Preparation method and application of bimetallic conductive CuCo-HHTP complex / graphene composite material

By using bimetallic conductive CuCo-HHTP complex/graphene composite material and sulfur S8 in lithium sulfur batteries, the problem of poor conductivity of lithium sulfur batteries during charging and discharging is solved, and the electrochemical performance and rate performance are improved. Suitable for industrial production.

CN119050295APending Publication Date: 2024-11-29HENAN AGRICULTURAL UNIVERSITY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411125734.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

During the charging and discharging process of lithium sulfur batteries, there are problems such as poor conductivity, low utilization rate of active substances, poor rate performance and low Coulomb efficiency, especially due to the insulating properties of sulfur elements and intermediate products and the generation of lithium dendrites, the electrochemical performance is insufficient. .

Method used

Using bimetallic conductive CuCo-HHTP complex and graphene composite, an aqueous graphene solution was prepared by the improved Hummer's method, and mixed with Cu, Co, HHTP ligands, stirred and reacted at 85°C, followed by precipitation of sulfur S8. Combined, the positive electrode material used for lithium sulfur batteries is prepared by argon calcination.

Benefits of technology

It improves the conductivity of the cathode material of lithium sulfur battery and improves the electrochemical performance. It is suitable for large-scale industrial production, is cheap, and the material shows good cycle stability and rate performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119050295A_ABST
    Figure CN119050295A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of a bimetallic conductive CuCo-HHTP complex / graphene composite material, and belongs to the technical field of composite material preparation. The preparation method comprises the following specific steps: preparing a graphene oxide aqueous solution; the method comprises the following steps: dissolving a copper source and a cobalt source in a graphene oxide aqueous solution to prepare a solution A; adding a ligand HHTP into a mixed solution of DMF and ammonia water to prepare a solution B; adding the solution B while stirring the solution A, then pouring into a reaction kettle, and reacting for 2 hours at the temperature of 85 DEG C to prepare a bimetallic conductive CuCo-HHTP complex / graphene composite material; and finally, compounding with settled sulfur S8 to be used as the positive electrode material of the lithium-sulfur battery. According to the present invention, the sulfur is compounded in the host material to improve the conductivity of the active material sulfur, and the sulfur compounded host material is applied to the lithium-sulfur battery, such that the sulfur compounded host material can provide good electrochemical performance in the lithium-sulfur battery so as to provide the possibility for the future application of the lithium-sulfur battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite material preparation, and in particular relates to a method for preparing a bimetallic conductive CuCo-HHTP complex / graphene composite material used for positive electrode materials of lithium-sulfur batteries. Background Art

[0002] Electrochemical energy storage technology is a key step in energy conversion. It plays a pivotal role in temporarily storing other energy sources and then applying them in other places. It can not only effectively store renewable energy sources, such as tidal energy and solar energy, but these energy sources are not stable enough and are also intermittent. However, they can be stored through energy storage devices and applied to other places. Since the 1970s, lithium-sulfur batteries have gone through several important development stages. In the early stages of development, lithium-sulfur batteries faced the problem that polysulfide lithium was difficult to oxidize again, which resulted in only one discharge, that is, only a single battery. This problem prompted researchers to explore new electrolyte systems to achieve reversible cycles. In the late 1970s, researchers studied a variety of electrolyte systems and finally successfully achieved reversible cycles at room temperature. The successful breakthrough of electrolytes has become a key step in the commercialization of lithium-sulfur batteries. Later, researchers began to gradually analyze the electrochemical reaction mechanism of lithium-sulfur batteries. With the in-depth study of the reaction mechanism of lithium-sulfur batteries, scientists began to explore the conversion mechanism of sulfur positive electrodes, including adsorption models, lithium ion diffusion models, etc., which provided theoretical support for the optimization route of lithium-sulfur batteries. Finally, there is the research on solid-state electrolytes. In recent times, the research on all-solid lithium-sulfur batteries has become a hot topic. All-solid-state lithium-sulfur batteries can provide higher energy density and safety. However, the discharge capacity of all-solid-state batteries is usually lower than the theoretical value, indicating that all-solid-state lithium-sulfur batteries need to be further optimized in terms of material utilization and electrochemistry. Lithium-sulfur batteries have attracted much attention due to their high energy density. Thanks to sulfur as the main active substance, it is abundant in nature and inexpensive, so using sulfur as an active material will reduce costs.

