Hard carbon negative electrode material and preparation method and application thereof

Through the combination of starch, phenolic resin, phosphoric acid and coating agent, a stable hard carbon negative electrode material is prepared, which solves the problem of expansion and fusion of hard carbon materials during the preparation process, and improves the electrochemical performance and cycle stability of the battery. .

CN119050348APending Publication Date: 2024-11-29SOUTH CHINA NORMAL UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411159011.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing hard carbon anode materials are prone to expand and merge during the preparation process, resulting in a decrease in electrochemical performance and complex phosphoric acid leaching treatment, affecting the material performance.

Method used

Using starch, phenolic resin, phosphoric acid and coating agent as raw materials, hard carbon negative electrode materials are prepared through crosslinking, acid leaching, coating and carbonization steps, and phosphoric acid is used to remove impurities and doped phosphorus elements to form a porous structure to improve conductivity and Specific capacity.

Benefits of technology

The stable preparation of hard carbon negative electrode materials is achieved, the specific capacity of the battery and the first-time Coulomb efficiency are improved, the conductivity and cyclic stability of the material are ensured, and the electrochemical performance is excellent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005903900000071
    Figure BDA0005005903900000071
  • Figure BDA0005005903900000081
    Figure BDA0005005903900000081
  • Figure HDA0005005903910000011
    Figure HDA0005005903910000011
Patent Text Reader

Abstract

The invention relates to the technical field of battery materials, and discloses a hard carbon negative electrode material and a preparation method and application thereof. The hard carbon negative electrode material is prepared from the following raw materials: starch, phenolic resin, phosphoric acid and a coating agent. The hard carbon negative electrode material provided by the invention is easy to obtain and low in cost, through phenolic resin crosslinking treatment, expansion and fusion of starch in the carbonization process can be prevented, the microsphere structure of the starch can be prevented from being damaged, the hard carbon negative electrode material can be prepared through phosphoric acid leaching impurity removal, phosphorus doping, coating agent coating and carbonization, and the preparation method is simple. Phosphoric acid leaching treatment is beneficial to change of graphite interlamellar spacing and formation of defects, and doping of phosphorus can better control the structure of hard carbon in the carbonization process, so that the material performance is improved, and the specific capacity and the first coulombic efficiency of the battery are improved; closed pores can be manufactured through coating of the coating agent, the conductivity of the hard carbon negative electrode material is improved, direct contact between electrolyte and hard carbon is reduced, and the first coulombic efficiency of the battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a hard carbon negative electrode material and a preparation method and application thereof. Background Art

[0002] Lithium-ion batteries (LIBs) dominate various battery energy storage technologies due to their high energy density, excellent cycle performance, long life, and high output power. However, the global lithium resources are unevenly distributed and high-grade lithium ore is scarce, resulting in an increasing cost of raw materials for lithium-ion batteries, and the development of alternative battery technologies continues. Sodium is a member of the same family as lithium, has abundant reserves in the earth's crust, and is cheap. Sodium-ion batteries (SIBs) have obvious cost advantages. SIBs have a similar structure to LIBs, and can use the technology and equipment used in LIB production, thereby reducing production costs. Therefore, sodium-ion batteries have great development potential, and advanced negative electrode materials are the key to the development of sodium-ion batteries.

[0003] As a key part of sodium-ion batteries, negative electrode materials can generally be divided into four types: carbon-based materials, metal oxides, alloys and organic matter. However, the above materials have defects such as complex preparation process and poor electrochemical properties, which limits the practical application of sodium-ion batteries. Carbon-based materials are abundant in resources, low in cost and simple to produce, including soft carbon (SC) and hard carbon (HC). SC has a relatively low ICE due to its high degree of graphitization, limited interlayer distance and weak competitiveness; HC has the advantages of diverse structures, low price, good conductivity, high sodium storage capacity, small volume deformation after sodium insertion, environmental friendliness and low redox potential, and is considered to be the most promising negative electrode material for sodium-ion batteries.

