Method for coating Prussian blue sodium battery positive electrode material by vapor deposition method and positive electrode material prepared by method

The vapor deposition method coats iron element nanoparticles on the surface of Prussian blue sodium electropositive electrode material, which solves the problems of low conductivity and water absorption of the material, improves the stability and rate performance of the electrochemical interface, and achieves a significant improvement in material performance. .

CN119050255APending Publication Date: 2024-11-29SHANDONG HAIHUA GRP CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411073777.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The Prussian blue sodium electropositive electrode material has low actual capacity, poor cycle stability and low inherent conductivity, which limits its wide application and it is difficult for the prior art to improve the stability and conductivity of the electrochemical interface at the same time.

Method used

The vapor deposition method is used to coat iron element nanoparticles on the surface of Prussian blue sodium electropositive electrode material to form a conductive layer, which improves the conductivity of the material and reduces water absorption. Fe(CO)5 is heated under a protective atmosphere to form Fe(CO) )5 The mixture is coated with air flow rate and temperature conditions.

Benefits of technology

Effectively improve the conductivity and electrochemical interface stability of the material, reduce water absorption, improve the circulation and rate performance of the material, avoid direct contact with the electrolyte and contact with the water in the air, and extend the service life of the material .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050255A_ABST
    Figure CN119050255A_ABST
Patent Text Reader

Abstract

The invention discloses a method for coating a Prussian blue sodium battery positive electrode material by a vapor deposition method and a positive electrode material prepared by the method, pentacarbonyl iron Fe (CO) 5 is used as a raw material, and the Prussian blue sodium battery positive electrode material coated and modified by an iron elementary substance is prepared by the vapor deposition method. Under the high-temperature gas-phase condition, the Prussian blue sodium battery positive electrode material is always kept in a dry state in the coating process, and the problems that more organic solvents and deionized water are needed for modification and secondary drying is needed by liquid-phase methods such as a solvothermal method or a hydrothermal method can be avoided. The elemental iron coating layer can isolate direct contact between water and an electrolyte and the Prussian blue sodium battery positive electrode material, the water absorption of the material is reduced, and the purpose of improving the conductivity and the interface stability of the material is achieved at the same time, so that the rate capability and the cycle performance of the material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion batteries, and specifically relates to a method for coating a Prussian blue sodium-ion positive electrode material by a vapor deposition method and a positive electrode material prepared by the method. Background Art

[0002] Sodium-ion batteries are considered to be one of the most promising energy storage systems for grid-scale applications due to their natural abundance of sodium, low cost, and safety. Prussian blue sodium cathode materials are considered to be one of the most promising cathode materials for sodium-ion batteries due to their high theoretical energy density, low cost, and simple preparation. However, their low actual capacity and poor cycle stability limit their widespread practical applications.

[0003] There are three main reasons for the poor performance of Prussian blue sodium cathode materials: ① Vacancies and crystal water in the crystals during the synthesis of the material cause poor structural stability; ② Electrochemical interface side reactions between Prussian blue sodium cathode materials and electrolytes cause poor interface stability; ③ The inherent conductivity of Prussian blue sodium cathode materials is relatively low, which makes the electrochemical reactivity kinetics weak, resulting in poor rate performance of the material. In response to the problems of vacancies and crystal water, the main means are concentrated on optimizing the bulk structure of the crystal. By adjusting and optimizing the synthesis method of the material, the crystal water and vacancies are reduced, thereby improving the integrity of the crystal structure, or by further adjusting the crystal element composition through element doping, the synergistic effect of multiple elements is exerted. Crystal water is inevitably present in the structure of Prussian blue sodium cathode materials, which can be removed by heat treatment under vacuum or protective atmosphere. However, the material that removes crystal water by heat treatment is also very easy to absorb water again when exposed to air again, resulting in poor processing performance and deterioration of electrochemical performance. The problems of interface stability and conductivity can be solved by surface coating modification.