[0003] Lithium-sulfur batteries are more environmentally friendly and have no heavy metal pollution compared to lithium-ion batteries. In the earliest lithium-sulfur batteries, sulfur was simply used as the negative electrode and lithium metal as the positive electrode. However, there is a different reaction process in lithium-sulfur batteries. The special thing about lithium-sulfur batteries is that they start with discharge. In this process, the positive electrode will oxidize to Li +, and then react with sulfur at the positive electrode to form Li2S, and then convert into sulfur and Li2S8 during the charging process. Because the intermediate products and sulfur are non-conductive during this conversion process, this will affect the transfer of charge and thus the electrochemical performance. Although lithium-sulfur batteries have many advantages, there are still many shortcomings in the electrochemical performance of the battery, including low utilization of active materials, poor rate performance and low coulombic efficiency. Commercialization requires solutions to key issues such as non-conductive discharge products and soluble intermediates, the increase in volume of lithium-sulfur batteries during charging and discharging, and the growth of lithium dendrites.

[0004] Problems with lithium-sulfur batteries: insulation of sulfur and discharge products, dissolution of products in the intermediate process, volume change of sulfur electrode, and generation of lithium dendrites. The key component of the composite positive electrode of lithium-sulfur batteries is the sulfur host material, which plays an important role in lithium-sulfur batteries, and improves the conductivity of sulfur itself through the host material. By characterizing the synthesized positive electrode conductive material and related tests on the electrochemical performance of lithium-sulfur batteries, an effective way is provided for the application of this positive electrode material in lithium-sulfur batteries. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a bimetallic conductive CuCo-HHTP complex / graphene composite material. The bimetallic conductive CuCo-HHTP complex / graphene composite material prepared by the preparation method can be used as a positive electrode material in a lithium-sulfur battery.

[0006] To achieve the above object, the technical solution adopted by the present invention is: A method for preparing a bimetallic conductive CuCo-HHTP complex / graphene composite material, the specific steps are as follows: (1) Preparation of graphene oxide aqueous solution Graphene oxide was prepared by using the improved Hummer's method, and deionized water was added and ultrasonicated for 40 min to prepare a graphene oxide aqueous solution. (2) Preparation of bimetallic conductive CuCo-HHTP complex / graphene composites A certain amount of copper acetate tetrahydrate and cobalt acetate tetrahydrate were weighed and dissolved in the graphene oxide aqueous solution, stirred for 30 min to prepare solution A; the ligand HHTP was added to the mixed solution of DMF and ammonia water, stirred for 20 min to prepare solution B; solution B was added while stirring solution A, the solution turned dark blue, and stirring was continued for 30 min; then the mixed solution was poured into a reactor and reacted at 85°C for 2 h; after the reaction, the solution was transferred to a centrifuge tube, washed with ethanol and deionized water 4 times each, and freeze-dried at -60°C to obtain a bimetallic conductive CuCo-HHTP complex / graphene composite material.

[0007] Furthermore, the bimetallic conductive CuCo-HHTP complex / graphene composite material is combined with precipitated sulfur S8 to be used as a positive electrode material for a lithium-sulfur battery.

[0008] Furthermore, the process of compounding the bimetallic conductive CuCo-HHTP complex / graphene composite material with precipitated sulfur S8 is as follows: the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in step (2) and precipitated sulfur S8 are uniformly mixed and then transferred to a porcelain boat, and calcined under argon conditions to obtain a positive electrode material for a lithium-sulfur battery.

[0009] Furthermore, the concentration of the graphene oxide aqueous solution in step (1) is 0-5 mg / mL.

[0010] Furthermore, in step (2), the molar ratio of Cu to Co is 1-49:1.

[0011] Furthermore, in the step (2), the mass ratio of Cu to graphene oxide is 3-8:25.

[0012] Furthermore, in the step (2), the molar ratio of the metals Cu and Co to the ligand HHTP is 2:1.

[0013] Furthermore, the mass ratio of the bimetallic conductive CuCo-HHTP complex / graphene composite material to the precipitated sulfur S8 is 2-3:7-8, preferably 3:7.

[0014] Furthermore, the calcination temperature of the molten sulfur-carrying material is 155° C., and the calcination time is 12 hours.

[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention improves the conductivity of active material sulfur by compounding sulfur in a host material and applies it to a lithium-sulfur battery. The sulfur-compounded host material can exhibit good electrochemical properties in a lithium-sulfur battery, providing possibilities for the future application of lithium-sulfur batteries.

