Solar cell and polishing and texturing method

By forming a second suede with a spaced pyramid structure on the back of the silicon wafer of the solar cell, and combining with a specific polishing and fleece making method, the problem of poor contact between the electrode and the polysilicon layer in the prior art is solved, and the solar cell is improved Photoelectric conversion efficiency and fill factor simplify the process flow.

CN119050179APending Publication Date: 2024-11-29HANGZHOU JINGBAO NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411144806.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing solar cell technology cannot meet the requirements of passivation and contact characteristics on the back of the battery at the same time, resulting in poor contact between the electrode and the polysilicon layer, affecting the photoelectric conversion efficiency.

Method used

A solar cell design is adopted in which the back of the silicon wafer forms a second suede with a spaced pyramid structure, and a specific polishing method is used to combine alkaline solutions and additives to control the number and size of the pyramids to achieve semi-polishing. Semi-suede microscopic surface, improving ohmic contact between the electrode and the silicon wafer.

Benefits of technology

While not reducing the passivation effect, the filling factor and photoelectric conversion efficiency of solar cells are significantly improved, and the process flow is simplified and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050179A_ABST
    Figure CN119050179A_ABST
Patent Text Reader

Abstract

The invention discloses a solar cell, and relates to the field of photovoltaic cells, the solar cell comprises a silicon substrate, the silicon substrate comprises a first suede and a second suede, and the first suede and the second suede are respectively arranged on the front surface and the back surface of the solar cell. A plurality of pyramid structures are formed on the first suede surface and the second suede surface, and gaps exist between tower footings of at least part of adjacent pyramid structures on the second suede surface. The invention further discloses a polishing and texturing method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of photovoltaic cells, in particular to a solar cell and a polishing and texturing method. Background Art

[0002] At present, solar cell technology forms the back structure by preparing a full-contact passivation film and a metal electrode on the back of the silicon wafer. Therefore, the morphology of the back of the silicon wafer has an important influence on the passivation and contact characteristics. At present, the back of the silicon wafer is mainly processed by the following technologies:

[0003] (1) Back side alkaline polishing: Use alkaline solution to form a flat mirror structure to achieve high reflectivity on the back side of the silicon wafer, increase the uniformity of the passivation contact structure, and improve the overall passivation quality. However, this back side morphology will reduce the actual contact between the electrode and the polysilicon layer, increase the contact resistance, and reduce the photoelectric conversion efficiency.

[0004] (2) Backside acid polishing: Use an acid solution to etch the silicon wafer. After being etched by the acid solution, the back side of the silicon wafer cannot achieve a good flat structure and has large surface defects, which limits the improvement of the photoelectric conversion efficiency. In addition, the process cost of nitric acid / hydrofluoric acid solution is high and the discharge treatment is not environmentally friendly.

[0005] (3) Back velvet: Growing a pyramid velvet on the back can improve the ohmic contact between the back electrode and the polysilicon layer, but at the same time it may lead to an increase in surface defects and affect the passivation effect.

[0006] The existing technology cannot simultaneously meet the requirements of the back passivation and contact characteristics of the battery. Therefore, it is an urgent problem to prepare a new type of solar cell that can meet the contact characteristics requirements between the metal and the substrate and the passivation contact requirements. Summary of the invention

[0007] The present invention aims to solve the technical problems in the related art to a certain extent. To this end, the present invention provides a solar cell and a polishing and texturing method.

[0008] As a first scheme of the present invention, a solar cell is provided, which includes a silicon substrate, the silicon substrate includes a first velvet surface and a second velvet surface, and the first velvet surface and the second velvet surface are respectively arranged on the front surface and the back surface of the solar cell, a plurality of pyramid structures are formed on the first velvet surface and the second velvet surface, and there is a gap between the bases of at least part of two adjacent pyramid structures on the second velvet surface.

[0009] Furthermore, the size of the pyramid base on the second velvet surface is between 0.1 microns and 2 microns.