[0004] Currently, a variety of precursors have been used to prepare hard carbon, such as polymers such as polyacrylonitrile, epoxy resins and phenolic resins, as well as biomass such as starch, bamboo, bagasse and coffee grounds. Among them, starch as a raw material has the advantages of being green, environmentally friendly, widely available and renewable, but direct high-temperature sintering of starch particles will cause the microsphere structure of starch particles to be destroyed and expand and fuse due to the diffusion of water and small molecules, which will eventually affect the electrochemical properties of the finished material. Summary of the invention

[0005] The present invention aims to solve at least one of the above-mentioned technical problems existing in the prior art. To this end, one of the purposes of the present invention is to provide a hard carbon negative electrode material; the second purpose of the present invention is to provide a method for preparing the hard carbon negative electrode material; the third purpose of the present invention is to provide a negative electrode sheet; the fourth purpose of the present invention is to provide a sodium ion battery.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A first aspect of the present invention provides a hard carbon negative electrode material, comprising the following preparation raw materials: starch, phenolic resin, phosphoric acid and a coating agent.

[0008] Preferably, the starch includes at least one of corn starch, potato starch, wheat starch, tapioca starch, rice starch, mung bean starch, pea starch and sweet potato starch.

[0009] Preferably, the mass ratio of the starch to the phenolic resin is 100:(10-70); further preferably, the mass ratio of the starch to the phenolic resin is 100:(40-50).

[0010] Preferably, the concentration of the phosphoric acid is 0.5-6 mol / L; further preferably, the concentration of the phosphoric acid is 1-3 mol / L.

[0011] Preferably, the mass of the coating agent is 0.1-10% of the total mass of the starch and the phenolic resin; further preferably, the mass of the coating agent is 2-4% of the total mass of the starch and the phenolic resin.

[0012] Preferably, the coating agent includes at least one of asphalt and industrial syrup; further preferably, the coating agent is asphalt.

[0013] The second aspect of the present invention provides a method for preparing the hard carbon negative electrode material according to the first aspect of the present invention, comprising the following steps:

[0014] S1, mixing starch and phenolic resin, and ball milling to obtain cross-linked starch;

[0015] S2, subjecting the cross-linked starch to phosphoric acid leaching to obtain activated starch,

[0016] S3, mixing the activated starch with a coating agent to obtain coated starch;

[0017] S4, carbonizing the coated starch to obtain the hard carbon negative electrode material.

[0018] Preferably, in step S1, the particle size of the cross-linked starch is less than 80 μm; further preferably, the particle size of the cross-linked starch is 50-70 μm.

[0019] Preferably, in step S2, the acid leaching time is 1-3 hours; more preferably, the acid leaching time is 1.5-2.5 hours. Phosphoric acid can be used to remove impurities such as lignin and hemicellulose in starch, and can also be used as a precursor for phosphorus doping to achieve phosphorus doping.

[0020] Preferably, in step S2, after the acid leaching is completed, washing and drying steps are also included.

[0021] Preferably, in step S3, the specific operation of mixing the activated starch with the coating agent is: dissolving the coating agent in an organic solvent to form a mixed solution, and then mixing the mixed solution with the activated starch for coating.

[0022] Preferably, the solid-liquid ratio of the coating agent to the organic solvent is (3-5) mg:1 mL; further preferably, the solid-liquid ratio of the coating agent to the organic solvent is (3.5-4.5) mg:1 mL.

[0023] Preferably, the organic solvent comprises tetrahydrofuran.

[0024] Preferably, in step S3, the temperature at which the activated starch and the coating agent are mixed is 35-45°C; further preferably, the temperature at which the activated starch and the coating agent are mixed is 37-42°C.

[0025] Preferably, in step S3, the activated starch and the coating agent are mixed for 1-2 hours; further preferably, the activated starch and the coating agent are mixed for 1-1.5 hours.

[0026] Preferably, in step S4, the carbonization temperature rising program is as follows: the initial temperature is 18-22°C, the temperature is raised to 350-450°C at a rate of 0.5-10°C / min, and the temperature is kept for 1.5-2.5h; the temperature is then raised to 900-1600°C at a rate of 0.5-10°C / min, and the temperature is kept for 1.5-2.5h; further preferably, the carbonization temperature rising program is as follows: the initial temperature is 18-22°C, the temperature is raised to 390-410°C at a rate of 1.5-2.5°C / min, and the temperature is kept for 1.8-2.3h; the temperature is then raised to 1000-1500°C at a rate of 1.5-2.5°C / min, and the temperature is kept for 1.7-2.2h.

[0027] Preferably, in step S4, the carbonization is performed under an inert atmosphere; the inert gas includes one of argon and nitrogen.