[0016] 2. The present invention has low cost and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a scanning electron microscope photograph of the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in Example 1; Figure 2 is the X-ray diffraction pattern of the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in Example 1; Figure 3This is a scanning electron microscope photograph of the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in Example 2; Figure 4 is the X-ray diffraction pattern of the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in Example 2; Figure 5 This is a scanning electron microscope photograph of the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in Example 3; Figure 6 is the X-ray diffraction pattern of the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in Example 3; Figure 7 The cyclic voltammetry test diagram of Test Example 1 as the positive electrode of a lithium-sulfur battery; Figure 8 The cyclic voltammetry test diagram of Test Example 2 as the positive electrode of a lithium-sulfur battery; Fig. 9 The cyclic voltammetry test diagram of Test Example 3 as the positive electrode of a lithium-sulfur battery; Fig.10 The cycle performance diagram of testing Example 1, Example 2, and Example 3 as the positive electrode of a lithium-sulfur battery; Fig.11 To test the electrochemical impedance diagram of Example 1, Example 2, and Example 3 as the positive electrode of a lithium-sulfur battery; Fig.12 This is a rate performance diagram for testing Example 1, Example 2, and Example 3 as positive electrodes for lithium-sulfur batteries. DETAILED DESCRIPTION

[0018] The technical solution and effects of the present invention are further described below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereto.

[0019] The invention provides a method for preparing a bimetallic conductive CuCo-HHTP complex / graphene composite material. The specific steps are as follows: firstly preparing a graphene oxide aqueous solution, and then preparing the bimetallic conductive CuCo-HHTP complex / graphene composite material.

[0020] The present invention adopts an improved Hummer's method to prepare graphene oxide (this part is the prior art and will not be repeated in the present invention), adds a certain amount of deionized water to the graphene oxide, and ultrasonicates for 40 minutes to prepare a graphene oxide aqueous solution. The concentration of the graphene oxide aqueous solution in the present invention is 0-5 mg / mL. As a specific embodiment, the concentration of the graphene oxide aqueous solution prepared by the present invention is 2 mg / mL, but it is not limited thereto, and 0.1 mg / mL, 0.5 mg / mL, 1 mg / mL, 3 mg / mL, 4 mg / mL, and 5 mg / mL can also be used.

[0021] The preparation of bimetallic conductive CuCo-HHTP complex / graphene composite material is the core of the present invention. The specific steps are: weigh a certain amount of copper acetate tetrahydrate and cobalt acetate tetrahydrate, dissolve them in a graphene oxide aqueous solution, stir for 30 minutes, and prepare solution A; add the ligand HHTP (2,3,6,7,10,11-hexahydroxytriphenyl) to a mixed solution of DMF and ammonia water, stir for 20 minutes, and prepare solution B; add solution B while stirring solution A, the solution turns dark blue, and continue to stir for 30 minutes; then pour the mixed solution into a reactor and react at 85°C for 2 hours; after the reaction is completed, transfer the solution to a centrifuge tube, and wash it with ethanol and deionized water 4 times each, and freeze-dry at -60°C to obtain a bimetallic conductive CuCo-HHTP complex / graphene composite material.

[0022] Among them, the molar ratio of Cu and Co is 1-49:1-49. As some embodiments of the present invention, the molar ratio of Cu and Co can be selected as 1-49:1. The inventors found that the greater the proportion of Cu content, the better the electrochemical performance of the composite material after being used as a positive electrode material for lithium-sulfur batteries. As a specific embodiment, the molar ratio of Cu and Co is 1:1, 4:1, 49:1. The molar ratio of the two metals Cu and Co to the ligand HHTP is 2:1. The inventors found that when the molar ratio of the metal to the ligand HHTP in the bimetallic conductive CuCo-HHTP complex / graphene composite material is 2:1, it is useful for the composite material to be used as a positive electrode material. When the amount of graphene oxide is 3-8:25, the mass ratio of Cu to graphene oxide is useful for the composite material to be used as a positive electrode material.

[0023] There is no particular restriction on the amount of DMF and ammonia water used in solution B. As long as the appropriate concentration of the ligand HHTP is ensured, the mass concentration of ammonia water in solution B can be 0.0091 g / L, the volume ratio of DMF to ammonia water is 25:0.6, and the mass concentration of the ligand HTTP is 1.625 mg / mL.

[0024] Reaction Conditions of Mixed Solution The inventors found that reaction at 85° C. for 2 h is useful for preparing the composite material of the present invention.

