Fe-coated Ni3S2 / NF electrode material and preparation method thereof

Through the preparation method of Fe@Ni3S2/NF electrode material, high-valent Fe ions are used to promote the dissolution effect and redox reaction of sodium thiosulfate on Ni ions, and realize a one-step hydrothermal reaction to prepare composite materials, solving the problem of nickel-based sulfide electrode material. The problems of self-aggregation and poor conductivity of nanoparticles during charging and discharging significantly improve the discharge capacity and cyclic stability of the electrode material.

CN119050256APending Publication Date: 2024-11-29GUIYANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411159726.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

Smart Images

  • Figure CN119050256A_ABST
    Figure CN119050256A_ABST
Patent Text Reader

Abstract

The invention provides a Fe-coated Ni3S2 / NF electrode material and a preparation method thereof, and the preparation method of the Fe-coated Ni3S2 / NF electrode material comprises the following steps: placing a porous nickel material in a hydrochloric acid solution for ultrasonic treatment, then repeatedly cleaning with ethanol and deionized water, drying, reacting the dried porous nickel material with a reaction solution at a reaction temperature of 60-100 DEG C for 6-12 h, and drying to obtain the Fe-coated Ni3S2 / NF electrode material, the reaction liquid is mainly prepared by mixing Fe (NO3) 3.9 H2O, Na2S2O3. 5H2O and deionized water, wherein the mass ratio of Fe (NO3) 3.9 H2O to Na2S2O3. 5H2O is (2: 1)-(10: 1). The electrode material prepared by the preparation method disclosed by the invention has good electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of electrode material preparation, and in particular to a Fe@Ni3S2 / NF electrode material and a preparation method thereof. Background Art

[0002] The large-scale and rapid consumption of traditional resources by modern society and industrial systems has led to the risk of their depletion. The development of new renewable energy sources such as wind power and solar energy is the key to solving this problem. However, new energy sources are unstable and intermittent, so it is necessary to develop energy storage systems with excellent performance and reliability. Aqueous zinc-ion batteries have the advantages of low cost, high safety, rapid ion migration, high capacity and long life, and are an excellent solution to the current energy storage problem. However, this battery is difficult to be widely used due to the limitations of large electrode volume expansion, structural deformation and poor rate performance. In this case, it is imperative to design and prepare composite electrode materials with suitable structures.

[0003] Transition metal sulfides are considered to be extremely promising cathode materials for aqueous zinc-ion batteries (AZIBs) due to their high capacity and redox potential. Researchers have conducted extensive research on nickel-based sulfides among transition metal sulfides, but the main obstacle to the widespread application of these nickel-based sulfide electrodes is their complex preparation process. In addition, the electrochemical properties of nickel-based sulfide electrode materials obtained by existing preparation methods, such as energy density and cycle stability, are still insufficient. During repeated charge and discharge processes, nickel disulfide usually exhibits self-aggregation of nanoparticles or volume expansion. In addition, due to its poor conductivity, the diffusion of electrons and ions is slow, resulting in low discharge capacity, rate capability and cycle life.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The first purpose of the present invention is to provide a method for preparing a Fe@Ni3S2 / NF electrode material. The preparation method utilizes high-valent Fe ions to promote the dissolution effect of sodium thiosulfate on Ni ions and the redox reaction between the two, thereby realizing a one-step hydrothermal reaction to prepare a composite material without the need to add any surfactant or adhesive, greatly shortening the preparation cycle, having the characteristics of low-temperature synthesis, and the resulting product has high purity and good electrochemical properties.

[0006] The second purpose of the present invention is to provide a Fe@Ni3S2 / NF electrode material prepared by the above-mentioned preparation method. When the electrode material is matched with a treated pure Zn electrode to form a Fe@Ni3S2 / NF / / Zn aqueous zinc ion battery, it exhibits high discharge capacity, significant rate performance and good cycle stability, and has good electrochemical properties.

[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0008] The present invention provides a method for preparing a Fe@Ni3S2 / NF electrode material, comprising the following steps:

[0009] The porous nickel material is placed in a hydrochloric acid solution for ultrasonic treatment, and then repeatedly washed with ethanol and deionized water for 3-5 times, and then dried. The dried porous nickel material is reacted with the reaction solution at a reaction temperature of 60-100° C. for a reaction time of 6-12 hours, and then dried to obtain the product;

[0010] The reaction solution is mainly prepared by mixing Fe(NO3)3·9H2O and Na2S2O3·5H2O in a molar ratio of (2:1) to (10:1) and deionized water.