[0004] CN113921798A, CN115411260A and CN114620758A etc. disclose technical solutions for coating oxides on the surface of Prussian blue sodium positive electrode materials. After coating the surface of Prussian blue sodium positive electrode materials with oxides, the material and electrolyte can be avoided, and the stability of the electrochemical reaction interface can be improved. In addition, the coating layer can also isolate the direct contact with water in the air and inhibit water absorption. The cycle performance of the material is improved after oxide coating. However, the conductivity of the coated oxide is extremely low, usually around 10 -6 to 10 -4 The low conductivity of the oxide cannot solve the problem of low inherent conductivity on the surface of Prussian blue sodium cathode materials. The wrapping on the surface of the material is not conducive to the transmission of electrons and affects the rate performance of the material.

[0005] In order to simultaneously solve the problems of poor electrochemical interface stability and low inherent conductivity of Prussian blue sodium cathode materials and improve the cycle performance and rate performance of the materials, it is necessary to find a coating modification material with higher conductivity for surface coating modification. Carbon materials have relatively high conductivity and good stability, and are relatively ideal coating modification materials, which are commonly used in surface modification of lithium iron phosphate materials. However, the density of carbon materials is relatively low. After coating modification, the bulk density of the material will be reduced, resulting in a decrease in the tap density of the material, which does not improve the volume energy density of sodium ion batteries. Metallic elements have extremely high electronic conductivity and high tap density, and are more rational coating modification materials other than carbon materials. In order to achieve metal element coating modification, metal nanoparticles can be used as raw materials and combined with battery materials by ball milling or heat treatment. However, due to the uniformity and dispersibility of metal element particle size in this type of technical solution, it is difficult to achieve the technical effect of uniform metal element coating battery materials. Another type of solution is to use metal element compounds to in-situ reduce the surface of the battery material to form a uniform metal element coating layer. However, this type of technical solution generally requires a high-temperature heat treatment process under a protective atmosphere to achieve metal element reduction. The required temperature is generally greater than 500°C, which is much higher than the decomposition temperature of Prussian blue materials at 350°C. Therefore, the use of this type of technical solution to coat Prussian blue sodium cathode materials with metal elements faces huge challenges. Summary of the invention

[0006] The purpose of the present invention is to provide a method for coating a Prussian blue sodium cathode material by a vapor deposition method. The conductive layer formed by the deposition of iron element nanoparticles on the surface of the Prussian blue material can achieve the beneficial effect of improving the electrical conductivity of the material. At the same time, the iron element coating layer can also reduce the water absorption of the Prussian blue sodium cathode material and improve the electrochemical interface stability of the material. The purpose of the present invention is also to provide an iron element coated modified Prussian blue sodium cathode material prepared by the above method.

[0007] In order to solve the above technical problems, the preparation method of the present invention comprises the following steps: (1) Fe(CO)5 is heated to boiling point under a protective atmosphere and vaporized to form a mixed gas containing Fe(CO)5 with the protective gas as a carrier, wherein the mass fraction of Fe(CO)5 in the mixed gas is 1% to 20%; (2) placing an appropriate amount of Prussian blue sodium cathode material into a coating furnace, controlling the mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium cathode material to be 1:10-20, and introducing protective gas to replace the air in the coating furnace; (3) Turn off the protective gas in step (2), and feed the Fe(CO)5 mixed gas in step (1) into and continuously pass through the coating furnace, with the flow rate of the Fe(CO)5 mixed gas being 3 to 150 ml / min; (4) After the Fe(CO)5 mixed gas in step (3) is introduced into the coating furnace at room temperature for 10 to 70 minutes, the reactants in the coating furnace are heated to 140 to 310°C at a rate of 2 to 15°C / min and then kept at this temperature for 1 to 15 hours. During the heating and keeping period, the mixed gas is continuously introduced at a flow rate of 3 to 150 ml / min. (5) After the insulation in step (4) is completed, the Fe(CO)5 mixed gas is turned off, and the protective gas is introduced. The coating furnace is naturally cooled to room temperature to obtain a modified Prussian blue sodium-based positive electrode material, the surface of which is coated with a layer of iron.

[0008] In the step (1), the protective gas includes one of nitrogen, argon and helium; preferably, the protective gas includes one of nitrogen and argon; more preferably, the protective gas is nitrogen.

[0009] In the step (1), the mass fraction of Fe(CO)5 in the mixed gas is 5% to 16%; preferably, the mass fraction of Fe(CO)5 in the mixed gas is 9% to 11%.