[0010] Furthermore, the size of the pyramid base on the first velvet surface is between 0.5 microns and 3 microns.

[0011] As a second solution of the present invention, a polishing and texturing method is provided, comprising:

[0012] The alkaline solution is mixed with an additive to obtain a polishing and texturing solution, wherein the additive comprises:

[0013] 0.5wt% to 5.0wt% of a polishing accelerator, wherein the polishing accelerator comprises an oxidizing agent;

[0014] Velvet nucleating agent 0.01wt% to 0.5wt%;

[0015] A silicon wafer is placed in the polishing and texturing liquid to obtain a silicon substrate, wherein the silicon substrate includes a first texture surface and a second texture surface, and the first texture surface and the second texture surface are respectively arranged on the front surface and the back surface of the solar cell, and multiple pyramid structures are formed on the first texture surface and the second texture surface, and there is a gap between the bases of at least part of two adjacent pyramid structures on the second texture surface.

[0016] Furthermore, before placing the silicon wafer in the polishing and texturing liquid, the method further comprises:

[0017] Placing the initial silicon wafer in a texturing solution to obtain a first silicon substrate;

[0018] performing phosphorus diffusion or boron diffusion on the first silicon substrate to obtain a second silicon substrate;

[0019] The second silicon substrate is back-etched to obtain the silicon wafer.

[0020] Furthermore, the polishing accelerator is selected from at least one of peroxide, persulfate, iodate, hypoiodite, periodate, peracetic acid and potassium permanganate, and the velvet nucleating agent is selected from at least one of carboxymethyl-modified pullulan, carboxymethyl-modified cyclodextrin, methyl-modified cyclodextrin, methyl-modified lignin sulfonate and carboxymethyl-modified starch.

[0021] Furthermore, the additive also includes a defoaming agent, and the content of the defoaming agent in the additive is between 0.5wt% and 5wt%.

[0022] Furthermore, the content of alkali in the alkaline solution is between 0.5wt% and 2.0wt%, and the mass ratio of the additive to the alkaline solution is between 0.2:100 and 2:100.

[0023] Furthermore, the silicon wafer is placed in the polishing and texturing liquid for a period of 2 minutes to 5 minutes.

[0024] Furthermore, the temperature of placing the silicon wafer in the polishing and texturing liquid is between 55°C and 85°C.

[0025] The present invention has the following beneficial effects: there are gaps between adjacent pyramid structures on the upper part of the second velvet surface of the solar cell of the present invention, and this velvet surface structure can significantly improve the ohmic contact between the silicon wafer and the electrode without reducing the normal passivation effect, so that the solar cell can obtain a higher fill factor and photoelectric conversion efficiency.

[0026] At the same time, the present invention provides a polishing and texturing method, which is simple and easy to implement. By using additives containing specific components, the number and size of pyramids on the surface of the silicon wafer can be controlled, and the polishing and texturing processes can be carried out together, greatly shortening the time and process costs.

[0027] These features and advantages of the present invention will be disclosed in detail in the following specific embodiments and drawings. The best embodiments or means of the present invention will be described in detail in conjunction with the drawings, but they are not intended to limit the technical solutions of the present invention. In addition, there are multiple features, elements, and components that appear in each of the following texts and drawings, and different symbols or numbers are marked for convenience, but they all represent components with the same or similar structures or functions. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0029] Figure 1 It is a structural schematic diagram of an embodiment of a solar cell provided by the present invention;

[0030] Figure 2 It is a flow chart of an implementation method of the polishing and texturing method provided by the present invention;

[0031] Figure 3 This is a scanning electron microscope (SEM) photograph of an embodiment of the first velvet surface of a solar cell of the present invention;

[0032] FIG4( a ) is a SEM photograph of the second velvet surface on the silicon wafer surface of Example 1 at a magnification of 20 thousand times;

[0033] FIG4( b ) is a SEM photograph of the second textured surface of the silicon wafer of Example 1 at a magnification of 2,000 times;

[0034] FIG5( a ) is a SEM photograph of the second textured surface of the silicon wafer of Example 2 at a magnification of 20 thousand times;

[0035] FIG5( b ) is a SEM photograph of the second textured surface of the silicon wafer of Example 2 at a magnification of 2,000 times;

[0036] FIG6( a ) is a SEM photograph of the second textured surface of the silicon wafer of Example 3 at a magnification of 20 thousand times;

[0037] FIG6( b ) is a SEM photograph of the second textured surface of the silicon wafer of Example 3 at a magnification of 2,000 times.