[0028] The third aspect of the present invention provides a negative electrode plate, comprising the hard carbon negative electrode material described in the first aspect of the present invention.

[0029] Preferably, the negative electrode plate further includes a conductive agent, an adhesive and a solvent.

[0030] Preferably, the mass ratio of the hard carbon negative electrode material, the conductive agent and the adhesive is (7-9):(0.8-1.2):1.

[0031] Preferably, the conductive agent includes carbon black (Super-P).

[0032] Preferably, the binder comprises carboxymethyl cellulose (CMC).

[0033] Preferably, the solvent comprises deionized water.

[0034] Preferably, the negative electrode plate is prepared by a method comprising the following steps: mixing the hard carbon negative electrode material, a conductive agent, an adhesive and a solvent, and coating the mixture on a copper foil current collector to obtain the negative electrode plate.

[0035] The fourth aspect of the present invention provides a sodium ion battery, comprising the negative electrode sheet described in the third aspect of the present invention.

[0036] Preferably, the sodium ion battery uses metallic sodium as the counter electrode.

[0037] Preferably, the electrolyte of the sodium ion battery includes sodium hexafluorophosphate electrolyte.

[0038] Compared with the prior art, the present invention has the following beneficial effects:

[0039] 1) The hard carbon negative electrode material provided by the present invention is easy to obtain and has low cost. It can prevent starch from swelling and melting during the carbonization process and prevent its microsphere structure from being destroyed after being cross-linked with phenolic resin. It can then be prepared by phosphoric acid leaching to remove impurities and doping with phosphorus, coating with a coating agent and carbonization. The preparation method is simple.

[0040] 2) Phosphoric acid leaching treatment is beneficial to changing the spacing between graphite layers and forming defects. The doping of phosphorus can better control the structure of hard carbon during the carbonization process, thereby improving material performance and increasing the specific capacity and first coulombic efficiency of the battery. Phosphoric acid leaching removes inorganic impurities and activates them, and also provides a basis for the subsequent preparation of porous materials. The coating agent coating converts open pores into closed pores, which can improve the conductivity of the hard carbon negative electrode material and reduce the direct contact between the electrolyte and the hard carbon, thereby improving the first coulombic efficiency of the battery.

[0041] 3) Hard carbon negative electrode materials are used to prepare negative electrode sheets and assemble sodium ion batteries, at 30 mAh g -1 The discharge capacity at a current density of 369.54 mAh g -1 , the charging capacity can reach 296mAh g -1 The first coulombic efficiency can reach 82.31%, with high charge and discharge efficiency, good cycle stability and excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 The hard carbon negative electrode material in Example 1 corresponds to the sodium ion battery at 30 mA g -1 Schematic diagram of capacity and first coulombic efficiency at current density;

[0043] Figure 2 The hard carbon negative electrode material in Example 2 corresponds to the sodium ion battery at 30 mA g-1 Schematic diagram of capacity and first coulombic efficiency at current density;

[0044] Figure 3 The hard carbon negative electrode material in Comparative Example 1 corresponds to the sodium ion battery at 30 mA g -1 Schematic diagram of capacity and first coulombic efficiency at different current densities. DETAILED DESCRIPTION

[0045] The present invention is further described in detail below by specific examples. Unless otherwise specified, the raw materials, reagents or devices used in the examples and comparative examples can be obtained from conventional commercial sources or can be obtained by prior art methods. Unless otherwise specified, the experiments or test methods are conventional methods in the art.

[0046] Example 1

[0047] This embodiment prepares a hard carbon negative electrode material, and the steps are as follows:

[0048] S1, mixing corn starch and phenolic resin in a mass ratio of 7:3, and ball milling to obtain cross-linked starch with a particle size of 5-70 μm;

[0049] S2, taking 20g of cross-linked starch, placing it in 200mL of 1mol / L phosphoric acid for acid washing and activation, stirring for 2h, then washing with deionized water until neutral, and drying to obtain activated starch;

[0050] S3, taking 0.4 g of asphalt and dissolving it in 100 mL of tetrahydrofuran to obtain a mixed solution, adding activated starch, and stirring at 40° C. for 1 h to obtain coated starch;

[0051] S4. Place the coated starch in a tubular furnace under the protection of inert gas, with an initial temperature of 20°C, heat it to 400°C at a heating rate of 2°C / min, keep it warm for 1 hour, then heat it to 1300°C at a heating rate of 2°C / min, keep it warm for 2 hours, then cool it to room temperature, carry out acid washing and drying, and obtain a hard carbon negative electrode material.