[0025] When the prepared composite material is used, the bimetallic conductive CuCo-HHTP complex / graphene composite material needs to be compounded with precipitated sulfur S8 for use as a positive electrode material for a lithium-sulfur battery. The compounding process of the bimetallic conductive CuCo-HHTP complex / graphene composite material and the precipitated sulfur S8 is as follows: the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in step (2) and the precipitated sulfur S8 are evenly mixed and transferred to a porcelain boat, and calcined under argon conditions to obtain a positive electrode material for a lithium-sulfur battery. When compounded with the precipitated sulfur S8, the mass ratio of the bimetallic conductive CuCo-HHTP complex / graphene composite material to the precipitated sulfur S8 is 2-3:7-8, preferably 3:7. The calcination temperature of the molten sulfur carrier is 155°C, and the calcination time is 12h. Example 1

[0026] This embodiment provides a method for preparing a bimetallic conductive CuCo-HHTP complex / graphene composite material, and the specific steps are as follows: (1) Preparation of graphene oxide aqueous solution 100 mg of graphene oxide prepared by the improved Hummer's method was taken, and 25 mL of deionized water was added to prepare a 4 mg / mL graphene oxide aqueous solution, which was placed in an ultrasonic cleaner for 40 minutes to form a uniformly dispersed graphene oxide aqueous dispersion.

[0027] (2) Preparation of bimetallic conductive CuCo-HHTP complex / graphene composites Weigh 0.0499 g of copper acetate tetrahydrate and 0.0623 g of cobalt acetate tetrahydrate and dissolve them in graphene oxide aqueous dispersion (Cu:Co=1:1), continue stirring for 30 min, and prepare solution A. Mix a mixed solution of 25 mL of DMF and 0.6 mL of ammonia water with 81.25 mg of ligand HHTP and stir for 20 min to prepare solution B. Add solution B while stirring solution A, the solution turns dark blue, and continue stirring for 30 min. After stirring, pour the solution into the reactor and react at 85°C for 2 h. After the reaction is completed, transfer the solution to a centrifuge tube and wash it four times with ethanol and deionized water. Finally, freeze-dry in a freeze dryer to obtain the final product.

[0028] (3) Sulfur compounding process The material synthesized in (2) and precipitated sulfur (S8) (0.07 g) were mixed evenly in a mass ratio of 3:7 and transferred to a porcelain boat, which was then placed in a tube furnace filled with argon and sealed. The tube furnace was heated to 155°C and calcined for 12 h.

[0029] Figure 1 This is a scanning electron microscope photo of the bimetallic conductive CuCo-HHTP complex / graphene composite material obtained in Example 1 of the present invention. Figure 1 It can be seen that the material forms a two-dimensional layered structure, which is relatively uniform and has a certain specific surface area. Figure 2 The X-ray diffraction pattern of the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in Example 1 of the present invention has obvious characteristic peaks at 2θ=10° and 2θ=14°, which is very similar to the well-crystallized CuCo-MOF crystal. Example 2

[0030] This embodiment provides a method for preparing a bimetallic conductive CuCo-HHTP complex / graphene composite material, and the specific steps are as follows: (1) Preparation of graphene oxide aqueous solution Graphene oxide was prepared using the improved Hummer's method. A certain amount of deionized water was added to prepare 25 mL, 4 mg / mL graphene oxide aqueous dispersion, which was placed in an ultrasonic cleaner for 40 minutes to evenly disperse the graphene oxide and deionized water.

[0031] (2) Preparation of bimetallic conductive CuCo-HHTP complex / graphene composites Weigh 0.0799 g of copper acetate tetrahydrate and 0.0249 g of cobalt acetate tetrahydrate and dissolve them in graphene oxide aqueous dispersion (Cu:Co=4:1), continue stirring for 30 min, and prepare solution A. Mix a mixed solution of 25 mL of DMF and 0.6 mL of ammonia water with 81.25 mg of ligand HHTP and stir for 20 min to prepare solution B. Add solution B while stirring solution A, the solution turns dark blue, and continue stirring for 30 min. After stirring, pour the solution into the reactor and react at 85°C for 2 h. After the reaction is completed, transfer the solution to a centrifuge tube and wash it four times with ethanol and deionized water. Finally, freeze-dry in a freeze dryer to obtain the final product.

[0032] (3) Sulfur compounding process The material synthesized in (2) and precipitated sulfur (S8) (0.07 g) were mixed evenly in a mass ratio of 3:7 and transferred to a porcelain boat, which was then placed in a tube furnace filled with argon and sealed. The tube furnace was heated to 155°C and calcined for 12 h.

