydrogen peroxide: 96% concentrated sulfuric acid = 1:1:4, and soak in SPM solution for 5 minutes;

[0064] Optionally, in the second step, a Piranha solution is prepared according to a volume ratio of 30% hydrogen peroxide: 98% concentrated sulfuric acid = 1:3, and the Piranha solution is used for soaking for 1 minute; in the third step, deionized water or ultrapure water is used for soaking and heated to 90° C., and then cooled to room temperature.

[0065] Step 2: Reference Figure 3 , performing ion implantation on the second surface 23b of the β-Ga2O3 layer 23 prepared in step 1 to form an ion implantation layer 24, the implanted ions may be H, Fe, Mg, and the implantation angle is 7°, so as to facilitate subsequent heterogeneous substrate bonding;

[0066] Optionally, after the ion implantation of the second surface 23 b is completed, the surface of the ion implantation layer 24 is bombarded with Ar ions.

[0067] Step 3: Reference Figure 4 , providing a P-type substrate 21, wherein the P-type substrate 21 is a P-type SiC substrate, and an Al (aluminum) doped P-type SiC substrate is selected (the carrier concentration is controlled at 1×10 18 cm -3 -1×10 20 cm -3 range, preferably, the carrier concentration is controlled within 1x10 19 -4x 10 19 cm-3 range), which can improve the heat dissipation capacity of the device, inhibit the self-heating effect, and increase the device operating temperature and high-temperature reliability;

[0068] Optionally, it may be a P-type SiC substrate co-doped with Al (aluminum) and B (boron), a P-type SiC substrate co-doped with Al (aluminum) and N (nitrogen), or a P-type SiC substrate co-doped with Al (aluminum) and P (phosphorus).

[0069] refer to Figure 5 , a plasma enhanced PEALD process is used to grow a bonding intermediate layer 23 on the surface of the first substrate 21. The PEALD process specifically controls the growth temperature at 350°C, uses trimethylaluminum (Me3Al, TMA) and ozone O3 as reaction precursors, grows a 10-40nm α-Al2O3 layer (corundum type crystal structure) as the bonding intermediate layer 23, and performs nitrogen high temperature annealing to activate the injected ions to facilitate subsequent transfer. The α-Al2O3 layer grown by the ozone enhanced PEALD process is conducive to improving the transfer effect of the film, improving the film quality and bonding effect.

[0070] Step 4: Reference Figure 6 After completing step 3, the "universal ion knife" intelligent stripping and transfer technology is used to transfer the β-Ga2O3 with a thickness of about 300-800nm ​​to the P-type substrate 21 to form the following SOI-like structure wafers: β-Ga2O3 / Al2O3 / 4H-SiC, β-Ga2O3 / Al2O3 / 6H-SiC, β-Ga2O3 / Al2O3 / 3C-SiC.

[0071] Step 5: Reference Figure 7 , the β-Ga2O3 layer 24 of the heterogeneous integrated substrate 20 prepared in step 4 is thinned by ICP etching, RIE etching, CMP polishing or wet etching (using hydrofluoric acid HF) to control the thickness of the β-Ga2O3 film to be less than or equal to 100nm. Preferably, the thickness of the β-Ga2O3 film is between 60-100nm, and the thickness can be tested by ellipsometry or step profiler. Using a thicker β-Ga2O3 layer in the transfer process and thinning it in subsequent steps can, on the one hand, reduce the difficulty of transferring an overly thin β-Ga2O3 layer, and on the other hand, can remove surface defects that may exist or be generated on the surface of the original β-Ga2O3 layer by subsequent thinning to improve the surface quality and flatness of the material, and this process can also be applied to different β-Ga2O3 layer thickness requirements under different performance requirements.