[0011] The preparation method of the present invention adds Fe(NO3)3·9H2O and Na2S2O3·5H2O in a certain molar ratio as a reaction solution to carry out a hydrothermal synthesis reaction, which is equivalent to using high-valent Fe ions to promote the dissolution effect of sodium thiosulfate on Ni ions and the redox reaction between the two, thereby realizing the one-step hydrothermal reaction synthesis of Ni3S2 electrode materials at a relatively low temperature, and ensuring that the Fe@Ni3S2 nanoflower array and NF in the prepared electrode material have a stable and close combination. In addition, the incorporation of iron elements can promote the formation of ultrathin nanosheets, affect the morphology of sulfide nanosheets, and significantly adjust the surface electron density. The present invention makes the electrode material have the optimal number of active site exposures and intrinsic activity by regulating the incorporation amount of iron elements (i.e., controlling the molar ratio of iron nitrate to sodium thiosulfate), thereby solving the problem that the nickel-based sulfide electrode materials prepared by the prior art still have insufficient electrochemical properties such as energy density and cycle stability.

[0012] The reason why the electrode material prepared by the method of the present invention has good electrochemical performance is that during the preparation process, sulfide nanoparticles are evenly distributed on the surface of nickel foam, providing more redox active sites and better adsorption capacity for anions in the electrolyte, thereby improving the performance of the electrode material.

[0013] In this way, when the electrode material is applied, for example, in the assembly of an aqueous zinc ion secondary battery, the treated pure zinc electrode is used as the negative electrode, the single electrode Fe@Ni3S2 / NF electrode prepared by the scheme of the present invention is used as the positive electrode, a 6M KOH aqueous solution is used as the electrolyte, and the glass fiber is used as the separator; the positive electrode and the negative electrode are assembled into an aqueous zinc ion battery, and then the electrochemical performance of the battery is tested, and it is found that it exhibits high discharge capacity, significant rate performance and good cycle stability.

[0014] Preferably, as a further implementable scheme, the molar ratio of Fe(NO3)3·9H2O and Na2S2O3·5H2O is (3:1) to (7:1).

[0015] Preferably, as a further feasible solution, the molar ratio of Fe(NO3)3·9H2O and Na2S2O3·5H2O is 5:1.

[0016] Preferably, as a further feasible scheme, the reaction temperature is 80-90°C.

[0017] Preferably, as a further feasible solution, the reaction time is 8-10 h.

[0018] The present invention uses a chemical etching process, that is, hydrolysis to generate OH -1 The metallic Ni is dissolved in the form of Ni(OH)2, and in the case of Fe doping, the metallic Ni is in situ converted into an ultrathin metal sulfide array grown on the NF.

[0019] The reaction formula for the reaction of elemental Ni and sodium thiosulfate to generate Ni3S2 is:

[0020] 3Ni+2Na2S2O3=Ni3S2+2Na2SO3

[0021] Converted to Ni 2+ The reaction formula for the subsequent reaction to generate Ni3S2 is:

[0022] 3Ni 2+ +2S2O3 2- =Ni3S2+2SO3 2+

[0023] Therefore, the above mechanism can also show that the scheme of the present invention can realize the synthesis of Ni3S2 at a lower temperature.

[0024] The incorporation of iron can promote the formation of ultrathin nanosheets, affect the morphology of sulfide nanosheets, and significantly adjust the surface electron density. Therefore, the appropriate regulation of the amount of iron incorporation (i.e., controlling the molar ratio of iron nitrate to sodium thiosulfate) can obtain the optimal number of active site exposures and intrinsic activity. In addition, in-situ growth through direct etching process can ensure a stable and close bond between the Fe@Ni3S2 nanoflower array and NF in the prepared electrode material. Of course, the amount of iron added is also limited, and it cannot be excessive or insufficient, so the above molar ratio needs to be controlled within an appropriate range.

[0025] The above components can be replaced by FeCl3 and Fe2(SO3)3 except Fe(NO3)3. Sodium thiosulfate NaS2SO3 can also be replaced by thioacetamide.

[0026] Preferably, as a further feasible solution, the concentration of the hydrochloric acid solution is 2-4 mol / L, and the ultrasonic time is 4-6 min.

[0027] Preferably, as a further feasible solution, after washing 3-5 times, the drying temperature is 50-70° C. and the drying time is 2-4 hours.

[0028] Preferably, as a further feasible solution, the drying temperature after the reaction is 80-120° C., the drying time is more than 6 hours, and more preferably the drying and heat preservation is 12 hours.

[0029] The present invention also provides a Fe@Ni3S2 / NF electrode material prepared by the above preparation method.