[0010] In the step (2), the Prussian blue sodium positive electrode material includes one of an iron-based Prussian blue sodium positive electrode material, an iron-manganese-based Prussian blue sodium positive electrode material, an iron-cobalt-based Prussian blue sodium positive electrode material, an iron-nickel-based Prussian blue sodium positive electrode material, and an iron-copper-based Prussian blue sodium positive electrode material.

[0011] In the step (2), the coating furnace includes one of a rotary kiln, a tubular atmosphere furnace, and a box-type atmosphere furnace; preferably, the coating furnace includes one of a rotary kiln and a tubular atmosphere furnace; more preferably, the coating furnace is a rotary kiln.

[0012] In the step (2), the mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium-based cathode material is controlled to be 1:12-18; preferably, the mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium-based cathode material is controlled to be 1:14-16.

[0013] In the step (2), the protective gas includes one of nitrogen, argon and helium; preferably, the protective gas includes one of nitrogen and argon; more preferably, the protective gas is nitrogen.

[0014] In the step (3), the flow rate of the Fe(CO)5 mixed gas is 10 to 100 ml / min; preferably, the flow rate of the Fe(CO)5 mixed gas is 50 to 60 ml / min.

[0015] In the step (4), the time for introducing the Fe(CO)5 mixed gas before the coating furnace is heated up is 20 to 60 minutes; preferably, the time for introducing the Fe(CO)5 mixed gas before the coating furnace is heated up is 35 to 45 minutes.

[0016] In the step (4), the heating rate of the coating furnace is 4 to 12°C / min; preferably, the heating rate of the coating furnace is 7 to 9°C / min.

[0017] In the step (4), the insulation temperature is 160-280°C; preferably, the insulation temperature is 210-230°C.

[0018] In the step (4), the insulation time is 4 to 12 hours; preferably, the insulation time is 7 to 9 hours.

[0019] In the step (4), the flow rate of the Fe(CO)5 mixed gas during the heating and insulation period is 10 to 100 ml / min; preferably, the flow rate of the Fe(CO)5 mixed gas during the heating and insulation period is 50 to 60 ml / min.

[0020] In the step (5), the protective gas includes one of nitrogen, argon and helium; preferably, the protective gas includes one of nitrogen and argon; more preferably, the protective gas is nitrogen.

[0021] In the step (5), the flow rate of the protective gas is 5 to 100 ml / min; preferably, the flow rate of the protective gas is 25 to 80 ml / min; more preferably, the flow rate of the protective gas is 45 to 55 ml / min.

[0022] The present invention also provides a modified Prussian blue sodium-based positive electrode material, which is prepared by the above method; the positive electrode material comprises a Prussian blue sodium-based positive electrode material matrix and an iron element coating layer.

[0023] The method provided by the present invention and the obtained modified Prussian blue sodium-based positive electrode material have the following beneficial effects: (1) During the modification process, the vaporized Fe(CO)5 is brought into the coating furnace by the protective gas and decomposed into iron nanoparticles and CO at a temperature of 140-310°C. The decomposition reaction is carried out under gas phase conditions. During the coating process, the Prussian blue sodium cathode material is always kept dry, which can avoid the problem of using more organic solvents and deionized water and secondary drying in liquid phase modification such as solvothermal or hydrothermal methods.

[0024] (2) Iron is not easy to react with water and is insoluble in water. The technical solution forms a layer of iron coating on the surface of the Prussian blue sodium cathode material by chemical vapor deposition. The presence of this coating can prevent the Prussian blue sodium cathode material from direct contact with water, reduce its water absorption in the air, and help improve the processing performance of the Prussian blue sodium cathode material.

[0025] (3) The presence of the iron coating can prevent the base material from direct contact with the electrolyte, thereby preventing the HF formed by trace water in the electrolyte from corroding the Prussian blue sodium cathode material base, thereby improving the material's cycle performance.

[0026] (4) FeF2 formed by the reaction of iron and HF is a phase-change cathode material that can play a role in passivation protection, inhibit the occurrence of electrochemical interface side reactions, and increase the electrochemical interface stability of the material.