[0072] Then, magnetron sputtering metal combined with high-temperature annealing is used to realize ohmic contact electrodes on the heterogeneous integrated substrate to form an electrode cathode 10. The specific metal and annealing method used are related to the substrate material selected in step 4. For example, when SiC is used as the first substrate 21, metal tungsten (W) or metal nickel (Ni) can be used to prepare the metal cathode 10 and high-temperature annealing is performed at 1000°C and nitrogen (N2) atmosphere for 3-5 minutes. The material of the metal cathode 10 is selected from Au, Al, Ti, Sn, Ge, In, Ni, Co, Pt, W, Mo, Cr, Cu, Pb or any combination of alloys thereof or any combination of stacked layers thereof or conductive compounds ITO, AZO, FTO.

[0073] The ICP etching or RIE etching can be selected with different mixed gas atmospheres such as Cl2, BCl3, Ar, Cl2 / BCl3, Cl2 / Ar / BCl3 with a purity of 99.999% by mass, the mixing ratio can be 35:5 or 30:5, the ICP power is 300-900W, the RF power is 15-100W, and the etching temperature can be selected from room temperature to 80°C. Under this working condition, β-Ga2O3 can be stably and uniformly etched. The wet etching process can be selected under different solution conditions such as 10%-50% HF (room temperature), 40%-70% HNO3 (60°C), 80%-85% H3PO4 (80°C), KOH (95°C combined with 254nmHg lamp ultraviolet light) to stably and uniformly etch β-Ga2O3.

[0074] Step 6: The surface of the heterogeneous integrated substrate 20 obtained after the treatment in step 5 is subjected to ion bombardment for 5-20 minutes under the action of O plasma using a plasma glue machine to clean surface impurities. The plasma bombardment power range may be 200-400W.

[0075] Optionally, the cleaning process used in step 6 can be a combination of organic cleaning and inorganic cleaning. More preferably, the cleaning process uses organic cleaning first and then inorganic cleaning. The cleaning process can refer to the operating steps of organic cleaning and inorganic cleaning of the P-type substrate 21 in step 1, and will not be elaborated here.

[0076] Optionally, the heterogeneous integrated substrate 20 obtained in step 6 is subjected to ultraviolet ozone passivation treatment. The process uses a high-intensity ultraviolet lamp source with a wavelength of 185nm or 254nm, combined with an O3 atmosphere, the treatment time can be selected to be 15-30min, and the treatment temperature can be 25-200°C; in some preferred embodiments, the treatment temperature is 100-150°C, which can better suppress oxygen vacancies, regulate the quality of the film to be better and the crystal structure to be more orderly;

[0077] It should be noted that the step 6 adopts organic cleaning first and then inorganic cleaning, combined with ultraviolet ozone passivation treatment of the cleaned heterogeneous integrated substrate 20, can better remove OH-, H+ and organic matter attached by inorganic cleaning, while inhibiting oxygen vacancies, so as to better improve the quality of gallium oxide film.

[0078] Step 7: Reference Figure 8 The heterogeneous integrated substrate 20 prepared by cleaning in step 6 is grown with a halide vapor phase epitaxy (HVPE) device to form a 6 μm thick, non-intentionally doped UID β-Ga2O3 layer (buffer N-type layer 31), and the carrier concentration is controlled at 5×10 13 cm -3 -5×10 15 cm -3 Range. The growth temperature of HVPE can be selected from 700-1000°C, using high-purity gallium chloride GaCl (≥99.9999%) as the Ga precursor source, high-purity ozone O3 (≥99.999%) as the O precursor source, and high-purity argon Ar (≥99.999%) or nitrogen N2 (≥99.999%) as the inert carrier gas. Oxygen O2 can also be used as a substitute for the O precursor source. The grown sample is subjected to high-temperature annealing in an ozone atmosphere at 600-800 degrees Celsius for 20-60 minutes to further optimize the film quality of the buffer N-type layer 31, suppress the oxygen vacancy concentration, and achieve a lower carrier concentration and better film quality.

[0079] Optionally, the buffer N-type layer 31 obtained in step 7 is subjected to UV-ozone passivation treatment. The process uses a high-intensity UV lamp source with a wavelength of 185nm or 254nm, combined with an O3 atmosphere, the treatment time can be selected as 15-30min, and the treatment temperature can be 25-200°C; in some preferred embodiments, the treatment temperature is 100-150°C.