[0038] Description of Reference Numerals

[0039] 11: Silicon substrate

[0040] 12: First suede

[0041] 13: Second suede DETAILED DESCRIPTION

[0042] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments in the implementation manner are intended to be used to explain the present invention and should not be construed as limiting the present invention.

[0043] References to "one embodiment" or "an example" or "an example" in this specification mean that a particular feature, structure, or characteristic described in conjunction with the embodiment itself may be included in at least one embodiment disclosed in the present application. The appearance of the phrase "in one embodiment" in various places in the specification does not necessarily refer to the same embodiment.

[0044] As a first aspect of the present invention, a solar cell is provided. Figure 1 As shown, the solar cell 1 includes a silicon substrate 11, and the silicon substrate 11 includes a first velvet surface 12 and a second velvet surface 13, and the first velvet surface 12 and the second velvet surface 13 are respectively arranged on the front and back sides of the silicon wafer, and a plurality of pyramid structures are formed on the first velvet surface 12 and the second velvet surface 13. For all the pyramid structures on the first velvet surface 12, the bases of two adjacent pyramid structures are in contact with each other, and for at least part of the pyramid structures on the second velvet surface 13, there is a gap between the bases of two adjacent pyramid structures.

[0045] The first velvet surface is arranged on the front side of the silicon wafer, which refers to the light-receiving side of the solar cell, also called the front side, and the second velvet surface is arranged on the back side of the silicon wafer, which refers to the non-light-receiving side of the solar cell, also called the back side.

[0046] The present invention does not specifically limit the number and distribution of the pyramid structures of the second velvet surface, and only needs to satisfy that there are intervals between the tower bases of at least some of the pyramid structures. In some embodiments, the pyramid structures are distributed on the second velvet surface over the entire surface, and there are interval areas between all adjacent pyramid structure tower bases, and the sizes of the multiple interval areas are not completely the same; in other embodiments, the pyramid structures are evenly distributed on the second velvet surface, and the sizes of the multiple interval areas are the same.

[0047] The present invention does not specifically limit how to obtain the silicon substrate. For example, the silicon substrate can be obtained by purchasing from outside. For another example, the silicon substrate can be obtained by a preparation method.

[0048] The present invention does not specifically limit the type of solar cell including the second velvet surface, and only needs to satisfy that a passivation layer and a back electrode are formed on the back of the cell. For example, the solar cell can be a tunnel oxide passivated contact cell (TOPCon), an intrinsic thin film heterojunction cell (HJT), an emitter and back passivated cell (PERC) and is not limited to a crystalline silicon cell, but can also be a stacked cell using the above cells, such as a perovskite stacked cell.

[0049] In the present invention, the surface roughness of the area with the pyramid structure on the second velvet surface is relatively large. When the passivation film is deposited in the area with the pyramid structure, the contact area with the metal electrode is larger, thereby enhancing the bonding ability between the metal in this area and the silicon wafer, thereby making the metal and the silicon wafer have better ohmic contact.

[0050] In the present invention, there are spacing areas between the bases of some adjacent pyramid structures, and the microscopic surface of the spacing area is flat and smooth. As shown in Figure 4(a), the silicon wafer reacts in the polishing and texturing liquid to form a polishing surface and a texturing surface at the same time. There is a spacing between at least some of the pyramid texturing surfaces. Compared with the texturing surface, the subsequent passivation film deposition growth on such a semi-polished and semi-textured microscopic surface can obtain better deposition uniformity, high density and higher quality passivation film, thereby improving the passivation effect of the film on surface defects, reducing the recombination loss of carriers on the battery surface, thereby improving the conversion efficiency of the solar cell; compared with the pure polishing surface, the direct ohmic contact between the silicon wafer and the electrode on such a semi-polished and semi-textured microscopic surface is improved due to the presence of small pyramids, thereby improving the filling factor and conversion efficiency of the solar cell.