[0033] Figure 3 This is a scanning electron microscope photo of the bimetallic conductive CuCo-HHTP complex / graphene composite material obtained in Example 2 of the present invention. Figure 3It can be seen that the material forms a two-dimensional layered structure, which is relatively uniform and has a certain specific surface area. Figure 4 The X-ray diffraction pattern of the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in Example 2 of the present invention has obvious characteristic peaks at 2θ=10° and 2θ=14°. As the Cu content increases, the number of diffraction peaks increases and the intensity increases, which indicates that the crystallinity is improved compared to the material ratio of Example 1 (Cu:Co=1:1). Example 3

[0034] This embodiment provides a method for preparing a bimetallic conductive CuCo-HHTP complex / graphene composite material, and the specific steps are as follows: (1) Preparation of graphene oxide aqueous solution Graphene oxide was prepared by using the improved Hummer's method. A certain amount of deionized water was added to prepare 25 mL, 4 mg / mL graphene oxide aqueous dispersion, which was placed in an ultrasonic cleaner for 40 minutes to evenly disperse the graphene oxide and deionized water.

[0035] (2) Preparation of bimetallic conductive CuCo-HHTP complex / graphene composites Weigh 0.0978 g of copper acetate tetrahydrate and 0.0025 g of cobalt acetate tetrahydrate and dissolve them in graphene oxide aqueous dispersion (Cu:Co=98:2), continue stirring for 30 min, and prepare solution A. Mix a mixed solution of 25 mL of DMF and 0.6 mL of ammonia water with 81.25 mg of ligand HHTP and stir for 20 min to prepare solution B. Add solution B while stirring solution A, the solution turns dark blue, and continue stirring for 30 min. After stirring, pour the solution into the reactor and react at 85°C for 2 h. After the reaction is completed, transfer the solution to a centrifuge tube and wash it four times with ethanol and deionized water. Finally, freeze-dry in a freeze dryer to obtain the final product.

[0036] (3) Sulfur compounding process The material synthesized in (2) and precipitated sulfur (S8) (0.07 g) were mixed evenly in a mass ratio of 3:7 and transferred to a porcelain boat, which was then placed in a tube furnace filled with argon and sealed. The tube furnace was heated to 155°C and calcined for 12 h.

[0037] Figure 5 This is a scanning electron microscope photo of the bimetallic conductive CuCo-HHTP complex / graphene composite material obtained in Example 3 of the present invention. Figure 5 It can be seen that the material forms a two-dimensional layered structure, which is relatively uniform and has a certain specific surface area. Figure 6The X-ray diffraction pattern of the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in Example 3 of the present invention has obvious characteristic peaks at 2θ=10° and 2θ=14°, which is very similar to the well-crystallized CuCo-MOF crystal.

[0038] In order to explore the performance of the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in Example 1, Example 2, and Example 3 as an electrode material for lithium-sulfur batteries, the cycle performance of the battery was tested. The current density during the test was 0.1 mV·s -1 , the voltage range is 1.7 V-2.8 V, Figure 7 , Figure 8 , Fig. 9 The CV curves of the first three weeks and the first half of the fourth week are shown. During the scanning process, two peaks appeared, near 2.3 V and 2.4 V respectively. The cycles of the second and third weeks are very similar, indicating that the stability inside the battery is good. It can be seen that Example 3 has a higher reduction potential and a lower oxidation potential, indicating that the polarization degree of the material in Example 3 is lower during the reaction. The three materials prepared in Examples 1-3 were analyzed for cycle performance. Fig.10 It can be seen that at 0.5 C, the capacity of the three batteries all showed obvious attenuation as the cycle progressed. The specific capacities of Example 1, Example 2, and Example 3 in the first week were 1392 mAh·g -1 、1121 mAh·g -1 、977 mAh·g -1 , the capacity is 480 mAh·g at 50 and 120 cycles respectively. - 1 、526 mAh·g -1 、658 mAh·g -1 ; 421 mAh g -1 、422 mAh·g -1 、597 mAh·g -1 , the specific capacity at 200 cycles is 361 mAh·g -1 、367 mAh·g -1 、561 mAh·g -1. At 200 weeks, the capacity retention rates of the three materials were 40.3%, 32.7%, and 36.9%, respectively. In general, the discharge specific capacity of the material in Example 3 is higher than that in Example 1 and Example 2. From the voltage capacity diagram of cf, it can be seen that the discharge platform of the material in Example 3 is the longest from the first week to the 200th week, and the voltage difference between the two platforms is the smallest, indicating its faster reaction kinetics. As the cycle progresses, the subsequent voltage platforms are all between 2.0 V and 2.1 V, indicating that the internal materials of the battery have stabilized.