[0027] (5) Elemental iron has extremely high electronic conductivity. Coating it on the surface of the matrix material can solve the problem of low inherent conductivity of Prussian blue sodium cathode materials to a certain extent, thereby achieving the beneficial effect of improving the material's rate performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The charge and discharge curves at 0.1C of the iron-based Prussian blue sodium-based cathode material modified by iron element coating prepared in Example 1 of the present invention and the iron-based Prussian blue sodium-based cathode material of the comparative example.

[0029] Figure 2 This is an X-ray diffraction (XRD) pattern of the iron-based Prussian blue sodium-based cathode material modified by iron element coating prepared in Example 1 of the present invention.

[0030] Figure 3 This is a scanning electron microscope (SEM) image of the iron-based Prussian blue sodium-based cathode material modified by iron element coating prepared in Example 1. (Abstract attached) Figure 4 This is a scanning electron microscope (SEM) image of the iron-manganese-based Prussian blue sodium-like positive electrode material in the comparative example of the present invention without any treatment.

[0031] Figure 5 This is an electron image collected when performing energy dispersive X-ray spectroscopy analysis on the iron-based Prussian blue-like sodium-based cathode material coated with iron element modified in Example 1 of the present invention.

[0032] Figure 6 for Figure 5 Energy dispersive X-ray spectroscopy (EDS) of selected areas. DETAILED DESCRIPTION

[0033] In order to make the present invention more obvious and easy to understand, the technical solution of the present invention is further explained below through embodiments in combination with the drawings, but it is not intended to limit the protection scope of the present invention.

[0034] The unmodified Prussian blue sodium positive electrode material includes but is not limited to one or more of an iron-based Prussian blue material, an iron-manganese-based Prussian blue material, an iron-cobalt-based Prussian blue material, an iron-nickel-based Prussian blue material, and an iron-copper-based Prussian blue material. The unmodified Prussian blue sodium positive electrode material selected in the embodiment of the present invention is an iron-manganese-based Prussian blue material. Example 1

[0035] Fe(CO)5 is heated to boiling point and vaporized under nitrogen protection to form a Fe(CO)5 mixed gas with nitrogen as carrier, and the mass fraction of Fe(CO)5 in the mixed gas is 10%. The mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium positive electrode material is controlled to be 1:15. The iron-manganese-based Prussian blue sodium positive electrode material is placed in a rotary kiln, and nitrogen is introduced to replace the air in the rotary kiln. Subsequently, the protective gas is turned off, and the Fe(CO)5 mixed gas is fed into the rotary kiln at a rate of 55ml / min. After the Fe(CO)5 mixed gas is passed into the rotary kiln for 40 minutes, the reactants in the rotary kiln are heated to 220℃ at 8℃ / min and then kept warm for 8h. During the heating and insulation period, the Fe(CO)5 mixed gas is continuously passed at a flow rate of 55ml / min. After the insulation is completed, the Fe(CO)5 mixed gas is turned off, and nitrogen is introduced at 50 ml / min until the rotary furnace naturally cools to room temperature, thereby obtaining a modified Prussian blue sodium-based positive electrode material, the surface of which is coated with a layer of iron element.

[0036] Fe(CO)5 can easily decompose to form iron and carbon monoxide under high temperature conditions. Using the vapor deposition modification process, the iron nanoparticles formed by the thermal decomposition of Fe(CO)5 will deposit the iron-manganese-based Prussian blue sodium-type cathode material to form a surface coating layer. The thickness of the iron coating layer can be controlled by controlling the mass fraction of Fe(CO)5 in the mixed gas, the mass ratio of the Fe(CO)5 used in the coating process to the mass ratio of the Prussian blue sodium-type cathode material, and the air flow velocity and time of the Fe(CO)5 mixed gas passing into the rotary kiln.

[0037] This technical solution is carried out under gas phase conditions, and the Prussian blue sodium positive electrode material is always kept in a dry state during the coating process, which can avoid the problem that more organic solvents and deionized water and secondary drying are required for liquid phase modification such as solvothermal method or hydrothermal method. Iron is not easy to react with water and is insoluble in water. This technical solution forms a layer of iron coating on the surface of Prussian blue sodium positive electrode material by vapor deposition. The presence of this coating can avoid direct contact between Prussian blue sodium positive electrode material and water, reduce its water absorption in the air, and help improve the processing performance of Prussian blue sodium positive electrode material. The presence of iron coating can avoid direct contact between the base material and the electrolyte, inhibit the occurrence of electrochemical interface side reactions, increase the electrochemical interface stability of the material, and thus improve the material cycle performance. Iron has extremely high electronic conductivity. Coating on the surface of the base material can solve the problem of low inherent conductivity of Prussian blue sodium positive electrode material to a certain extent, thereby achieving the beneficial effect of improving the material rate performance.