[0051] The structure of the second velvet surface can significantly improve the ohmic contact between the silicon wafer and the back electrode without reducing the normal passivation effect, so that the solar cell can obtain a higher fill factor and photoelectric conversion efficiency.

[0052] In the embodiment of the present invention, the overall structure of the solar cell is not particularly limited. As an optional embodiment, the solar cell further includes a silicon dioxide layer, a polysilicon layer and a silicon nitride layer stacked in sequence on the back side of the silicon substrate, and the solar cell further includes a heavily doped layer and a silicon nitride layer stacked in sequence on the front side of the silicon substrate. As another optional embodiment, the solar cell further includes an aluminum oxide layer and a silicon nitride layer stacked in sequence on the back side of the silicon substrate, and the solar cell further includes a heavily doped layer and a silicon nitride layer stacked in sequence on the front side of the silicon substrate.

[0053] The present invention does not impose any special limitation on the size of the bases of the multiple pyramid structures on the second velvet surface. The function of the pyramid structures on the back side is to provide more contact area with the metal to improve the ohmic performance. However, a larger-sized pyramid will lead to a decrease in flatness and thus reduce the passivation performance. At this time, the existence of the smooth spacing area compensates for the decrease in passivation performance caused by the pyramid. The combination of the pyramid structure and the spacing area enables the solar cell to significantly improve the ohmic contact performance while ensuring sufficient passivation performance. In other embodiments, the base sizes may also be exactly the same.

[0054] Preferably, the size of the pyramid bases on the second velvet surface is between 0.1 microns and 2 microns, and the size of the pyramid bases on the first velvet surface is between 0.5 microns and 3 microns.

[0055] The overall pyramid base size of the second velvet surface of the present invention is smaller than that of the first velvet surface, which has less impact on the surface flatness of the silicon wafer, thereby reducing the passivation performance of the solar cell.

[0056] As a second aspect of the present invention, a polishing and texturing method is provided, comprising:

[0057] The alkaline solution is mixed with an additive to obtain a polishing and texturing solution, wherein the additive comprises:

[0058] 0.5wt% to 5.0wt% of a polishing accelerator, wherein the polishing accelerator comprises an oxidizing agent;

[0059] Velvet nucleating agent 0.01wt% to 0.5wt%;

[0060] The silicon wafer is placed in the above-mentioned polishing and texturing liquid to obtain the silicon substrate of the above-mentioned solar cell. The silicon substrate includes a first textured surface and a second textured surface, and the first textured surface and the second textured surface are respectively arranged on the front surface and the back surface of the solar cell. A plurality of pyramid structures are formed on the first textured surface and the second textured surface, and there is a gap between the bases of at least part of two adjacent pyramid structures on the second textured surface.

[0061] Before placing the silicon wafer in the polishing and texturing liquid, the method further comprises:

[0062] Placing the initial silicon wafer in a texturing solution to obtain a first silicon substrate;

[0063] performing phosphorus diffusion or boron diffusion on the first silicon substrate to obtain a second silicon substrate;

[0064] The second silicon substrate is back-etched to obtain the silicon wafer.

[0065] As a specific embodiment of the polishing and velveting method of the present invention, Figure 2 As shown, including:

[0066] In step S110, the initial silicon wafer is placed in a conventional texturing liquid for double-sided texturing to obtain a first silicon substrate having pyramid structures on both sides.

[0067] In step S120, the first silicon substrate obtained in step S110 is placed in a tubular diffusion furnace for phosphorus diffusion or boron diffusion to obtain a second silicon substrate. The present invention does not specifically limit the specific process conditions for phosphorus diffusion or boron diffusion.