[0039] Impedance analysis was performed on the three materials obtained in Examples 1-3. Fig.11 It can be seen that Example 2 has the smallest semicircle diameter, indicating that its Rct internal resistance is the smallest. Overall, with the increase of Cu content, the Rct internal resistance first decreases and then tends to expand, indicating that with the increase of Cu content, the conductive performance may eventually decrease.

[0040] The rate performance of the three materials obtained in Examples 1-3 was analyzed. Fig.12 It can be seen that there is little difference between Example 2 and Example 3 at 0.1 C, while the electrochemical performance of Example 1 is significantly worse. As the current density increases, Example 3 shows better rate performance. It can be seen that Example 3 can maintain a better working state at a high rate. The coulombic efficiency of the three materials has almost no change, indicating that the three materials have good stability during the working process. Overall, with the increase of Cu content, the rate performance tends to improve.

[0041] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A method for preparing a bimetallic conductive CuCo-HHTP complex / graphene composite material, characterized in that: The specific steps of the preparation method are as follows: (1) Preparation of graphene oxide aqueous solution Graphene oxide was prepared by using the improved Hummer's method, and deionized water was added and ultrasonicated for 40 min to prepare a graphene oxide aqueous solution. (2) Preparation of bimetallic conductive CuCo-HHTP complex / graphene composites A certain amount of copper acetate tetrahydrate and cobalt acetate tetrahydrate were weighed and dissolved in the graphene oxide aqueous solution, stirred for 30 min to prepare solution A; the ligand HHTP was added to the mixed solution of DMF and ammonia water, stirred for 20 min to prepare solution B; solution B was added while stirring solution A, the solution turned dark blue, and stirring was continued for 30 min; then the mixed solution was poured into a reactor and reacted at 85°C for 2 h; after the reaction, the solution was transferred to a centrifuge tube, washed with ethanol and deionized water 4 times each, and freeze-dried at -60°C to obtain a bimetallic conductive CuCo-HHTP complex / graphene composite material.

2. The method for preparing the bimetallic conductive CuCo-HHTP complex / graphene composite material according to claim 1, characterized in that: The bimetallic conductive CuCo-HHTP complex / graphene composite material is combined with precipitated sulfur S8 to form a positive electrode material for a lithium-sulfur battery.

3. The method for preparing the bimetallic conductive CuCo-HHTP complex / graphene composite material according to claim 2, characterized in that: The process of compounding the bimetallic conductive CuCo-HHTP complex / graphene composite material with precipitated sulfur S8 is as follows: the bimetallic conductive CuCo-HHTP complex / graphene composite material prepared in step (2) and precipitated sulfur S8 are uniformly mixed and then transferred to a porcelain boat, and calcined under argon conditions to obtain a positive electrode material for a lithium-sulfur battery.

4. The method for preparing the bimetallic conductive CuCo-HHTP complex / graphene composite material according to claim 3, characterized in that: The mass ratio of the bimetallic conductive CuCo-HHTP complex / graphene composite material to the precipitated sulfur S8 is 2-3:7-8.

5. The method for preparing the bimetallic conductive CuCo-HHTP complex / graphene composite material according to claim 3, characterized in that: The calcination temperature of the molten sulfur-carrying agent is 155° C. and the calcination time is 12 hours.

6. The method for preparing the bimetallic conductive CuCo-HHTP complex / graphene composite material according to claim 1, characterized in that: The concentration of the graphene oxide aqueous solution in step (1) is 0-5 mg / mL.

7. The method for preparing the bimetallic conductive CuCo-HHTP complex / graphene composite material according to claim 1, characterized in that: The molar ratio of Cu to Co in the step (2) is 1-49:

1.

8. The method for preparing the bimetallic conductive CuCo-HHTP complex / graphene composite material according to claim 1, characterized in that: In the step (2), the mass ratio of Cu to graphene oxide is 3-8:

25.

9. The method for preparing the bimetallic conductive CuCo-HHTP complex / graphene composite material according to claim 1, characterized in that: In the step (2), the molar ratio of the metals Cu and Co to the ligand HHTP is 2:1.

Citation Information

Cited By

  • NH3 gas sensor based on high-conductivity bimetallic Co / Cu-HHTP sensitive material and preparation method thereof

    CN116482189A

  • An NH3 gas sensor based on highly conductive bimetallic Co / Cu-HHTP sensitive material and its preparation method

    CN116482189B