[0052] Example 2

[0053] This embodiment prepares a hard carbon negative electrode material, and the steps are as follows:

[0054] S1, mixing corn starch and phenolic resin in a mass ratio of 7:3, and ball milling to obtain cross-linked starch with a particle size of 5-70 μm;

[0055] S2, taking 20g of cross-linked starch, placing it in 200mL of 6mol / L phosphoric acid for acid washing and activation, stirring for 2h, then washing with deionized water until neutral, and drying to obtain activated starch;

[0056] S3, taking 0.4 g of asphalt and dissolving it in 100 mL of tetrahydrofuran to obtain a mixed solution, adding activated starch, and stirring at 40° C. for 1 h to obtain coated starch;

[0057] S4. Place the coated starch in a tubular furnace under the protection of inert gas, with an initial temperature of 20°C, heat it to 400°C at a heating rate of 2°C / min, keep it warm for 1 hour, then heat it to 1300°C at a heating rate of 2°C / min, keep it warm for 2 hours, then cool it to room temperature, carry out acid washing and drying, and obtain a hard carbon negative electrode material.

[0058] Example 3

[0059] This embodiment prepares a hard carbon negative electrode material, and the steps are as follows:

[0060] S1, mixing corn starch and phenolic resin in a mass ratio of 7:3, and ball milling to obtain cross-linked starch with a particle size of 5-70 μm;

[0061] S2, taking 20g of cross-linked starch, placing it in 200mL of 1mol / L phosphoric acid for acid washing and activation, stirring for 2h, then washing with deionized water until neutral, and drying to obtain activated starch;

[0062] S3, taking 0.4 g of asphalt and dissolving it in 100 mL of tetrahydrofuran to obtain a mixed solution, adding activated starch, and stirring at 40° C. for 1 h to obtain coated starch;

[0063] S4. Place the coated starch in a tubular furnace under the protection of inert gas, with an initial temperature of 20°C, heat it to 400°C at a heating rate of 2°C / min, keep it warm for 1 hour, then heat it to 1000°C at a heating rate of 2°C / min, keep it warm for 2 hours, then cool it to room temperature, carry out acid washing and drying, and obtain a hard carbon negative electrode material.

[0064] Example 4

[0065] This embodiment prepares a hard carbon negative electrode material, and the steps are as follows:

[0066] S1, mixing corn starch and phenolic resin in a mass ratio of 7:3, and ball milling to obtain cross-linked starch with a particle size of 5-70 μm;

[0067] S2, taking 20g of cross-linked starch, placing it in 200mL of 1mol / L phosphoric acid for acid washing and activation, stirring for 2h, then washing with deionized water until neutral, and drying to obtain activated starch;

[0068] S3, taking 0.4 g of asphalt and dissolving it in 100 mL of tetrahydrofuran to obtain a mixed solution, adding activated starch, and stirring at 40° C. for 1 h to obtain coated starch;

[0069] S4. Place the coated starch in a tubular furnace under the protection of inert gas, with an initial temperature of 20°C, heat it to 400°C at a heating rate of 2°C / min, keep it warm for 1 hour, then heat it to 1200°C at a heating rate of 2°C / min, keep it warm for 2 hours, then cool it to room temperature, carry out acid washing and drying, and obtain a hard carbon negative electrode material.

[0070] Example 5

[0071] This embodiment prepares a hard carbon negative electrode material, and the steps are as follows:

[0072] S1, mixing corn starch and phenolic resin in a mass ratio of 7:3, and ball milling to obtain cross-linked starch with a particle size of 5-70 μm;

[0073] S2, taking 20g of cross-linked starch, placing it in 200mL of 1mol / L phosphoric acid for acid washing and activation, stirring for 2h, then washing with deionized water until neutral, and drying to obtain activated starch;

[0074] S3, taking 0.4 g of asphalt and dissolving it in 100 mL of tetrahydrofuran to obtain a mixed solution, adding activated starch, and stirring at 40° C. for 1 h to obtain coated starch;

[0075] S4. Place the coated starch in a tubular furnace under the protection of inert gas, with an initial temperature of 20°C, heat it to 400°C at a heating rate of 2°C / min, keep it warm for 1 hour, then heat it to 1500°C at a heating rate of 2°C / min, keep it warm for 2 hours, then cool it to room temperature, pickle and dry it, and obtain a hard carbon negative electrode material.