[0038] Figure 1 The first charge and discharge curves of the materials obtained in Example 1 and the comparative example at 0.1C are shown. It can be seen from the figure that the 0.1C discharge capacity of the material in Example 1 is about 4.4 mAh / g higher than that of the comparative example. In addition, the coulombic efficiency of the first charge and discharge of the material obtained in Example 1 is 96.5%, while the first efficiency of the comparative example material is only 89.0%, which can indicate that after the iron element is coated and modified, the interface side reaction between the substrate and the electrolyte can be suppressed, and the interface stability of the electrochemical reaction can be increased.

[0039] Figure 2 The X-ray diffraction (XRD) diagram of the iron-based Prussian blue sodium-type positive electrode material prepared in Example 1 of the present invention, from which it can be seen that the main characteristic peaks in the X-ray diffraction (XRD) diagram are consistent with the iron-based Prussian blue sodium-type positive electrode material, which shows that the iron-based Prussian blue sodium-type positive electrode material is not changed by the iron-based Prussian blue sodium-type positive electrode material by the vapor deposition process. In addition, a weak characteristic peak of the iron element appears near 44.7°, which shows that this technical solution successfully deposits a layer of iron element on the surface of the Prussian blue sodium-type positive electrode material. Example 2

[0040] Fe(CO)5 was heated to boiling point and vaporized under argon protection to form a Fe(CO)5 mixed gas with argon as carrier, and the mass fraction of Fe(CO)5 in the mixed gas was 9%. The mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium positive electrode material was controlled to be 1:14, and the iron-manganese-based Prussian blue sodium positive electrode material was placed in a tubular atmosphere furnace, and argon was introduced to replace the air in the tubular atmosphere furnace. Subsequently, the protective gas was turned off, and the Fe(CO)5 mixed gas was fed into the tubular atmosphere furnace at a rate of 50ml / min. After the Fe(CO)5 mixed gas was introduced into the tubular atmosphere furnace for 45min, the reactants in the tubular atmosphere furnace were heated to 230℃ at 7℃ / min, and then kept warm for 7h. During the heating and keeping warm period, the Fe(CO)5 mixed gas was continuously introduced at a flow rate of 50ml / min. After the insulation was completed, the Fe(CO)5 mixed gas was turned off, and argon gas was introduced at 55 ml / min until the tubular atmosphere furnace naturally cooled to room temperature, thereby obtaining a modified Prussian blue sodium-based positive electrode material, the surface of which was coated with a layer of iron element. Example 3

[0041] Fe(CO)5 is heated to boiling point and vaporized under the protection of helium to form a mixed gas containing Fe(CO)5 with helium as the carrier, and the mass fraction of Fe(CO)5 in the mixed gas is 11%. The mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium-based cathode material is controlled to be 1:16. The iron-manganese-based Prussian blue sodium-based cathode material is placed in a box-type atmosphere furnace, and helium is introduced to replace the air in the box-type atmosphere furnace. Subsequently, the protective gas is turned off, and the mixed gas containing Fe(CO)5 is fed into the box-type atmosphere furnace at a rate of 60ml / min. After the mixed gas containing Fe(CO)5 is introduced into the box-type atmosphere furnace for 35min, the reactants in the box-type atmosphere furnace are heated to 210℃ at 9℃ / min and then kept warm for 9h. During the heating and insulation period, the mixed gas containing Fe(CO)5 is continuously introduced at a flow rate of 60ml / min. After the insulation is completed, the Fe(CO)5 mixed gas is turned off, and helium is introduced at 45 ml / min until the box-type atmosphere furnace naturally cools to room temperature, thereby obtaining a modified Prussian blue sodium-based positive electrode material, the surface of which is coated with a layer of iron element. Example 4