[0030] The particle size of Ni3S2 in the electrode material is 400-500nm.

[0031] In summary, the Fe@Ni3S2 / NF electrode material obtained by the present invention has a unique nanoflower structure. When the electrode material is used in an aqueous zinc ion battery, the aqueous zinc ion battery is -2 The discharge capacity at the current density reached 0.58 mAh cm -2 , at 20 mA cm -2 The discharge capacity is maintained at 0.35 mAh cm at the current density -2 , the capacity retention rate is 87.2% after 1000 charge and discharge cycles.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The electrode material prepared by the present invention has a Fe@Ni3S2 / NF composite material with a unique nanoflower structure. The unique multi-layer nanostructured particles inside the material help to expose more electrochemically active sites and increase the contact area between the electrode and the electrolyte. At the same time, the doping of Fe ions improves the attraction of the positive electrode material to the anions in the electrolyte, promotes the transfer of ions, and increases the electroactive sites of the positive electrode material. When matched with the treated pure Zn electrode to form a Fe@Ni3S2 / NF / / Zn aqueous zinc ion battery, it exhibits high discharge capacity, significant rate performance and good cycle stability.

[0034] (2) The preparation method has simple operation of the entire preparation process, low energy consumption of low-temperature reaction, and a simple one-step synthesis process. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] By reading the detailed description of the preferred embodiment below, various other advantages and benefits will become clear to those of ordinary skill in the art. The accompanying drawings are only used for the purpose of illustrating the preferred embodiment and are not considered to be limitations of the present invention. In addition, the same reference symbols are used to represent the same components throughout the accompanying drawings.

[0036] Figure 1 This is a scanning electron microscope image of the Fe@Ni3S2 / NF electrode material prepared in Example 1 of the present invention;

[0037] Figure 2 X-ray diffraction images of the electrode materials prepared in Example 1 and Comparative Example 1 of the present invention, a is Example 1, and b is Comparative Example 1;

[0038] Figure 3 This is the constant current charge and discharge curve of the Fe@Ni3S2 / NF electrode material prepared in Example 1 of the present invention;

[0039] Figure 4 This is a rate performance diagram of the Fe@Ni3S2 / NF electrode material prepared in Example 1 of the present invention;

[0040] Figure 5 This is the long cycle curve of the Fe@Ni3S2 / NF electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0041] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0042] Example 1

[0043] The preparation method of Fe@Ni3S2 / NF electrode material includes the following steps:

[0044] 1) Cut the nickel foam sheet into 1×2 cm 2 Thin slices, the porous nickel material was placed in a 3 mol / L hydrochloric acid solution for 5 minutes of ultrasonic treatment, and then taken out and washed repeatedly with ethanol and deionized water for 3 to 5 times;

[0045] 2) placing the cleaned porous nickel material in an ethanol solution, ultrasonicating it for 15 minutes, and then placing it in an oven for drying at 60°C for 3 hours;

[0046] 3) Put 0.404 g (1 mmol) of Fe(NO3)3·9H2O and 0.0496 g (0.2 mmol) of Na2S2O3·5H2O into a beaker, add 30 mL of deionized water, stir evenly, transfer to a polytetrafluoroethylene inner cylinder, put in the treated porous nickel material, and transfer to the reactor together;

[0047] 4) The reactor was placed in an oven, the reaction temperature was set to 60°C, and the reaction vessel was taken out after the hydrothermal reaction for 6 hours. After being washed with deionized water, the reaction vessel was placed in an oven and dried at 100°C for 6 hours to obtain the electrode material.

[0048] The electrochemical performance of the Fe@Ni3S2 / NF electrode material obtained in this example was tested using a double electrode system: -2 At this current density, the discharge capacity is 0.58 mAh cm -2 , at 20mAh·cm -2 At this current density, the discharge capacity is 0.35 mAh cm -2 , at 4 mAh cm -2 After 1000 cycles under current density conditions, the discharge capacity retention rate is 87.2%. Figure 1-5 shown.

[0049] Example 2

[0050] The only difference from Example 1 is that 0.808 g (2 mmol) of Fe(NO3)3·9H2O and 0.0496 g (0.2 mmol) of Na2S2O3·5H2O are put into a beaker.

[0051] Finally, the prepared electrode material was tested using a double electrode system for the electrochemical performance of the Fe@Ni3S2 / NF electrode material obtained in this example: at 2 mA·cm -2 At this current density, the discharge capacity is 0.28 mAh cm -2 , at 20mA·g -1 At this current density, the discharge capacity is 0.17 mAh cm -2 , at 2 mA cm -2 After 1000 cycles under current density conditions, the capacitance retention rate is 79.2%.