[0080] The growth process of step 7 can also be replaced by MOCVD or PLD process, but the film quality is reduced after replacement, and the growth rate and thickness of the film are difficult to control. The above processes all use a mixed gas atmosphere of O2 and Ar. The HVPE process can use a growth temperature of 650-800°C, the MOCVD process can use a growth temperature of 700-800°C and use metal gallium as the gallium source and ozone as the oxygen source, and the PLD process can use a growth temperature of 500-800°C.

[0081] Step 8: Reference Fig. 9 , a 300-500nm Si-doped N-type β-Ga2O3 layer (N + The epitaxial layer 32) is doped at a concentration of 1×10 18 cm-3 -1×10 20 cm -3 range, the doping elements can be replaced by Sn and Ge.

[0082] The growth process of step 8 can be replaced by LPCVD process, MOCVD process or PLD process, but the quality of the grown film is reduced after the replacement, and the growth rate and thickness of the film are difficult to control. The above processes all use a mixed gas atmosphere of O2 and Ar. The MBE process can use a growth temperature of 650-800°C, the CVD process can use a growth temperature of 700-800°C and metal gallium as the gallium source and ozone as the oxygen source, and the PLD process can use a growth temperature of 500-800°C.

[0083] Step 9: After completing step 8 + After the growth of the epitaxial layer 32, the sample is subjected to high temperature slow annealing to improve the epitaxial film and adjust the oxygen vacancy concentration of the film. The annealing temperature can be selected in the range of 600-800°C, the duration is 20min-60min, and the annealing atmosphere can be selected from ozone (O3) or oxygen (O2) gas, or nitrogen (N2) / argon (Ar) gas, where O3 is the optimal gas atmosphere condition.

[0084] In a preferred embodiment, the annealing treatment in step 9 can also be followed by an ultraviolet ozone treatment (UV / O3) process to further improve the epitaxial quality and regulate the oxygen vacancy concentration. The process uses a high-intensity ultraviolet light source with a wavelength of 185nm or 254nm, combined with an O3 atmosphere, the treatment time can be selected to be 15-30min, and the treatment temperature can be 25-200°C; in some preferred embodiments, the treatment temperature is 100-150°C.

[0085] Step 10: Reference Fig.10 , after completing step 9 of N + After the epitaxial layer 32 is annealed, + The upper surface of the epitaxial layer 32 is etched using a photolithography mask plate I 50 and a positive photoresist as a mask. The sample is then placed in a plasma etcher and dry etching ICP or RIE technology is used to etch and form the required first inclined surface 20a and second inclined surface 30a.

[0086] The ICP etching or RIE etching used to form the inclined surface can use a mixed gas atmosphere of BCl3 / Ar or Cl2 / Ar / BCl3 with a purity of 99.999% by mass, and the mixing ratio is controlled in the range of 35:5-50:1, or 1:1:6-1:1:8, the ICP power is 540-760W, the RF power is 35-70W, and the etching temperature can be selected to be 45-85°C. By adjusting the above-mentioned appropriate etching gas ratio, etching power, and etching temperature, the physical reaction in dry etching can be suppressed, and the chemical reaction in dry etching can be strengthened, thereby realizing an inclined surface with a certain slope, with a positive bevel angle greater than 60° and less than 70°.

[0087] Preferably, the positive bevel angle θ is less than or equal to 68° and greater than or equal to 64°.

[0088] Step 11: After completing step 10 to form the inclined surface, the sample is subjected to surface passivation treatment based on ozone (O3). This process can be implemented using ICP etching equipment or ultraviolet ozone cleaning machine, and an O3 gas atmosphere with a mass percentage purity of 99.999% is selected. The power of ICP or ultraviolet ozone cleaning machine is controlled at 200-400W and 20-30W respectively, the process temperature is controlled at 45-60°C, and the processing time is 20-40min. The ozone passivation process can effectively regulate the film quality and oxygen vacancy concentration of the Ga2O3 epitaxial layer, thereby suppressing defects and improving the device performance of the diode.