[0068] In step S130, the oxide layer formed on the back side of the second silicon substrate obtained in step S120 due to diffusion is removed and the front oxide layer is retained to obtain a silicon wafer. The present invention does not specifically limit the method for removing the oxide layer.

[0069] In step S140, an alkaline solution is mixed with a polishing and texturing additive to obtain a polishing and texturing liquid, wherein the additive includes: 0.5wt% to 5.0wt% of a polishing accelerator, the polishing accelerator includes an oxidant; 0.05wt% to 0.5wt% of a texturing nucleating agent, and the silicon wafer obtained in step S130 is placed in the above-mentioned polishing and texturing liquid to obtain the silicon substrate of the above-mentioned solar cell, the silicon substrate includes a first texturing surface and a second texturing surface, and the first texturing surface and the second texturing surface are respectively arranged on the front surface and the back surface of the solar cell, a plurality of pyramid structures are formed on the first texturing surface and the second texturing surface, and there is a gap between the bases of at least part of two adjacent pyramid structures on the second texturing surface.

[0070] Compared with the traditional polishing or texturing process, the process of the present invention is simple and easy to implement. The present invention can perform polishing and texturing at the same time, which shortens the time and process cost. Moreover, the equipment used in the present invention only needs an alkaline polishing tank and is compatible with the existing battery production line.

[0071] The polishing accelerator acts as an oxidant during the alkaline polishing process. In a low-concentration alkaline solution, the oxidant can form an oxide film with weak bonding force on the surface of the silicon wafer, protecting the alkaline solution from local corrosion on the surface of the silicon wafer, and can effectively reduce the corrosion rate of the alkaline solution on the silicon wafer. Under the combined action of the oxidative protection of the oxidant and the corrosion of the alkaline solution, the entire surface will eventually tend to be flat and smooth, and the surface of the silicon wafer can achieve a high-quality overall flattening effect. The polishing accelerator is required to react with the silicon wafer to form an oxide film, and can be slightly corroded by the alkaline solution, and does not react with other chemical components.

[0072] As an optional embodiment, the polishing accelerator is selected from at least one of peroxide, persulfate, iodate, hypoiodite, periodate, peracetic acid and potassium permanganate.

[0073] After the velvet nucleating agent comes into contact with the surface of the silicon wafer, it can be quickly adsorbed on the surface of the silicon wafer and serve as the nucleation points for velvet. These nucleation points are evenly dispersed on the surface of the silicon wafer, regulating the corrosion rate of the alkaline solution on each crystal plane of the silicon surface, and serve as the base point for forming the pyramid morphology in the subsequent reaction. The nucleating agent is evenly distributed in the additive, helping the silicon wafer surface to achieve a uniform velvet effect. By controlling the concentration and proportion of this component, the size and uniformity of the pyramid can be regulated.

[0074] As an optional embodiment, the velvet nucleating agent is selected from at least one of carboxymethyl-modified pullulan, carboxymethyl-modified cyclodextrin, methyl-modified cyclodextrin, methyl-modified lignin sulfonate and carboxymethyl-modified starch.

[0075] The additive further comprises a defoaming agent, and the content of the defoaming agent in the additive is between 0.5wt% and 5wt%.

[0076] A large number of bubbles will be generated during the polishing and texturing reaction process. The degassing agent can change the surface tension of the polishing tank liquid, increase the wettability of the silicon wafer, and help the bubbles and silicon-containing products generated by the reaction to quickly leave the surface of the silicon wafer, thereby preventing bubble marks from being left on the surface of the silicon wafer. At the same time, the degassing agent helps the bubbles and silicon-containing by-products to quickly leave the surface of the silicon wafer, thereby promoting the contact reaction rate between silicon and the alkaline solution, and obtaining a small and uniform pyramid structure, thereby improving the quality of the prepared velvet structure.

[0077] As an optional embodiment, the defoaming agent is selected from at least one of a cationic quaternary ammonium salt surfactant and a water-soluble polysaccharide.