[0052] Example 3

[0053] The only difference from Example 1 is that 0.162 g (0.4 mmol) of Fe(NO3)3·9H2O and 0.0496 g (0.2 mmol) of Na2S2O3·5H2O are put into a beaker.

[0054] Finally, the electrode material was obtained. The electrochemical performance of the Fe@Ni3S2 / NF electrode material obtained in this example was tested using a double electrode system: -2 At the current density, the discharge capacity is 0.15 mAh cm -2 , at 20 mA cm -2 At this current density, the discharge capacity is 0.11 mAh cm -2 , at 4 mA cm -2 After 1000 cycles under current density conditions, the capacitance retention rate is 82.1%.

[0055] Example 4

[0056] The only difference from Example 1 is that the reaction temperature is set at 100° C., the hydrothermal reaction is performed for 12 hours, the mixture is taken out, washed with deionized water, and then placed in an oven at 100° C. for 6 hours to obtain the electrode material.

[0057] The electrochemical performance of the Fe@Ni3S2 / NF electrode material obtained in this example was tested using a double electrode system: -2 At this current density, the discharge capacity is 0.46 mAh cm -2 , at 20 mA cm -2 At this current density, the discharge capacity is 0.28 mAh cm -2 , at 4 mA cm -2 After 1000 cycles under current density conditions, the capacitance retention rate is 71.7%.

[0058] Example 5

[0059] The only difference from Example 1 is that the reaction temperature is set at 80° C., the sample is taken out after the hydrothermal reaction for 12 hours, washed with deionized water, and then dried in an oven at 100° C. for 6 hours to obtain the electrode material.

[0060] The electrochemical performance of the Fe@Ni3S2 / NF electrode material obtained in this example was tested using a double electrode system: -2 At this current density, the discharge capacity is 0.59 mAh cm -2 , at 20mAh·cm -2 At this current density, the discharge capacity is 0.37 mAh cm -2 , at 4 mAh cm -2 After 1000 cycles under current density conditions, the discharge capacity retention rate is 89.1%.

[0061] Example 6

[0062] The preparation method of Fe@Ni3S2 / NF electrode material includes the following steps:

[0063] 1) Cut the nickel foam sheet into 1×2 cm 2 Thin slices, the porous nickel material was placed in a 2 mol / L hydrochloric acid solution for 6 minutes of ultrasonic treatment, and then taken out and washed repeatedly with ethanol and deionized water for 3 to 5 times;

[0064] 2) placing the cleaned porous nickel material in an ethanol solution, ultrasonicating it for 15 minutes, and then transferring it to an oven for drying at 50°C for 4 hours;

[0065] 3) Put 0.404 g (1 mmol) of Fe(NO3)3·9H2O and 0.0496 g (0.2 mmol) of Na2S2O3·5H2O into a beaker, add 30 mL of deionized water, stir evenly, transfer to a polytetrafluoroethylene inner cylinder, put in the treated porous nickel material, and transfer to the reactor together;

[0066] 4) The reactor was placed in an oven, the reaction temperature was set to 90°C, and the reaction was carried out after 10 hours of hydrothermal reaction. The reactor was taken out, washed with deionized water, and then placed in an oven at 120°C for 10 hours to obtain an electrode material.

[0067] The electrochemical performance of the Fe@Ni3S2 / NF electrode material obtained in this example was tested using a double electrode system: -2 At this current density, the discharge capacity is 0.54 mAh cm -2 , at 20mAh·cm -2 At this current density, the discharge capacity is 0.28 mAh cm -2 , at 4 mAh cm -2 After 1000 cycles under current density conditions, the discharge capacity retention rate is 83.4%.

[0068] Example 7

[0069] The preparation method of Fe@Ni3S2 / NF electrode material includes the following steps:

[0070] 1) Cut the nickel foam sheet into 1×2 cm 2 Thin slices, the porous nickel material was placed in a 4 mol / L hydrochloric acid solution for 4 minutes of ultrasonic treatment, and then taken out and washed repeatedly with ethanol and deionized water for 3 to 5 times;

[0071] 2) placing the cleaned porous nickel material in an ethanol solution, ultrasonicating it for 15 minutes, and then transferring it to an oven for drying at 70°C for 2 hours;

[0072] 3) Put 0.404 g (1 mmol) of Fe(NO3)3·9H2O and 0.0496 g (0.2 mmol) of Na2S2O3·5H2O into a beaker, add 30 mL of deionized water, stir evenly, transfer to a polytetrafluoroethylene inner cylinder, put in the treated porous nickel material, and transfer to the reactor together;

[0073] 4) The reactor was placed in an oven, the reaction temperature was set to 90°C, and the reaction was carried out for 10 hours. The reactor was taken out, washed with deionized water, and then placed in an oven at 80°C for 9 hours to obtain an electrode material.