[0076] Comparative Example 1

[0077] This comparative example prepares a hard carbon negative electrode material, which is different from Example 1 in that acid leaching is not performed, and the preparation steps are as follows:

[0078] S1, mixing corn starch and phenolic resin in a mass ratio of 7:3, and ball milling to obtain cross-linked starch with a particle size of 5-70 μm;

[0079] S2, take 20g of cross-linked starch and dry it;

[0080] S3, taking 0.4 g of asphalt and dissolving it in 100 mL of tetrahydrofuran to obtain a mixed solution, adding the dried cross-linked starch, and stirring at 40° C. for 1 h to obtain coated starch;

[0081] S4. Place the coated starch in a tubular furnace under the protection of inert gas, with an initial temperature of 20°C, heat it to 400°C at a heating rate of 2°C / min, keep it warm for 1 hour, then heat it to 1300°C at a heating rate of 2°C / min, keep it warm for 2 hours, then cool it to room temperature, carry out acid washing and drying, and obtain a hard carbon negative electrode material.

[0082] Comparative Example 2

[0083] This comparative example prepares a hard carbon negative electrode material. The difference from Example 1 is that acid leaching is not performed, but thiourea is used for S and N element doping. The preparation steps are as follows:

[0084] S1, mixing corn starch and phenolic resin in a mass ratio of 7:3, and ball milling to obtain cross-linked starch with a particle size of 5-70 μm;

[0085] S2, take 20g of cross-linked starch and add 3.5g of thiourea for doping;

[0086] S3, taking 0.4 g of asphalt and dissolving it in 100 mL of tetrahydrofuran to obtain a mixed solution, adding the doped cross-linked starch, and stirring at 40° C. for 1 h to obtain coated starch;

[0087] S4. Place the coated starch in a tubular furnace under the protection of inert gas, with an initial temperature of 20°C, heat it to 400°C at a heating rate of 2°C / min, keep it warm for 1 hour, then heat it to 1300°C at a heating rate of 2°C / min, keep it warm for 2 hours, then cool it to room temperature, carry out acid washing and drying, and obtain a hard carbon negative electrode material.

[0088] Comparative Example 3

[0089] This comparative example prepares a hard carbon negative electrode material, which is different from Example 1 in that hydrochloric acid is used for acid leaching. The preparation steps are as follows:

[0090] S1, mixing corn starch and phenolic resin in a mass ratio of 7:3, and ball milling to obtain cross-linked starch with a particle size of 5-70 μm;

[0091] S2, taking 20g of cross-linked starch, placing it in 200mL of 1mol / L hydrochloric acid for acid washing and activation, stirring for 2h, then washing with deionized water until neutral, and drying to obtain activated starch;

[0092] S3, taking 0.4 g of asphalt and dissolving it in 100 mL of tetrahydrofuran to obtain a mixed solution, adding the dried cross-linked starch, and stirring at 40° C. for 1 h to obtain coated starch;

[0093] S4. Place the coated starch in a tubular furnace under the protection of inert gas, with an initial temperature of 20°C, heat it to 400°C at a heating rate of 2°C / min, keep it warm for 1 hour, then heat it to 1300°C at a heating rate of 2°C / min, keep it warm for 2 hours, then cool it to room temperature, carry out acid washing and drying, and obtain a hard carbon negative electrode material.

[0094] Comparative Example 4

[0095] This comparative example prepares a hard carbon negative electrode material, which is different from Example 1 in that no coating agent is used, and the preparation steps are as follows:

[0096] S1, mixing corn starch and phenolic resin in a mass ratio of 7:3, and ball milling to obtain cross-linked starch with a particle size of 5-70 μm;

[0097] S2, taking 20g of cross-linked starch, placing it in 200mL of 1mol / L phosphoric acid for acid washing and activation, stirring for 2h, then washing with deionized water until neutral, and drying to obtain activated starch;

[0098] S3. Place the activated starch in a tubular furnace under the protection of inert gas, with an initial temperature of 20°C, heat it to 400°C at a heating rate of 2°C / min, keep it warm for 1 hour, then heat it to 1300°C at a heating rate of 2°C / min, keep it warm for 2 hours, then cool it to room temperature, carry out acid washing and drying, and obtain a hard carbon negative electrode material.