[0078] The present invention does not specifically limit the composition of the alkaline solution. In some embodiments, the alkali in the alkaline solution may include at least one of sodium hydroxide, sodium hydroxide, sodium methoxide, sodium ethoxide, and tetramethylammonium hydroxide. In addition, the choice of the alkaline solution can be determined according to the solution used in the production line, and no additional purchase is required, saving procurement costs.

[0079] The content of alkali in the alkaline solution is between 0.5wt% and 2.0wt%, and the mass ratio of the additive to the alkaline solution is between 0.2:100 and 2:100. In some embodiments, by adjusting the proportion of the additive in the alkaline solution, not only the desired proportion of the pyramid structure to the silicon wafer surface can be obtained, but also the size and uniformity of the pyramid structure can be regulated.

[0080] The cleaned incoming material is placed in the polishing and texturing liquid for 2 minutes to 5 minutes, and the temperature of the polishing and texturing liquid is between 55°C and 85°C. Polishing and texturing under short-time and low-temperature conditions can avoid the formation of excessive and large-sized pyramids, and prevent the significant reduction of passivation performance. The pyramid structure tower base size formed by the present invention is small, the surface flatness and passivation characteristics of the silicon wafer are less affected, and the pyramid structure and the locally smooth microscopic area are formed on the surface of the silicon wafer in a short time, shortening the process time and saving the process operation cost.

[0081] The present invention is further described in detail below by way of examples.

[0082] Example

[0083] Example 1

[0084] A method for processing a silicon substrate, comprising:

[0085] First, immerse the pre-cleaned silicon substrate in a texturing liquid for double-sided texturing. The concentration of NaOH in the texturing liquid is 1%, the concentration of the texturing additive is 0.5%, the temperature of the texturing liquid is 80°C, and the texturing time is 420S. After the texturing process, the silicon substrate is cleaned and dried. The dried silicon substrate is placed in a tubular diffusion furnace in the form of back-to-back inserts for boron diffusion. The diffusion temperature is 980°C and the time is 70 minutes. After the diffusion is completed, a heavily doped boron layer and a borosilicate glass oxide layer are formed on the front surface of the silicon substrate, and a small amount of a surrounding boron diffusion layer and a back oxide layer are formed on the back of the silicon substrate. The back oxide layer of the obtained silicon substrate is removed by a single-sided deoxidation process.

[0086] The alkaline solution is mixed with a polishing and texturing additive to obtain a polishing and texturing liquid, wherein the components in the additive include:

[0087] Polishing accelerator 0.5wt%;

[0088] Suede nucleating agent 0.01wt%;

[0089] Defoaming agent 0.5wt%;

[0090] The polishing accelerator is sodium persulfate, the velvet nucleating agent is carboxymethyl-modified pullulan, and the defoaming agent is polyquaternary ammonium salt;

[0091] The alkali of the alkaline solution is KOH, and the content of the alkali in the alkaline solution is 1.5wt%;

[0092] The mass ratio of the additive to the alkaline solution is 0.2:100, and a polishing texturing liquid is obtained.

[0093] The silicon substrate with the back oxide layer removed was immersed in the polishing and texturing solution, and reacted at 55° C. for 5 minutes. After the reaction, the silicon substrate was washed with deionized water and dried to obtain sample 1.

[0094] Example 2

[0095] The sample was prepared by the method provided in Example 1, except that the content of the velvet nucleating agent in the additive of Example 2 was 2 wt %, the polishing temperature was 85° C., and the reaction time was 2 min, to obtain Sample 2.

[0096] Example 3

[0097] The sample was prepared using the method provided in Example 1, except that the velvet nucleating agent in the additive of Example 3 was methyl-modified cyclodextrin, the content of the velvet polishing additive was 1 wt%, the polishing temperature was 70°C, and the reaction time was 3 min, to obtain Sample 3.