[0074] The electrochemical performance of the Fe@Ni3S2 / NF electrode material obtained in this example was tested using a double electrode system: -2 At this current density, the discharge capacity is 0.52 mAh cm -2 , at 20mAh·cm -2 At this current density, the discharge capacity is 0.23 mAh cm -2 , at 4 mAh cm -2 After 1000 cycles under current density conditions, the discharge capacity retention rate is 81.5%.

[0075] Comparative Example 1

[0076] The difference from Example 1 is that 0.0496 g (0.2 mmol) of Na2S2O3·5H2O is put into a beaker, and 30 mL of deionized water is added.

[0077] Finally, the electrode material was obtained. The electrochemical performance of the Fe@Ni3S2 / NF electrode material obtained in this example was tested using a double electrode system: -2 At this current density, the discharge capacity is 0.19 mAh cm -2 , at 20 mA cm -2 At this current density, the discharge capacity is 0.12 mAh cm -2 , at 4 mA cm -2 After 1000 cycles under current density conditions, the capacitance retention rate is 50.1%. For details, see the X-ray diffraction image. Figure 2 .

[0078] Comparative Example 2

[0079] The only difference from Example 1 is that 0.404 g (1 mmol) of Fe(NO3)3·9H2O is put into a beaker and 30 mL of deionized water is added.

[0080] Finally, the electrode material was obtained. The electrochemical performance of the Fe@Ni3S2 / NF electrode material obtained in this example was tested using a double electrode system:-2 At this current density, the discharge capacity is 0.23 mAh cm -2 , at 20 mA cm -2 At this current density, the discharge capacity is 0.11 mAh cm -2 , at 4 mA cm -2 After 1000 cycles under current density conditions, the capacitance retention rate is 48.3%.

[0081] From the electrochemical performance test results of the electrode materials of the above-mentioned embodiments and comparative examples, it can be known that for the entire Fe@Ni3S2 / NF electrode material preparation method, the ratio of the amounts of Fe(NO3)3·9H2O and Na2S2O3·5H2O substances added has a decisive influence on the electrochemical properties of the composite material finally obtained. Therefore, it is necessary to control the concentration parameter within an appropriate range and execute it according to the scheme of the present invention to finally prepare a positive electrode material with electrochemical properties that meet the requirements of the present invention.

[0082] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications within the scope of the present invention in the appended claims.

Claims

1. A method for preparing a Fe@Ni3S2 / NF electrode material, characterized in that: The steps include: The porous nickel material is placed in a hydrochloric acid solution for ultrasonic treatment, and then repeatedly washed with ethanol and deionized water for 3-5 times, and then dried. The dried porous nickel material is reacted with the reaction solution at a reaction temperature of 60-100° C. for a reaction time of 6-12 hours, and then dried to obtain the product; The reaction solution is mainly prepared by mixing Fe(NO3)3·9H2O and Na2S2O3·5H2O in a molar ratio of (2:1) to (10:1) and deionized water.

2. The preparation method according to claim 1, characterized in that: The molar ratio of Fe(NO3)3·9H2O and Na2S2O3·5H2O is (3:1) to (7:1).

3. The preparation method according to claim 1, characterized in that: The molar ratio of Fe(NO3)3·9H2O and Na2S2O3·5H2O is 5:

1.

4. The preparation method according to claim 1, characterized in that: The reaction temperature is 80-90°C.

5. The preparation method according to claim 1, characterized in that: The reaction time is 8-10h.

6. The preparation method according to claim 1, characterized in that: The concentration of the hydrochloric acid solution is 2-4 mol / L, and the ultrasonic time is 4-6 min.

7. The preparation method according to claim 1, characterized in that: After washing 3-5 times, the drying temperature is 50-70°C and the drying time is 2-4 hours.

8. The preparation method according to claim 1, characterized in that: The drying temperature after the reaction is 80-120°C and the drying time is more than 6 hours.

9. The Fe@Ni3S2 / NF electrode material prepared by the preparation method according to any one of claims 1 to 8.

10. The Fe@Ni3S2 / NF electrode material according to claim 9, characterized in that The particle size of Ni3S2 in the electrode material is 400-500nm.