[0042] Fe(CO)5 is heated to boiling point and vaporized under nitrogen protection to form a Fe(CO)5 mixed gas with nitrogen as carrier, and the mass fraction of Fe(CO)5 in the mixed gas is 16%. The mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium positive electrode material is controlled to be 1:12. The iron-manganese-based Prussian blue sodium positive electrode material is placed in a rotary kiln, and nitrogen is introduced to replace the air in the rotary kiln. Subsequently, the protective gas is turned off, and the Fe(CO)5 mixed gas is fed into the rotary kiln at a rate of 10ml / min. After the Fe(CO)5 mixed gas is passed into the rotary kiln for 60 minutes, the reactants in the rotary kiln are heated to 280℃ at 12℃ / min and then kept warm for 4h. During the heating and insulation period, the Fe(CO)5 mixed gas is continuously introduced at a flow rate of 10ml / min. After the insulation is completed, the Fe(CO)5 mixed gas is turned off, and nitrogen is introduced at 25 ml / min until the rotary furnace naturally cools to room temperature, thereby obtaining a modified Prussian blue sodium-based positive electrode material, the surface of which is coated with a layer of iron. Example 5

[0043] Fe(CO)5 is heated to boiling point and vaporized under nitrogen protection to form a Fe(CO)5 mixed gas with nitrogen as carrier, and the mass fraction of Fe(CO)5 in the mixed gas is 5%. The mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium positive electrode material is controlled to be 1:18, and the iron-manganese-based Prussian blue sodium positive electrode material is placed in a rotary kiln, and nitrogen is introduced to replace the air in the rotary kiln. Subsequently, the protective gas is turned off, and the Fe(CO)5 mixed gas is fed into the rotary kiln at a rate of 100ml / min. After the Fe(CO)5 mixed gas is passed into the rotary kiln for 20 minutes, the reactants in the rotary kiln are heated to 160℃ at 4℃ / min, and then kept warm for 12 hours. During the heating and insulation period, the Fe(CO)5 mixed gas is continuously passed at a flow rate of 100ml / min. After the insulation is completed, the Fe(CO)5 mixed gas is turned off, and nitrogen is introduced at 80 ml / min until the rotary furnace naturally cools to room temperature, thereby obtaining a modified Prussian blue sodium-based positive electrode material, the surface of which is coated with a layer of iron element. Example 6

[0044] Fe(CO)5 is heated to boiling point and vaporized under nitrogen protection to form a Fe(CO)5 mixed gas with nitrogen as carrier, and the mass fraction of Fe(CO)5 in the mixed gas is 1%. The mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium positive electrode material is controlled to be 1:10, and the iron-manganese-based Prussian blue sodium positive electrode material is placed in a rotary kiln, and nitrogen is introduced to replace the air in the rotary kiln. Subsequently, the protective gas is turned off, and the Fe(CO)5 mixed gas is fed into the rotary kiln at a rate of 3ml / min. After the Fe(CO)5 mixed gas is passed into the rotary kiln for 70 minutes, the reactants in the rotary kiln are heated to 140°C at 2°C / min and then kept warm for 15 hours. During the heating and insulation period, the Fe(CO)5 mixed gas is continuously introduced at a flow rate of 3ml / min. After the insulation is completed, the Fe(CO)5 mixed gas is turned off, and nitrogen is introduced at 5 ml / min until the rotary furnace naturally cools to room temperature, thereby obtaining a modified Prussian blue sodium-based positive electrode material, the surface of which is coated with a layer of iron. Example 7

[0045] Fe(CO)5 is heated to boiling point and vaporized under nitrogen protection to form a Fe(CO)5 mixed gas with nitrogen as carrier, and the mass fraction of Fe(CO)5 in the mixed gas is 20%. The mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium positive electrode material is controlled to be 1:20, and the iron-manganese-based Prussian blue sodium positive electrode material is placed in a rotary kiln, and nitrogen is introduced to replace the air in the rotary kiln. Subsequently, the protective gas is turned off, and the Fe(CO)5 mixed gas is fed into the rotary kiln at a rate of 150ml / min. After the Fe(CO)5 mixed gas is passed into the rotary kiln for 10 minutes, the reactants in the rotary kiln are heated to 310℃ at 15℃ / min, and then kept warm for 1h. During the heating and insulation period, the Fe(CO)5 mixed gas is continuously passed at a flow rate of 150ml / min. After the insulation is completed, the Fe(CO)5 mixed gas is turned off, and nitrogen is introduced at 100 ml / min until the rotary furnace naturally drops to room temperature, thereby obtaining a modified Prussian blue sodium-based positive electrode material, the surface of which is coated with a layer of iron element.