[0089] Step 12: Reference Fig.11 , using physical mask I 60, in N + A metal anode 40 , specifically metal Ni, is grown on the epitaxial layer 32 by magnetron sputtering.

[0090] After completing step 12, the magnetron sputtering process is used to grow the metal anode Ni by magnetron sputtering using a physical mask I 60. The sputtering target material is nickel with a mass purity of >99.99%, and Ar with a mass purity of 99.999% is used as a sputtering carrier gas to pass into the sputtering chamber. Before sputtering, the magnetron sputtering equipment chamber is cleaned with high-purity Ar for 5-10 minutes and then evacuated. At a vacuum degree of 6×10 -4 -1.3×10 -3 Pa, argon flow rate is 20-30cm 3 Under the conditions of 100W / s, target substrate distance of 10cm and working power of 20W-100W, anode nickel is prepared with an electrode thickness of 200-300nm.

[0091] The metal of the anode can be selected from different elements such as Au, Al, Ti, Ni, Pt, Cr and their 2-4 layer structure. For example, the first layer uses 2-4nm Ti or Cr to improve metal adhesion, and the remaining layers use elements such as Au, Pt, Ni with high metal work function to increase the turn-on voltage, or use transparent conductive materials such as ITO\FTO\AZO to reduce contact resistance. Among them, Au\Ag\Pt has stable chemical properties; Al\Ti\Ni has low cost.

[0092] Comparative Example 1

[0093] The difference from Example 1 is that no inclined surface is provided and the ozone passivation treatment step 11 is not performed.

[0094] The breakdown voltage V of the heterojunction diode provided in Comparative Example 1 is br About 435V;

[0095] The breakdown voltage V of the heterojunction diode prepared in Example 1 of the present application is br =1.32kV-1.91kV, the overall BFOM of the device is about the best at 1.44GW / cm 2 , the withstand voltage is increased by 3.03-4.4 times, the BFOM is increased by 9.18-19.36 times, and the terminal withstand voltage efficiency is increased by 70-90%. It will not have a negative impact on the conduction characteristics and conduction resistance.

[0096] In addition, the present application performs breakdown voltage tests for different positive bevel angles θ, and the results are shown in the following table:

[0097] Table 1

[0098] Positive bevel 0 30 35 40 45 50 55 60 <![CDATA[V br (V)]]> 434.9 718.4 778.6 818.6 826.4 961.7 1135 1319 Positive bevel 64 65 66 68 69 70 75 80 <![CDATA[V br (V)]]> 1821 1846 1919 1856 1774 1770 1480 1217

[0099] It can be seen that the breakdown voltage of the device with a positive bevel angle θ of 64°-68° can reach over 1800V.

[0100] In addition, those skilled in the art should understand that, although there are many problems in the prior art, each embodiment or technical solution of the present invention can be improved in only one or several aspects, without having to solve all the technical problems listed in the prior art or background technology at the same time. Those skilled in the art should understand that the content not mentioned in a claim should not be used as a limitation on the claim.

[0101] Although this article uses more metal cathodes, heterogeneous integrated substrates, P-type substrates, bonding intermediate layers, β-Ga2O3 layers, ion implantation layers, semiconductor layers, buffer N-type layers, N +The terms epitaxial layer, metal anode, photolithography mask I, physical mask I, etc. are used, but the possibility of using other terms is not excluded. These terms are used only to more conveniently describe and explain the essence of the present invention; interpreting them as any additional restrictions is contrary to the spirit of the present invention; the terms "first", "second", etc. (if any) in the description and claims of the embodiments of the present invention and the above drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence.