[0099] Preparation of negative electrode sheets and assembly of sodium-ion batteries

[0100] Take the hard carbon negative electrode material in Examples 1-5 and Comparative Examples 1-4, use carbon black (Super-P) as a conductive agent and carboxymethyl cellulose (CMC) as a binder, mix them in a mass ratio of hard carbon negative electrode material: conductive agent: binder = 8:1:1, add deionized water and stir, and evenly coat them on a copper foil current collector to obtain a negative electrode sheet.

[0101] The above negative electrode was used as the working electrode, metallic sodium was used as the counter electrode, and sodium hexafluorophosphate electrolyte 1MNaPF6 inEC:DMC (1:1 vol) was used as the electrolyte to assemble the sodium ion battery. All batteries were assembled in an argon-filled glove box (the oxygen and moisture contents were both less than 1 ppm).

[0102] Performance Testing

[0103] Using the battery test system Xinwei CT-4008Tn, at 25℃, 0-2.5V working voltage, 30mAh·g -1 The electrochemical performance test was carried out at a current density of 30 mAh·g. -1 The discharge specific capacity, charge specific capacity and first coulombic efficiency at the current density are shown in Table 1:

[0104] Table 1 Sodium ion battery performance test results

[0105]

[0106]

[0107] Table 1 shows the performance test results of sodium ion batteries. It can be seen from Table 1 that the sodium ion batteries assembled with the negative electrode sheets made of the hard carbon negative electrode materials in Examples 1-5 have a high performance at 30 mAh·g -1 The discharge capacity at a current density of 369.54 mAh g -1 , the charging capacity can reach 296mAh g -1 The first coulombic efficiency can reach 82.31%, indicating that the sodium ion battery provided by the present invention can store more electrical energy, has high charge and discharge efficiency, and good cycle stability, and can more effectively utilize active substances in the first cycle, release more charge, and has excellent electrochemical performance.

[0108] The difference between Comparative Example 2 and Example 1 is that phosphoric acid leaching is not performed, but thiourea is used for S and N element doping. From the data in Table 1, it can be seen that the hard carbon negative electrode material in Comparative Example 2 corresponds to a sodium ion battery at 30 mAh g -1 The discharge specific capacity and the first coulombic efficiency at a current density of 2.5 % and 1.5 % are significantly lower than those in Example 1, indicating that the effect of P element doping is better than that of S and N element doping.

[0109] The difference between Comparative Example 3 and Example 1 is that hydrochloric acid is used for acid leaching. From the data in Table 1, it can be seen that the hard carbon negative electrode material in Comparative Example 2 corresponds to a sodium ion battery at 30 mAh·g -1 The discharge specific capacity, charge specific capacity and first coulombic efficiency at the current density of are lower than those in Example 1, indicating that at the same concentration, the type of acid has a great influence on the material properties. Phosphoric acid leaching can not only remove impurities in the sample, but the doping of P element can also better control the structure of hard carbon during the carbonization process to increase the specific capacity.

[0110] The difference between Comparative Example 4 and Example 1 is that no coating agent is used. From the data in Table 1, it can be seen that the hard carbon negative electrode material in Comparative Example 4 corresponds to a sodium ion battery at 30 mAh·g -1 The discharge specific capacity, charge specific capacity and first coulombic efficiency at a current density of are lower than those in Example 1, especially the first coulombic efficiency is significantly reduced, indicating that after coating with asphalt, closed pores can be produced, the conductivity of the hard carbon negative electrode material can be improved, and the direct contact between the electrolyte and the hard carbon can be reduced, thereby improving the first coulombic efficiency of the battery.

[0111] Figure 1 The hard carbon negative electrode material in Example 1 corresponds to the sodium ion battery at 30 mA g -1 Schematic diagram of capacity and first coulombic efficiency at current density, given by Figure 1It can be seen that after the cross-linked starch in Example 1 was activated by phosphoric acid washing, impurity removal and P element doping, the platform capacity below 0.1V and the slope capacity above 0.1V of the hard carbon negative electrode material prepared were improved. Among them, the platform capacity below 0.1V was 151mAh·g -1 , indicating that phosphoric acid leaching treatment is beneficial to changing the graphite interlayer spacing and forming defects, thereby improving the battery's specific capacity and first coulombic efficiency.