[0098] Example 4

[0099] The above sample is prepared into a complete solar cell, comprising the following steps:

[0100] (1) depositing a tunnel oxide layer with a thickness of 1.5±0.2 nm and a polysilicon layer with a thickness of 90 nm±10 nm on the back side of any of the above samples;

[0101] (2) Back side phosphorus diffusion;

[0102] (3) removing the front interference polysilicon layer and the front oxide layer;

[0103] (4) A 5 nm thick aluminum oxide layer was deposited on the front side by atomic layer deposition, and then an 80 nm thick silicon nitride layer was deposited by plasma enhanced chemical vapor deposition;

[0104] (5) Depositing a 100 nm silicon nitride layer on the back side using plasma enhanced chemical vapor deposition;

[0105] (6) Print silver paste electrodes on the front and back sides respectively and sinter them.

[0106] Get a solar cell.

[0107] Comparative Example 1

[0108] The comparative example is a TOPCon solar cell currently available on the market, the difference being that the back side of the comparative example is a TOPCon solar cell with a conventional back side polishing structure.

[0109] Test Case

[0110] The microstructure of the silicon wafer surface in the embodiment was obtained by using a Hitachi S4700 electron microscope. Figure 3 The SEM image of the first velvet surface on the front side of the silicon substrate of Sample 1 shows that the pyramids of the first velvet surface are closely arranged, and there is no gap between adjacent pyramids. Figure 4 (a) and Figure 4 (b) show SEM images of the second velvet surface on the back side of the silicon substrate of Sample 1 at different magnifications. It can be seen that there is a gap between the bases of some adjacent pyramid structures, and the surface of the gap area is flat and smooth. The velvet nucleating agent content of Sample 1 is 0.01wt%, and the number of nucleation sites of the pyramid structure on the back surface of the silicon wafer is small, and the number of pyramid structures that are subsequently formed and grown is small, while the area of ​​the flat and smooth gap area is larger.

[0111] (a) and (b) in Figure 5 are SEM photos of sample 2 at different magnifications. The content of suede nucleating agent is 2wt%, the reaction temperature is higher than that of sample 1, and the reaction time is shorter than that of sample 1. Sample 2 has a large number of nucleation sites for the pyramid structure formed on the back surface of the silicon wafer, and a large number of pyramid structures that are subsequently formed and grown, while the area of ​​the flat and smooth spacing area is smaller.

[0112] (a) and (b) in Figure 6 are SEM photos of sample 3 at different magnifications. The velvet nucleating agent is 1wt% methyl-modified cyclodextrin, the reaction temperature is higher than that of sample 1, and the reaction time is shorter than that of sample 1. Sample 3 has a large number of nucleation sites for the pyramid structure formed on the back surface of the silicon wafer, and a large number of pyramid structures that are subsequently formed and grown, while the area of ​​the flat and smooth spacing area is smaller.

[0113] Table 1 shows the electrical performance test data of the embodiments and comparative examples.

[0114] Embodiment 1, embodiment 2 and embodiment 3 all adopt the solar cell with the second velvet structure of the present invention, and the comparative example is a solar cell with a conventional back-side polishing structure. It can be seen from Table 1 that the open circuit voltage of the embodiment is lower than the open circuit voltage of the comparative example, the short circuit current density of the embodiment is higher than the short circuit current density of the comparative example, the series resistance of the embodiment is lower than the series resistance of the comparative example, the parallel resistance of the embodiment is lower than the parallel resistance of the comparative example, and the filling factor and conversion efficiency of the embodiment are higher than the filling factor and conversion efficiency of the comparative example;

[0115] Compared with Example 1, Example 2 has an increased content of the velvet nucleating agent, an increased polishing temperature, and a shorter reaction time. The electrical properties of Example 2 are better than those of Example 1.

[0116] In Example 3, the velvet nucleating agent is replaced with methyl-modified cyclodextrin, the content of the velvet nucleating agent is increased, the polishing temperature is increased, and the reaction time is shorter. The electrical properties of Example 3 are better than those of Example 1.

[0117] Table 1 Solar cell performance test comparison is as follows.