[0046] In order to illustrate the necessity of each technical link of the present invention for the beneficial effects, the following comparative examples are implemented. Comparative Example

[0047] Except that Fe(CO)5 is not used as the coating agent, the other processes are consistent with those in Example 1.

[0048] The material prepared by the process of the embodiment and the comparative example is immediately used as an active material to prepare a positive electrode sheet for the assembly test of a sodium ion battery.

[0049] The preparation process of the positive electrode is as follows: acetylene black is used as a conductive additive, 25mg / ml polyvinylidene fluoride (PVDF) N-methylpyrrolidone (NMP) solution is used as a binder, the active material, conductive agent and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 7:2:1 and ground into a slurry with suitable viscosity, and then the slurry is evenly coated on the carbon-coated aluminum foil. The coated electrode is placed in a vacuum drying oven at 120°C for 8 hours. After drying, it is punched into a disc with a diameter of 12mm by a punching machine, and finally the battery is assembled in a glove box in an argon atmosphere.

[0050] The battery assembly process is as follows: the prepared positive electrode sheet is used as the positive electrode, the metal sodium sheet is used as the negative electrode, and the glass fiber is used as the separator. 250 μL of sodium hexafluorophosphate electrolyte with a concentration of 1 mol / L is added. The electrolyte solvent is a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) with a volume ratio of 1:1. 3% fluoroethylene carbonate (FEC) is added to the electrolyte as an additive. The assembled button half-cell adopts a constant current charge and discharge mode in the voltage range of 2.0 to 4.0 V to carry out the corresponding electrochemical performance test.

[0051] In addition, in order to test the storage performance of the materials, the materials prepared by the process of Example 1 and the comparative example were exposed to air for 15 hours to prepare electrode sheets and assemble batteries for corresponding electrochemical performance tests. The samples were marked as Example 1-15h and Comparative Example-15h, respectively. The electrochemical performance test results of each material are shown in Table 1.

[0052]

[0053] The difference in discharge capacity at different rates of Example 1 and the samples after being set aside for 15 hours is less than 1 mAh / g, and the difference in retention rate after 1100 cycles at 5C does not exceed 1%; the difference in discharge capacity at different rates of the control example and the samples set aside for 15 hours exceeds 10 mAh / g, and the difference in retention rate after 1100 cycles at 5C is greater than 10%, which indicates that the surface iron-coated modification of the Prussian blue sodium-based positive electrode material using the present technical solution inhibits the material from absorbing water again when exposed to air, thereby improving the storage stability of the material in air.

[0054] The embodiments are all better than the comparative examples, which shows that the electrochemical properties of the material can be significantly improved after the surface coating of the vapor-deposited iron element. Among all the embodiments, Example 1 has the best electrochemical performance. By comparing the discharge specific capacity of Example 1 with that of the comparative example, it can be seen that the difference in discharge specific capacity at 0.1C is relatively small, only 4.4mAh / g. However, as the battery discharge rate gradually increases from 1C to 20C, the difference in discharge specific capacity between the two becomes larger and larger. At 10C and 20C, the discharge specific capacity of Example 1 is 26.8mAh / g and 33mAh / g higher than that of the comparative example, respectively. This shows that the conductivity of the material is greatly improved after the iron element coating modification using this process scheme, which can solve the problems of poor electrochemical kinetics and stability caused by the inherent low conductivity of Prussian blue sodium positive electrode materials.

[0055] The 5C cycle 1100-week capacity retention rate of each embodiment is not less than 83%, and the 20C high-discharge capacity is not less than 118 mAh / g, which are better than the comparative example. From these two points of comparison, it can be seen that the iron single substance coating layer formed by vapor deposition on the surface of the material using the technical solution of the present invention can inhibit the interfacial side reaction between the Prussian blue sodium positive electrode material and the electrolyte, thereby solving the problem of poor electrochemical kinetics and stability, and further improving the rate performance and cycle performance of the material.