[0102] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a heterojunction diode, characterized in that: The method comprises the following preparation steps: Providing a P-type substrate; forming a bonding intermediate layer having a corundum type crystal structure on the upper surface of the P-type substrate; Providing a β-Ga2O3 layer, the β-Ga2O3 layer having a first surface and a second surface; Performing ion implantation on the second surface of the β-Ga2O3 layer; Transferring the β-Ga2O3 layer to the bonding intermediate layer so that the second surface of the β-Ga2O3 layer contacts the upper surface of the bonding intermediate layer to form a heterogeneous integrated substrate; A semiconductor layer is formed on the upper surface of the heterogeneous integrated substrate, wherein the semiconductor layer includes a buffer N-type layer and an N + Epitaxial layer; When viewed from above, the heterojunction diode is circular, and etching causes the circular side walls of the heterogeneous integrated substrate and the semiconductor layer to tilt toward the inside of the heterojunction diode to form an inclined surface, and the positive bevel angle θ of the inclined surface is less than 70° and greater than or equal to 60°; Performing ozone passivation treatment on the semiconductor layer; forming a metal anode on the upper surface of the semiconductor layer; Optionally, after forming the heterogeneous integrated substrate, a metal cathode is formed on the lower surface of the heterogeneous integrated substrate.

2. The method for preparing a heterojunction diode according to claim 1, characterized in that: The P-type substrate is a P-type SiC substrate; Preferably, the thickness of the P-type substrate is 2 μm-100 μm; Preferably, the ion types implanted on the upper surface of the β-Ga2O3 layer include hydrogen, iron or magnesium, and the implantation angle is 7°; Preferably, the method further comprises, after completing the ion implantation of the second surface, bombarding the surface of the ion implantation layer with Ar ions; Preferably, the thickness of the β-Ga2O3 layer is 60-100 nm.

3. The method for preparing a heterojunction diode according to claim 1, characterized in that: Forming the bonding intermediate layer includes: PEALD deposition; Preferably, the PEALD deposition includes forming the bonding intermediate layer at a certain temperature using trimethylaluminum and ozone as reaction precursors; Preferably, the thickness of the bonding intermediate layer is 10-40 nm.

4. The method for preparing a heterojunction diode according to claim 1, characterized in that: The material of the buffer N-type layer is an unintentionally doped UID β-Ga2O3 layer; Preferably, the thickness of the buffer N-type layer is 6 μm, and the carrier concentration of the buffer N-type layer is 1×10 14 cm -3 -1×10 16 cm -3 .

5. The method for preparing a heterojunction diode according to claim 1, characterized in that: The N + The material of the epitaxial layer is β-Ga2O3 doped with any one or at least two of Sn, Si and Ge; Preferably, the N + The thickness of the epitaxial layer is 300-500nm. + The carrier concentration of the epitaxial layer is 1×10 18 cm -3 -1×10 20 cm -3 .

6. The method for preparing a heterojunction diode according to claim 1, characterized in that: After forming the semiconductor layer, performing annealing treatment on the semiconductor layer; Preferably, the annealing temperature of the annealing treatment is 500-700° C., the annealing time is 20-60 min, and the annealing atmosphere is selected from any one of ozone, oxygen, nitrogen, and argon, or a combination of at least two of them.

7. The method for preparing a heterojunction diode according to claim 6, characterized in that: After the annealing treatment is completed, ultraviolet ozone treatment is performed; Preferably, the wavelength of the ultraviolet lamp source for the ultraviolet ozone treatment is 185nm or 254nm, the ultraviolet ozone treatment time is 15-30min, and the ultraviolet ozone treatment temperature is 25-200°C.

8. The method for preparing a heterojunction diode according to claim 1, characterized in that: The oxygen-based passivation treatment includes: performing a surface passivation treatment based on ozone, oxygen or oxygen plasma on the product after the inclined surface is formed.

9. The method for preparing a heterojunction diode according to claim 1, characterized in that: The thickness of the metal cathode is 200-300nm; The material of the metal cathode is selected from Au, Al, Ti, Sn, Ge, In, Ni, Co, Pt, W, Mo, Cr, Cu, Pb or any combination of alloys thereof or any combination of laminates or conductive compounds thereof; and / or The thickness of the metal anode is 200-300nm; The material of the metal anode is selected from Au, Al, Ti, Sn, Ge, In, Ni, Co, Pt, W, Mo, Cr, Cu, Pb, or an alloy of any combination thereof, or a stack of any combination thereof, or a conductive compound.

10. A heterojunction diode prepared according to the preparation method according to any one of claims 1 to 9.