[0118]

[0119]

[0120] The open circuit voltage of the solar cell adopting the second velvet structure of the present invention is lower than that of the solar cell with a conventional back structure, the short circuit current density is higher than that of the solar cell with a conventional back structure, the series resistance and the parallel resistance are lower than that of the solar cell with a conventional back structure, the filling factor and the conversion efficiency are better than those of the solar cell with a conventional back structure. On the other hand, the addition of the velvet nucleating agent in the present invention is more conducive to the formation of the second velvet structure, thereby improving the electrical performance of the solar cell.

[0121] The above are only specific embodiments of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that the present invention includes but is not limited to the contents described in the drawings and the above specific embodiments. Any modification that does not deviate from the functional and structural principles of the present invention will be included in the scope of the claims.

Claims

1. A solar cell, comprising a silicon substrate (11), wherein the silicon substrate (11) comprises a first velvet surface (12) and a second velvet surface (13), wherein the first velvet surface (12) and the second velvet surface (13) are respectively arranged on the front surface and the back surface of the solar cell, and a plurality of pyramid structures are formed on the first velvet surface (12) and the second velvet surface (13), It is characterized in that At least part of the pyramid structures on the second velvet surface (13) have a gap between the bases of two adjacent pyramid structures.

2. The solar cell according to claim 1, It is characterized in that The size of the pyramid base on the second velvet surface (13) is between 0.1 micrometers and 2 micrometers.

3. The solar cell according to any one of claims 1 or 2, It is characterized in that The size of the pyramid base on the first velvet surface (12) is between 0.5 microns and 3 microns.

4. A polishing and velveting method, It is characterized in that include: The alkaline solution is mixed with an additive to obtain a polishing and texturing solution, wherein the additive comprises: 0.5wt% to 5.0wt% of a polishing accelerator, wherein the polishing accelerator comprises an oxidizing agent; Velvet nucleating agent 0.01wt% to 0.5wt%; A silicon wafer is placed in the polishing and texturing liquid to obtain a silicon substrate, wherein the silicon substrate includes a first textured surface and a second textured surface, and the first textured surface and the second textured surface are respectively arranged on the front surface and the back surface of the solar cell, and a plurality of pyramid structures are formed on the first textured surface and the second textured surface, and there are gaps between the bases of at least some adjacent pyramid structures on the second textured surface.

5. The polishing and texturing method according to claim 4, It is characterized in that Before placing the silicon wafer in the polishing and texturing liquid, the method further comprises: Placing the initial silicon wafer in a texturing solution to obtain a first silicon substrate; performing phosphorus diffusion or boron diffusion on the first silicon substrate to obtain a second silicon substrate; The second silicon substrate is back-etched to obtain the silicon wafer.

6. The polishing and texturing method according to claim 4, It is characterized in that The polishing accelerator is selected from at least one of peroxide, persulfate, iodate, hypoiodite, periodate, peracetic acid and potassium permanganate, and the velvet nucleating agent is selected from at least one of carboxymethyl-modified pullulan, carboxymethyl-modified cyclodextrin, methyl-modified cyclodextrin, methyl-modified lignin sulfonate and carboxymethyl-modified starch.

7. The polishing and texturing method according to claim 4, It is characterized in that The additive further comprises a defoaming agent, and the content of the defoaming agent in the additive is between 0.5wt% and 5wt%.

8. The polishing and texturing method according to claim 4, It is characterized in that The content of alkali in the alkaline solution is between 0.5wt% and 2.0wt%, and the mass ratio of the additive to the alkaline solution is between 0.2:100 and 2:

100.

9. The polishing and texturing method according to any one of claims 4 to 8, It is characterized in that The silicon wafer is placed in the polishing and texturing liquid for a period of 2 minutes to 5 minutes.

10. The polishing and texturing method according to any one of claims 4 to 8, It is characterized in that The silicon wafer is placed in the polishing and texturing liquid, and the temperature of the polishing and texturing liquid is between 55°C and 85°C.