[0056] The above-described specific embodiments further illustrate the present invention in detail, but these descriptions cannot be understood as limiting the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for coating a Prussian blue sodium positive electrode material by vapor deposition, characterized in that: The following steps are involved: (1) Fe(CO)5 is heated to boiling point under a protective atmosphere and vaporized to form a mixed gas containing Fe(CO)5 with the protective gas as a carrier, wherein the mass fraction of Fe(CO)5 in the mixed gas is 1% to 20%; (2) placing an appropriate amount of Prussian blue sodium cathode material into a coating furnace, controlling the mass ratio of Fe(CO)5 used in the coating process to the mass ratio of Prussian blue sodium cathode material to be 1:10-20, and introducing protective gas to replace the air in the coating furnace; (3) Turn off the protective gas in step (2), and feed the Fe(CO)5 mixed gas in step (1) into and continuously pass through the coating furnace, with the flow rate of the Fe(CO)5 mixed gas being 3 to 150 ml / min; (4) After the Fe(CO)5 mixed gas in step (3) is introduced into the coating furnace at room temperature for 10 to 70 minutes, the reactants in the coating furnace are heated to 140 to 310°C at a rate of 2 to 15°C / min and then kept at this temperature for 1 to 15 hours. During the heating and keeping period, the mixed gas is continuously introduced at a flow rate of 3 to 150 ml / min. (5) After the insulation in step (4) is completed, the Fe(CO)5 mixed gas is turned off, and the protective gas is introduced. The coating furnace is naturally cooled to room temperature to obtain a modified Prussian blue sodium-based positive electrode material, the surface of which is coated with a layer of iron.

2. The method for coating a Prussian blue sodium-based cathode material by vapor deposition according to claim 1, characterized in that: In the step (1), the protective gas includes one of nitrogen, argon and helium; and the mass fraction of Fe(CO)5 in the mixed gas is 5% to 16%.

3. The method for coating a Prussian blue sodium positive electrode material by vapor deposition according to claim 1, characterized in that: In the step (2), the Prussian blue sodium positive electrode material includes one of an iron-based Prussian blue sodium positive electrode material, an iron-manganese-based Prussian blue sodium positive electrode material, an iron-cobalt-based Prussian blue sodium positive electrode material, an iron-nickel-based Prussian blue sodium positive electrode material, and an iron-copper-based Prussian blue sodium positive electrode material; the mass ratio of Fe(CO)5 used in the coating process to the mass ratio of the Prussian blue sodium positive electrode material is controlled to be 1:12-18; the coating furnace includes one of a rotary kiln, a tubular atmosphere furnace, and a box atmosphere furnace; and the protective gas includes one of nitrogen, argon, and helium.

4. The method for coating a Prussian blue sodium-based cathode material by vapor deposition according to claim 1, characterized in that: In the step (3), the flow rate of the Fe(CO)5 mixed gas is 10 to 100 ml / min.

5. The method for coating a Prussian blue sodium positive electrode material by vapor deposition according to claim 1, characterized in that: In the step (4), the time for introducing the Fe(CO)5 mixed gas before heating the coating furnace is 20 to 60 minutes; the heating rate of the coating furnace is 4 to 12°C / min; the insulation temperature is 160 to 280°C, and the insulation time is 4 to 10 hours; the flow rate of the Fe(CO)5 mixed gas during heating and insulation is 10 to 100 ml / min.

6. The method for coating a Prussian blue sodium-based cathode material by vapor deposition according to claim 1, characterized in that: In the step (5), the protective gas includes one of nitrogen, argon and helium; and the flow rate of the protective gas is 5 to 100 ml / min.

7. A modified Prussian blue sodium positive electrode material, characterized in that: The modified Prussian blue sodium cathode material is prepared by the method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Positive electrode material and preparation method thereof, positive electrode plate and sodium ion battery

    CN113921798A

  • Preparation method of copper oxide modified iron-based Prussian blue positive electrode material

    CN114620758A

  • Gas phase modification method of Prussian blue sodium battery positive electrode material and positive electrode material prepared by same

    CN115411260A