[0112] Figure 2 The hard carbon negative electrode material in Example 2 corresponds to the sodium ion battery at 30 mA g -1 Schematic diagram of capacity and first coulombic efficiency at current density, given by Figure 2 It can be seen that the platform capacity of the hard carbon negative electrode material in Example 2 corresponding to the sodium ion battery below 0.1V is 120mAh·g -1 The improvement of the capacity and the first coulombic efficiency of the sodium ion battery is not as good as that in Example 1. The reason is that the concentration of phosphoric acid used for acid leaching in Example 2 is relatively high (6 mol / L), indicating that the concentration of the acid solution has a greater influence on the material properties. The solubility and reaction activity of the low concentration (1-3 mol / L) acid solution are better and more suitable for the preparation of hard carbon negative electrode materials.

[0113] Figure 3 The hard carbon negative electrode material in Comparative Example 1 corresponds to the sodium ion battery at 30 mA g -1 Schematic diagram of capacity and first coulombic efficiency at current density, given by Figure 3 It can be seen that the hard carbon negative electrode material in Comparative Example 1 was not treated with acid leaching, and the capacity and first coulomb efficiency of the corresponding sodium ion battery were lower than those in Example 1, and the platform capacity below 0.1V was 127 mAh·g -1 , indicating that acid leaching treatment of hard carbon negative electrode materials is more conducive to improving the specific capacity and first coulombic efficiency of the battery.

[0114] The hard carbon negative electrode material provided by the present invention selects various types of low-priced and renewable biomass starch as the carbon source, and is subjected to phenolic resin cross-linking treatment, phosphoric acid leaching, impurity removal, P element doping treatment, asphalt and other coating agent coating and carbonization to obtain the hard carbon negative electrode material. The prepared negative electrode plate is assembled into a sodium ion battery, and the battery has high discharge specific capacity, high charge specific capacity, high first coulomb efficiency, and excellent electrochemical performance.

Claims

1. A hard carbon negative electrode material, characterized in that: The preparation method comprises the following raw materials: starch, phenolic resin, phosphoric acid and coating agent.

2. The hard carbon negative electrode material according to claim 1, characterized in that: The mass ratio of the starch to the phenolic resin is 100: (10-70)。 3. The hard carbon negative electrode material according to claim 1, characterized in that: The concentration of the phosphoric acid is 0.5-6 mol / L.

4. The hard carbon negative electrode material according to claim 1, characterized in that: The mass of the coating agent is 0.1-10% of the total mass of the starch and the phenolic resin; Preferably, the coating agent comprises at least one of asphalt and industrial syrup.

5. The method for preparing the hard carbon negative electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: S1, mixing starch and phenolic resin, and ball milling to obtain cross-linked starch; S2, subjecting the cross-linked starch to phosphoric acid leaching to obtain activated starch, S3, mixing the activated starch with a coating agent to obtain coated starch; S4, carbonizing the coated starch to obtain the hard carbon negative electrode material.

6. The preparation method according to claim 5, characterized in that: In the step S1, the particle size of the cross-linked starch is less than 80 μm.

7. The preparation method according to claim 5, characterized in that: In the step S2, the acid leaching time is 1-3 hours; and / or, in the step S3, the temperature of mixing the activated starch and the coating agent is 35-45° C. and the time is 1-2 hours.

8. The preparation method according to claim 5, characterized in that: In step S4, the carbonization temperature rising procedure is: the initial temperature is 18-22°C, the temperature is raised to 350-450°C at a rate of 0.5-10°C / min, and the temperature is kept for 1.5-2.5h; then the temperature is raised to 900-1600°C at a rate of 0.5-10°C / min, and the temperature is kept for 1.5-2.5h.

9. A negative electrode plate, characterized in that: The hard carbon negative electrode material comprises the hard carbon negative electrode material according to any one of claims 1 to 4.

10. A sodium ion battery, characterized in that: Including the negative electrode sheet as described in claim 9.

Citation Information

Cited By

  • Biomass-based hard carbon negative electrode material and preparation method thereof

    CN120004238A